Nanometer ZSM-5 molecular sieve aggregate as well as preparation method and application thereof
The nano ZSM-5 molecular sieve is formed in situ on the surface of the solid-phase silicon source core, which solves the high cost and energy consumption problems caused by organic material assembly, realizes the control and efficient recovery of nano-scale grains, and improves catalytic activity and wear resistance. , simplifies the process flow.
Patent Information
- Application Number
- CN202310480590.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, the preparation of nano ZSM-5 molecular sieve aggregates requires the use of organic materials for assembly, resulting in high production costs, high energy consumption of post-treatment steps, difficult to control nano-scale grain size, and difficult to recover nanomaterials.
Using solid-phase silicon source as raw material, nano ZSM-5 molecular sieve is formed in situ on the surface of the solid-phase silicon source core through hydrothermal synthesis, avoiding the use of organic materials, simplifying the preparation process, realizing the control of nano-scale grains and Efficient recycling.
The green synthesis of nano ZSM-5 molecular sieve aggregates is achieved, which reduces production costs, simplifies the process flow, improves the catalytic activity and wear resistance of molecular sieves, and is easy to filtration and separation.
Smart Images

Figure CN118877906A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve synthesis and relates to an in-situ formed nano ZSM-5 molecular sieve aggregate and a preparation method thereof. Background Art
[0002] In order to alleviate the mass transfer limitation of traditional microporous molecular sieves, a large number of studies have been devoted to the preparation of nanomolecular sieves with smaller crystal sizes. However, when the crystal size of the molecular sieve is too small (less than 400nm), it is difficult to collect samples by filtration, and high-speed centrifugation and other means are often required to collect the product. This problem will significantly increase the production cost and limit the production and application of small-crystal molecular sieves.
[0003] A large number of studies are devoted to making molecular sieve products easier to recycle under the premise of maintaining the performance of nanomolecular sieves. At present, preparing nanomolecular sieves as micrometer-scale aggregates is an effective means to strengthen the diffusion advantage of nanomolecular sieves and take into account the recovery efficiency. Yu Han et al. used triblock copolymer F127 to assemble 100nm nanomolecular sieves into micrometer-scale aggregates during the synthesis process (Chem. Mater., 2009, 21, 2344); Tang Yi et al. used urea-formaldehyde polymer polymerization to induce the assembly of nanomolecular sieves to form microspheres (Chem. Mater. 2006, 18, 1861-1866). CN102872909A reports the use of mesoporous particles with positive charges on the surface to bond molecular sieve nanoparticles with negative charges on the surface, and the electrostatic interaction between molecular sieve nanoparticles and mesoporous particles is combined to obtain nanomolecular sieve aggregates. In the prior art, the formation of the above-mentioned nanomolecular sieve aggregates is all assembled by organic matter to synthesize the molecular sieve, and the organic materials need to be removed by post-processing. The method is relatively cumbersome, the raw material cost is high, and the post-processing step has high energy consumption.
[0004] Some studies have reported methods for assembling and molding molecular sieves without using organic materials. For example, CN1105906A reported a method for preparing a binder-free ZSM molecular sieve, which uses a mixture of a silicon oxide binder and ZSM molecular raw powder, and converts it into an integrated ZSM molecular sieve through hydrothermal treatment in a template aqueous solution or steam; however, the primary grain size of the molecular sieve product obtained by the above method is difficult to control to the nanometer level, and the method requires the molecular sieve raw powder to be obtained in advance, and it is still difficult to avoid the problem of recycling nanomaterials in the process of obtaining the nano molecular sieve raw powder. Summary of the invention
[0005] The first technical problem to be solved by the present invention is to provide a green synthesis method of nano ZSM-5 molecular sieve aggregates in view of the above technical problems, which method does not require the addition of organic matter to form molecular sieve aggregates. The second technical problem to be solved by the present invention is to provide a nano ZSM-5 molecular sieve aggregate, which can enhance diffusion mass transfer. The third technical problem to be solved by the present invention is to provide an application method of the nano ZSM-5 molecular sieve aggregates.
[0006] The first aspect of the present invention provides a method for preparing nano ZSM-5 molecular sieve aggregates, which comprises:
[0007] (1) obtaining a silicon source fine powder having an average particle size of less than 30 μm;
[0008] (2) preparing a crystallization precursor solution: mixing an aluminum source, a microporous template agent and water such as deionized water, stirring, adding a structural aid, stirring, adding a silicon source fine powder, stirring, and obtaining a crystallization precursor solution; the structural aid is sodium bromide;
[0009] (3) Crystallization:
[0010] (4) Post-treatment to obtain nano ZSM-5 molecular sieve aggregates.
[0011] The second aspect of the present invention provides a nano ZSM-5 molecular sieve aggregate, wherein the nano ZSM-5 molecular sieve aggregate is a micro-mesoporous aggregate of surface-exposed ZSM-5 molecular sieve nanocrystals, and the micropore volume is 0.06-0.13cm 3 / g; mesopore volume is 0.05-0.10cm 3 / g.
[0012] According to the present invention, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate is 55-75% in terms of crystallinity. The crystallinity measurement method refers to the standard ASTM D3906-03, and the measured relative crystallinity is taken as the mass fraction of ZSM-5 molecular sieve.
[0013] According to the present invention, the nano ZSM-5 molecular sieve aggregate exists in a particle state, and the average size of the aggregate particles is 5 to 20 μm, for example, 5.1 to 19.8 μm. The average particle size is measured in accordance with the "Particle Size Analysis Laser Diffraction Method", standard number GB / T19077-2016.
[0014] According to the present invention, nano ZSM-5 molecular sieve crystals are distributed on the surface of the nano ZSM-5 molecular sieve aggregate particles, and the average grain size of the nano ZSM-5 molecular sieve crystals is 20-400 nm, for example, 210-380 nm.
[0015] According to the present invention, the nano ZSM-5 molecular sieve aggregate is an in-situ crystallized ZSM-5 molecular sieve material, having a solid silicon source core, and the ZSM-5 molecular sieve grains grow on the outer surface of the solid silicon source core. The average diameter of the internal solid silicon source core is 3 to 18 μm. The solid silicon source core is measured by an electron probe X-ray microanalysis method. The nano ZSM-5 molecular sieve aggregate has a solid silicon source core, which can make the molecular sieve have better wear resistance.
[0016] In one embodiment, the content of the solid silicon source core in the nano ZSM-5 molecular sieve aggregate is 25-45%. The solid silicon source core content is measured by X-ray diffraction relative crystallinity method, which is defined as 100% minus the relative crystallinity of ZSM-5 molecular sieve.
[0017] Furthermore, the effective factor of the nano ZSM-5 molecular sieve aggregate is 0.4-0.9. The effective factor measurement method is as follows: catalytic cracking reaction is carried out with isopropylbenzene, the reaction temperature is 450-550°C, the reaction time is 70s, the pressure is 0.09-0.3MPa, and the raw material feed weight space velocity is 50-120h -1 The effective factor (η) is the ratio of the actual observed apparent reaction rate to the theoretical reaction rate. The Siler modulus of the catalytic material is tested by the probe reaction. get. The apparent reaction activation energy and intrinsic activation energy in the catalytic system were obtained by testing the cracking reaction performance of cumene probe molecules. For details, see Xie, Z. et al., Enhanced accessibility and utilization efficiency of acid sites in hierarchical MFI zeolite catalyst for effective diffusivity improvement. RSC Advances 2014, 4(82), 43752-43755.)
[0018] The third aspect of the present invention provides the use of the nano ZSM-5 molecular sieve aggregates in the catalytic cracking reaction of hydrocarbons.
[0019] Furthermore, the reaction conditions of the catalytic cracking reaction are: the device is a fixed bed reactor, the reaction pressure is 0.09-0.3MPa, the reaction temperature is 450-550°C, the raw material feed weight space velocity is 50-120 hours -1 .
[0020] The synthesis method of the nano ZSM-5 molecular sieve aggregate provided by the present invention provides all silicon sources with a solid-phase matrix, and the silicon species dissolved from the solid-phase silicon source during the formation of molecular sieve grains provide a material basis. By regulating the synthesis conditions, under hydrothermal synthesis conditions, the chemical processes such as silicon source dissolution, crystal nucleation, and crystal growth are precisely regulated, so that molecular sieve nanocrystals are formed in situ on the surface of the solid-phase matrix, and finally exposed to the outer surface to form aggregates, and the regulation of the chemical behavior of silicon source dissolution, crystal nucleation, and crystal growth is achieved in one step. The synthesis method is simple, the process is simple, and no multi-step synthesis is required, which greatly saves production costs. A granular molecular sieve / matrix microporous-mesoporous composite material that forms molecular sieve nanoparticles by in-situ crystallization on the surface of solid-phase silicon source particles is obtained, and the dispersion of active components is improved. On the basis of low cost, maintaining the microporous structure of nano molecular sieves, strengthening mass transfer diffusion, and improving the wear resistance of molecular sieves, intercrystalline stacking mesopores are introduced, which further reduces diffusion restrictions and improves the catalytic activity of molecular sieve materials.
[0021] The nano ZSM-5 molecular sieve aggregate provided by the present invention has at least one of the following advantages, preferably all of the advantages:
[0022] (1) It is a microporous-mesoporous composite material containing nano ZSM-5 molecular sieve particles and silicon source cores, which reduces diffusion limitations, enhances mass transfer and diffusion, and improves the catalytic activity of the molecular sieve material.
[0023] (2) The nano ZSM-5 molecular sieve aggregates are easy to filter.
[0024] (3) Good wear resistance.
[0025] (4) The effective factor of the reaction is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the XRD diagram of the product obtained in Example 1 of the present invention.
[0027] Figure 2 This is a low-magnification scanning electron microscope image of the product obtained in Example 1 of the present invention.
[0028] Figure 3 This is a high-magnification scanning electron microscope image of the product obtained in Example 1 of the present invention.
[0029] Figure 4 This is the isothermal adsorption curve of the product obtained in Example 1 of the present invention.
[0030] Figure 5 This is the pore distribution curve of the product obtained in Example 1 of the present invention.
[0031] Figure 6 This is a transmission electron microscope image of the product obtained in Example 1 of the present invention.
[0032] Figure 7 This is the EPMA chart of the product obtained in Example 1 of the present invention.
[0033] Figure 8 This is the XRD diagram of the product obtained in Comparative Example 1 of the present invention.
[0034] Fig. 9 This is a scanning electron microscope image of the product obtained in Comparative Example 1 of the present invention.
[0035] Fig.10 This is a scanning electron microscope image of the product obtained in Comparative Example 2 of the present invention.
[0036] Fig.11 This is a scanning electron microscope image of the product obtained in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0037] According to the method for preparing nano ZSM-5 molecular sieve aggregates of the present invention, the silicon source is a solid silicon source, and its average particle size does not exceed 30 microns. The solid silicon source includes, for example, one or more of diatomaceous earth, white carbon black, and solid silica gel. Preferably, the SiO2 content of the silicon source is higher than 90% by weight.
[0038] According to the preparation method of nano ZSM-5 molecular sieve aggregates of the present invention, if the average particle size of the silicon source raw material is greater than 30 microns, the silicon source fine powder can be obtained by fully grinding the silicon source raw material. In one embodiment, the grinding is completed by a ball mill, for example, the grinding adopts a planetary ball mill, the ball milling time is 1 to 5 hours, and the rotation speed is 100 to 500 rpm. Planetary ball mills are well known to those skilled in the art, such as the JC-QM series vertical planetary ball mill of Juchuang Environmental Protection.
[0039] The average particle size of the silicon source fine powder is preferably 5 to 30 microns, for example, the average particle size is less than 20 microns or less than 10 microns or 6 to 25 microns; the particle size of the silicon source fine powder is measured by laser diffraction particle size analysis, see GB / T 19077-2016. The particle size refers to the diameter.
[0040] According to the method for preparing nano ZSM-5 molecular sieve aggregates of the present invention, in step (2), a crystallization precursor solution is prepared by adding an aluminum source and a microporous template agent into water, such as deionized water, and stirring the mixture thoroughly, for example, for more than 0.5 hours, for example, for 0.5 to 4 hours. Then, a structural additive is added and stirred thoroughly, for example, for more than 0.5 hours, for example, for 0.5 to 4 hours. Then, a silicon source fine powder is added and stirred thoroughly, for example, for more than 0.5 hours, preferably for 0.5 to 4 hours, to obtain a crystallization precursor solution.
[0041] According to the method for preparing nano ZSM-5 molecular sieve aggregates of the present invention, the aluminum source is an aluminum-containing compound known to those skilled in the art that can be used to prepare ZSM-5, for example, the aluminum source can be one or more of aluminum isopropoxide, aluminum trichloride, and aluminum sulfate.
[0042] According to the method for preparing nano ZSM-5 molecular sieve aggregates of the present invention, the microporous template agent is an organic amine and / or organic ammonium microporous template agent that is well known to those skilled in the art and can be used to prepare ZSM-5. Preferably, the microporous template agent can be one or more of tetrapropylammonium hydroxide and tetrapropylammonium bromide.
[0043] The structural aid is a water-soluble inorganic sodium salt, such as one or more of sodium bromide, sodium chloride, sodium nitrate, and sodium carbonate. In the method of the present invention, the addition of the structural aid can shorten the crystallization time, and cooperate with the solid silicon source and other conditions to form a nanocrystalline ZSM-5 molecular sieve. Preferably, the structural aid is sodium bromide, and the bromide ion can promote the nucleation of the molecular sieve, and cooperate with other characteristics to have the effect of accelerating the crystallization rate.
[0044] According to the preparation method of nano ZSM-5 molecular sieve aggregates provided by the present invention, in the crystallization precursor solution, R:SiO2=0.1-0.5:1 (molar ratio), R represents a template; preferably R:SiO2=0.2-0.4:1 (molar ratio).
[0045] According to the method for preparing nano ZSM-5 molecular sieve aggregates provided by the present invention, in the crystallization precursor solution, the molar ratio of Al2O3:SiO2 is 0.004-0.05:1, for example, 0.01-0.04:1.
[0046] According to the preparation method of nano ZSM-5 molecular sieve aggregates provided by the present invention, in the crystallization precursor solution, H2O:SiO2=6-24:1 (molar ratio); preferably, H2O:SiO2=10-20:1 (molar ratio).
[0047] According to the preparation method of nano ZSM-5 molecular sieve aggregates provided by the present invention, in the crystallization precursor solution, X:SiO2=0.1-0.4:1 (molar ratio), X represents a structural additive; preferably, X:SiO2=0.2-0.3:1 (molar ratio);
[0048] According to the method provided by the present invention, the pH value of the crystallization precursor solution is 10-12.
[0049] In one embodiment, the R:SiO2=0.2-0.4:1, the Al2O3:SiO2 molar ratio=0.004-0.012:1, H2O:SiO2=10-20:1, X:SiO2=0.1-0.3:1, the silicon source is silica gel or white carbon black, X is sodium chloride or sodium nitrate, and the average particle size of the silicon source fine powder is less than 25 microns, such as 5-25 microns. Further, the R:SiO2=0.35-0.4:1, the Al2O3:SiO2 molar ratio=0.008-0.012:1, H2O:SiO2=15-20:1, X:SiO2=0.12-0.15:1, the silicon source is silica gel, the average particle size of the silicon source fine powder is less than 25 microns, such as 6-25 microns, and X is sodium nitrate. It can have a higher conversion rate and / or selectivity.
[0050] According to the method for preparing nano ZSM-5 molecular sieve aggregates provided by the present invention, the crystallization precursor solution is crystallized. Preferably, the crystallization is carried out at 150-190° C. for 16-72 hours, for example, at 160-180° C. for 20-60 hours.
[0051] According to the method for preparing nano ZSM-5 molecular sieve aggregates provided by the present invention, the crystallization is static crystallization. In one embodiment, the crystallization precursor solution is loaded into a crystallization kettle and allowed to stand at 150-190° C. for 16-72 hours for crystallization.
[0052] According to the preparation method of nano ZSM-5 molecular sieve aggregates provided by the present invention, after the crystallization is completed, post-treatment is performed, including: solid-liquid separation of the mixture obtained after crystallization, and optionally washing, drying, and roasting. The solid-liquid separation can be carried out by filtering or centrifugal separation. In one embodiment, after the crystallization is completed, suction filtration, washing, and drying are performed in sequence; the dried crystallized product is roasted to remove the microporous template agent therein to obtain nano molecular sieve aggregates. The roasting is, for example, roasted at 500-600°C for 4-8 hours.
[0053] The present invention will be further described with reference to the following examples, but the present invention is not limited thereto.
[0054] The average grain size is the average value obtained by randomly measuring the sizes of 20 molecular sieve grains (or molecular sieve aggregate particles) in an electron microscope (Hitachi scanning electron microscope, S-4800) image by Nano Measurer software. In the measurement process, the size of a molecular sieve grain (or molecular sieve aggregate particle) is the straight-line distance obtained by connecting the two farthest endpoints on the particle in the electron microscope image.
[0055] The particle size of the molecular sieve aggregate and the average particle size of the silicon source fine powder are equivalent volume diameters obtained by laser particle size method. Test instrument: Malvern Mastersizer 3000.
[0056] The relative crystallinity is in accordance with ASTM D3906-03 standard. The ratio of the characteristic peak area at 2θ angle between 22.5-25.0° in the XRD spectrum of the crystallized product to the characteristic peak area of the standard molecular sieve is defined as the relative crystallinity. Test instrument: D5005 X-ray diffractometer of Siemens, Germany. Test conditions: Cu target, Kα radiation, solid detector, tube voltage 40kV, tube current 40mA, step scan, step width 0.02°, prefabrication time 2s, scanning range 5°~70°.
[0057] The mesoporous surface area and specific surface area, pore volume (total pore volume), and pore size distribution are measured by low-temperature nitrogen adsorption capacity method. Test instrument: ASAP2400 static nitrogen adsorption instrument of Micromeritics. Test conditions: The sample is vacuum degassed for 4 hours at 1.33 Pa and 300 ° C, and then contacted with liquid nitrogen at 77 K, isothermally adsorbed and desorbed, adsorption and desorption isotherms are measured, and specific surface area and pore volume are calculated using BET formula, and average pore size is calculated using BJH formula.
[0058] The ball milling was carried out using a Juchuang environmental protection vertical planetary ball mill (JC-QM-0.4).
[0059] In the following examples and comparative examples, the room temperature is 25°C.
[0060] [Example 1]
[0061] (1) Preparation of silicon source fine powder: Diatomaceous earth (Lingshou County Fengheng Mineral Products Processing Plant, diatomaceous earth powder, SiO2 mass fraction 95%) was fully ball-milled (ball-milling time 2 hours, rotation speed 400 rpm) to obtain silicon source fine powder with an average particle size of 11.2 μm;
[0062] (2) preparing a crystallization precursor solution: weighing 0.77 g of aluminum isopropoxide in a beaker, adding 31.50 g of tetrapropylammonium hydroxide and 6.75 g of deionized water, stirring at room temperature for 1 hour; adding 3.06 g of sodium bromide, stirring for 1 hour; adding 7.90 g of the diatomaceous earth fine powder obtained in the first step, stirring at room temperature for 1 hour, and obtaining a crystallization precursor solution;
[0063] In the crystallization precursor solution of this embodiment:
[0064] R: SiO2 = 0.3:1 (molar ratio); R represents a template;
[0065] Al2O3:SiO2=0.015:1 (molar ratio)
[0066] H2O:SiO2=13.5:1 (molar ratio);
[0067] X:SiO2=0.24:1 (molar ratio), X represents sodium bromide;
[0068] Crystallization precursor solution pH = 11;
[0069] (3) The crystallization precursor solution obtained above was placed into a crystallization reactor and statically crystallized at 170° C. for 30 h;
[0070] (4) Post-treatment: After the crystallization reaction is completed, the crystallized mixture is filtered, washed, and dried in sequence. The dried crystallized product is calcined at 550° C. for 6 hours to remove the microporous template agent therein and obtain nano ZSM-5 molecular sieve aggregates.
[0071] The XRD spectrum of the sample is as follows Figure 1 As shown, from Figure 1 It can be seen that the synthesized nano ZSM-5 molecular sieve aggregate has the characteristic diffraction peak of ZSM-5 molecular sieve, and an obvious five-finger diffraction peak appears at 22.0-25.0°. As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate synthesized in Example 1 is 67% (based on crystallinity).
[0072] like Figure 2 As shown, the synthesized nano ZSM-5 molecular sieve aggregates exist in a particle state. As shown in Table 1, the average size of the aggregate particles is 5.1 μm;
[0073] like Figure 3 As shown, the outer surface of the synthesized nano ZSM-5 molecular sieve aggregate is densely distributed with ZSM-5 molecular sieve grains, and the average size of the molecular sieve is 260nm (Table 1).
[0074] like Figure 4 , Figure 5 As shown in Table 1, the synthesized nano ZSM-5 molecular sieve aggregates have mesopores, and the hysteresis loop can be observed in the adsorption isotherm. The presence of mesopores in the sample can be observed from the pore size distribution curve. As shown in Table 1, the micropore volume of the synthesized nano ZSM-5 molecular sieve aggregates in Example 1 is 0.07 cm 3 / g, mesopore volume is 0.05cm 3 / g.
[0075] The method of using nano ZSM-5 molecular sieve aggregates for catalytic cracking is as follows:
[0076] First, the nano ZSM-5 molecular sieve aggregate powder prepared in Example 1 was placed in an aqueous solution of ammonium sulfate with a concentration of 0.1 g / mL (powder: ammonium sulfate mass ratio = 1:1), stirred at 80°C for 2 hours for ion exchange, and exchanged twice in total to obtain an ammonia-type nano ZSM-5 molecular sieve aggregate powder. Subsequently, the nano ZSM-5 molecular sieve aggregate powder was washed with water, dried, and calcined at 550°C for 4 hours to obtain a hydrogen-type nano ZSM-5 molecular sieve aggregate powder. The hydrogen-type nano ZSM-5 molecular sieve aggregate powder was tableted and sieved to obtain catalyst particles of 40-60 mesh for catalytic cracking experiments.
[0077] The catalyst particles were placed in a fixed bed reactor, the reaction pressure was 0.1 MPa, the reaction temperature was 500 °C, and the feed weight hourly space velocity (WHSV) of the raw material (1,3,5 triisopropylbenzene, abbreviated as TIPB) was 80 h -1 ; Agent-oil ratio 0.6 weight ratio. After the reaction, the liquid phase material was collected by cold bath, and the gas phase product was collected by drainage gas collection method. The liquid phase product was analyzed by Agilent 7890B (HP-PONA column) chromatography, and the gas phase product was analyzed by Agilent 6890 chromatography. The TIPB conversion rate was calculated according to the following formula: conversion rate = 1-(TIPB mass in liquid phase product / TIPB raw material mass).
[0078] Benzene selectivity = mass of benzene in the product ÷ (mass of TIPB feedstock × conversion rate).
[0079] The effective factor (η) is the ratio of the actual observed apparent reaction rate to the theoretical reaction rate. The apparent activation energy (E) of the catalytic material is tested by the cumene probe catalytic reaction. app ) and intrinsic activation energy (E ink ), and then calculate the Siler modulus (Formula 1) is obtained. Substituting into formula (2) we can obtain the effective factor.
[0080]
[0081]
[0082] Reference
[0083] [Example 2]
[0084] (1) Preparation of silicon source fine powder: White carbon black (Sidley Chemical, SiO2 mass fraction 97%) was fully ball-milled (ball-milling time 4 hours, rotation speed 200 rpm) to obtain silicon source fine powder with an average particle size of 12.0 μm;
[0085] (2) Prepare a crystallization precursor solution: weigh 0.65 g of aluminum sulfate in a beaker, add 20.00 g of tetrapropylammonium hydroxide and 15.00 g of deionized water, and stir at room temperature for 30 minutes; add 1.50 g of sodium chloride and stir thoroughly for 30 minutes; add 7.73 g of the white carbon black fine powder obtained in the first step, stir at room temperature for 30 minutes to obtain a crystallization precursor solution.
[0086] In this embodiment, the crystallization precursor solution
[0087] R: SiO2 = 0.2: 1 (molar ratio), R represents a template;
[0088] Al2O3:SiO2=0.004:1 (molar ratio)
[0089] H2O:SiO2=10:1 (molar ratio);
[0090] X: SiO2 = 0.3:1 (molar ratio); X represents the structural auxiliary agent sodium chloride;
[0091] Crystallization precursor solution pH = 12;
[0092] (3) The crystallization precursor solution obtained above was placed into a crystallization reactor and statically crystallized at 160° C. for 60 h.
[0093] (4) Post-treatment: After the crystallization reaction is completed, the crystallized mixture is subjected to solid-liquid separation, and then filtered, washed, and dried in sequence. The dried crystallized product is calcined at 500° C. for 8 hours to remove the microporous template agent therein and obtain nano-molecular sieve aggregates.
[0094] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate synthesized in Example 2 is 75% (based on crystallinity).
[0095] As shown in Table 1 , the average size of aggregate particles is 8.9 μm;
[0096] The synthesized nano ZSM-5 molecular sieve aggregates have mesopores, and a hysteresis loop can be observed in the adsorption isotherm. The presence of mesopores in the sample can be observed from the pore size distribution curve. As shown in Table 2, the micropore volume of the synthesized nano ZSM-5 molecular sieve aggregates in Example 2 is 0.11 cm 3 / g, and the mesopore volume is 0.08cm 3 / g.
[0097] Method for using nano ZSM-5 molecular sieve aggregates for catalytic cracking: same as Example 1.
[0098] [Example 3]
[0099] (1) Preparation of silicon source fine powder: Solid silica gel (Qingdao Jiyida Silica Gel Reagent Co., Ltd., SiO2 mass fraction 99%) was fully ball-milled (ball-milling time 5 hours, rotation speed 400 rpm) to obtain silicon source fine powder with an average particle size of 24.5 μm;
[0100] (2) Prepare a crystallization precursor solution: weigh 0.52 g of aluminum chloride in a beaker, add 53.00 g of tetrapropylammonium bromide and 19.60 g of deionized water, and stir at room temperature for 3 hours; add 1.90 g of sodium nitrate and stir thoroughly for 3 hours; add 10.00 g of the solid silica gel obtained in the first step, and stir at room temperature for 30 minutes to obtain a crystallization precursor solution;
[0101] In the crystallization precursor solution of this embodiment:
[0102] R: SiO2 = 0.4: 1 (molar ratio), R represents a template;
[0103] Al2O3:SiO2=0.01:1 (molar ratio)
[0104] H2O:SiO2=20:1 (molar ratio);
[0105] X: SiO2 = 0.14:1 (molar ratio); X represents the structural auxiliary agent sodium nitrate;
[0106] Crystallization precursor solution pH = 10;
[0107] (3) The crystallization precursor solution obtained above was placed into a crystallization reactor and statically crystallized at 180° C. for 20 h;
[0108] (4) Post-treatment: After the crystallization reaction is completed, the crystallized mixture is filtered, washed, and dried in sequence. The dried crystallized product is calcined at 600° C. for 4 hours to remove the microporous template agent therein and obtain nano ZSM-5 molecular sieve aggregates.
[0109] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate synthesized in Example 1 is 71% (based on crystallinity).
[0110] The synthesized nano ZSM-5 molecular sieve aggregates exist in a particle state. As shown in Table 1, the average size of the aggregate particles is 15.1 μm;
[0111] The outer surface of the synthesized nano ZSM-5 molecular sieve aggregate is densely distributed with ZSM-5 molecular sieve grains, and the average size of the molecular sieve (also called average particle size) is 150nm (Table 1).
[0112] The low-temperature nitrogen adsorption characterization results show that the synthesized nano ZSM-5 molecular sieve aggregates have mesopores. A hysteresis loop can be observed in the adsorption isotherm, and the presence of mesopores in the sample can be observed from the pore size distribution curve. As shown in Table 2, the micropore volume of the synthesized nano ZSM-5 molecular sieve aggregates in Example 3 is 0.08 cm 3 / g, and the mesopore volume is 0.06cm 3 / g.
[0113] The method for using nano ZSM-5 molecular sieve aggregates for catalytic cracking is the same as in Example 1.
[0114] [Example 4]
[0115] The silicon source fine powder is the same as that in Example 1, the amount of sodium carbonate added to the crystallization precursor solution is 2.30 g, and the other preparation conditions are the same as those in Example 1.
[0116] In the crystallization precursor solution of this embodiment:
[0117] R: SiO2 = 0.3: 1 (molar ratio), R represents a template;
[0118] Al2O3:SiO2=0.015:1 (molar ratio)
[0119] H2O:SiO2=13.5:1 (molar ratio);
[0120] X: SiO2 = 0.17: 1 (molar ratio), X represents the structural auxiliary agent sodium carbonate;
[0121] The crystallization precursor solution pH=11.
[0122] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate synthesized in Example 4 is 64% (based on crystallinity).
[0123] The synthesized nano ZSM-5 molecular sieve aggregates exist in a particle state. As shown in Table 1, the average size of the aggregate particles is 8.6 μm;
[0124] The outer surface of the synthesized nano ZSM-5 molecular sieve aggregate is densely distributed with ZSM-5 molecular sieve particles, and the average particle size of the molecular sieve is 340 nm (Table 1).
[0125] The synthesized nano ZSM-5 molecular sieve aggregates have mesopores, and a hysteresis loop can be observed in the adsorption isotherm. The presence of mesopores in the sample can be observed from the pore size distribution curve. As shown in Table 2, the micropore volume of the synthesized nano ZSM-5 molecular sieve aggregates in Example 4 is 0.07 cm 3 / g, mesopore volume is 0.05cm 3 / g.
[0126] Method for using nano ZSM-5 molecular sieve aggregates for catalytic cracking: same as Example 1.
[0127] [Example 5]
[0128] The silicon source fine powder is the same as that in Example 1, the amount of tetrapropylammonium hydroxide added to the crystallization precursor solution is 18.0 g, and the other preparation conditions are the same as those in Example 1.
[0129] In the crystallization precursor solution of this embodiment:
[0130] R: SiO2 = 0.15: 1 (molar ratio), R represents a template;
[0131] Al2O3:SiO2=0.015:1 (molar ratio)
[0132] H2O:SiO2=13.5:1 (molar ratio);
[0133] NaX:SiO2=0.24:1 (molar ratio); NaX represents sodium salt
[0134] The crystallization precursor solution pH=11.
[0135] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the nano ZSM-5 molecular sieve aggregate synthesized in Example 5 is 57% (based on crystallinity).
[0136] The synthesized nano ZSM-5 molecular sieve aggregates exist in a particle state. As shown in Table 1, the average size of the aggregate particles is 9.8 μm;
[0137] The outer surface of the synthesized nano ZSM-5 molecular sieve aggregate is densely distributed with ZSM-5 molecular sieve particles, and the average particle size of the molecular sieve is 380 nm (Table 1).
[0138] The synthesized nano ZSM-5 molecular sieve aggregates have mesopores, and a hysteresis loop can be observed in the adsorption isotherm. The presence of mesopores in the sample can be observed from the pore size distribution curve. As shown in Table 2, the micropore volume of the synthesized nano ZSM-5 molecular sieve aggregates in Example 1 is 0.07 cm 3 / g, mesopore volume is 0.05cm 3 / g.
[0139] Method for using nano ZSM-5 molecular sieve aggregates for catalytic cracking: same as Example 1.
[0140] [Comparative Example 1]
[0141] The silicon source fine powder is the same as that in Example 1, the amount of sodium bromide added to the crystallization precursor solution is 0.7 g, and the other preparation conditions are the same as those in Example 1.
[0142] In the crystallization precursor solution:
[0143] R: SiO2 = 0.3: 1 (molar ratio), R represents a template;
[0144] Al2O3:SiO2=0.015:1 (molar ratio)
[0145] H2O:SiO2=13.5:1 (molar ratio);
[0146] X: SiO2 = 0.05:1 (molar ratio); X represents a structural additive (sodium bromide);
[0147] Crystallization precursor solution pH = 11,
[0148] Method for using nano ZSM-5 molecular sieve aggregates for catalytic cracking of alkane molecules: same as Example 1.
[0149] The XRD spectrum of the sample is as follows Figure 8 As shown, from Figure 8 It can be seen that the obtained product does not have the characteristic diffraction peak of ZSM-5 molecular sieve, and no obvious five-finger diffraction peak appears at 22.0-25.0°. As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the synthetic material in Comparative Example 1 is 0% (based on crystallinity).
[0150] The SEM images of the samples are shown in Fig. 9 As shown, from Fig. 9 It can be seen that no molecular sieve grains were observed in the product obtained in Comparative Example 1, and only silicon source raw material particles were observed.
[0151] As shown in Table 2, the catalytic cracking reaction was carried out using the catalytic material obtained in Comparative Example 1 according to the method of Example 1. Under the same reaction conditions, the conversion rate was significantly lower than that of the example, and the selectivity of the deep cracking product benzene was significantly lower than that of the example.
[0152] [Comparative Example 2]
[0153] Using diatomite fine powder as a silicon source, a crystallization precursor solution was prepared according to the experimental scheme of preparing ZSM-5 molecular sieve by conventional in-situ crystallization of natural mineral soil: 11.60g of tetrapropylammonium hydroxide was weighed in a beaker, 57.3g of deionized water and 1.0g of aluminum isopropoxide were added, and stirred at room temperature for 1 hour; 0.58g of sodium hydroxide was added, and stirred at room temperature for 1 hour; 10.24g of diatomite fine powder was added, and stirred at room temperature for 1 hour to obtain a crystallization precursor solution. The crystallization conditions (temperature, time) and post-treatment method were the same as those in Example 1.
[0154] In this comparative example, the crystallization precursor solution
[0155] R: SiO2 = 0.05:1 (molar ratio); R represents a template;
[0156] Al2O3:SiO2=0.015:1 (molar ratio)
[0157] H2O:SiO2=22.8:1 (molar ratio);
[0158] NaOH:SiO2=0.09:1 (molar ratio);
[0159] The crystallization precursor solution pH=11.
[0160] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the synthetic material in Comparative Example 2 is 60% (based on crystallinity). Fig.10 As shown, the ZSM-5 molecular sieve in the product obtained in Comparative Example 2 is of micron size. As shown in Table 2, the conversion rate of the catalytic cracking reaction using the catalytic material obtained in Comparative Example 1 is significantly lower than that of the comparative example under the same reaction conditions, and the benzene selectivity of the deep cracking product is significantly lower than that of the embodiment.
[0161] [Comparative Example 3]
[0162] Molecular sieve synthesis was performed using a liquid silicon source (silica sol, LudoxAS40, SiO2 content 40wt%) instead of a solid silicon source. After mixing 23g of water and 22.5g of TPAOH, 10g of silica sol and 0.14g of aluminum isopropoxide were added dropwise to obtain a uniform mixed solution and stirred for 2 hours. The crystallization conditions (temperature, time) and post-treatment method were the same as those in Example 1.
[0163] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the material synthesized in Comparative Example 3 is 89% (based on crystallinity). The ZSM-5 molecular sieve in the product obtained in Comparative Example 3 presents a micron-sized size. As shown in Table 2, the material obtained in Comparative Example 3 is used as a catalyst to carry out a catalytic cracking reaction according to the method of Example 1. Under the same reaction conditions, the conversion rate is significantly lower than that of the example, and the selectivity of the deep cracking product benzene is significantly lower than that of the example.
[0164] [Comparative Example 4]
[0165] The silicon source fine powder is the same as that in Example 1. 31.50 g of tetrapropylammonium hydroxide, 6.75 g of deionized water and 3.06 g of sodium bromide are weighed in a beaker and stirred for 1 hour; 7.90 g of the diatomaceous earth fine powder obtained in the first step is added and stirred at room temperature for 1 hour, and finally 0.77 g of aluminum isopropoxide is added to obtain a crystallization precursor solution;
[0166] In the crystallization precursor solution of this embodiment:
[0167] R: SiO2 = 0.3:1 (molar ratio); R represents a template;
[0168] Al2O3:SiO2=0.015:1 (molar ratio)
[0169] H2O:SiO2=13.5:1 (molar ratio);
[0170] X:SiO2=0.24:1 (molar ratio), X represents sodium bromide;
[0171] Crystallization precursor solution pH = 11;
[0172] The crystallization conditions (temperature, time) and post-treatment method are the same as those in Example 1.
[0173] As shown in Table 1, the mass fraction of ZSM-5 molecular sieve in the material synthesized in Comparative Example 4 is 23% (based on crystallinity). The ZSM-5 molecular sieve in the product obtained in Comparative Example 4 presents a submicron size. As shown in Table 2, the material obtained in Comparative Example 4 is used as a catalyst to carry out a catalytic cracking reaction according to the method of Example 1. Under the same reaction conditions, the conversion rate is significantly lower than that of the example, and the selectivity of the deep cracking product benzene is significantly lower than that of the example.
[0174] Table 1 Properties of molecular sieve samples obtained in Examples and Comparative Examples
[0175]
[0176] It can be seen from Table 1 that, compared with the comparative example, the nano ZSM-5 molecular sieve aggregate obtained in the present invention not only has high crystallinity and large micropore specific surface area, but also has a mesoporous structure and is a multi-level porous material.
[0177] Table 2 Conversion rate of samples obtained from various examples and comparative examples in TIPB catalytic cracking reaction
[0178] Conversion rate (%) Benzene selectivity in product (%) Example 1 68 11 Example 2 79 13 Example 3 85 17 Example 4 76 12 Example 5 71 11 Comparative Example 1 <3 <3 Comparative Example 2 55 7 Comparative Example 3 62 9 Comparative Example 4 18 5
[0179] As can be seen from Table 2, the conversion rate of the molecular sieve product of the embodiment for catalytic cracking reaction is significantly higher than that of the comparative example under the same reaction conditions, and the selectivity of the deep cracking product benzene is significantly higher than that of the comparative example, showing a good catalytic effect.
[0180] The present invention adopts a solid silicon source and an in-situ method to synthesize nano ZSM-5 aggregates. On the basis of maintaining the microporous structure of the nano molecular sieve, strengthening mass transfer diffusion, and improving the wear resistance of the molecular sieve, intercrystalline stacking mesopores are introduced, which further reduces the diffusion limitation and improves the catalytic activity of the molecular sieve material. The nano ZSM-5 molecular sieve aggregates obtained by the present invention have higher conversion activity in macromolecular cracking reactions, higher macromolecular catalytic cracking activity, and higher yield of deep cracking products. The nano ZSM-5 molecular sieve aggregates obtained in the present invention can achieve product separation by simple filtration.
[0181] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing nano ZSM-5 molecular sieve aggregates, comprising the following steps: (1) obtaining a silicon source fine powder having an average particle size of less than 30 μm; (2) preparing a crystallization precursor solution: mixing an aluminum source, a microporous template agent and water, performing a first stirring, for example, stirring for more than 0.5 hours, adding a structural aid, performing a second stirring, for example, stirring for more than 0.5 hours, adding a silicon source fine powder, performing a third stirring, for example, stirring for more than 0.5 hours, to obtain a crystallization precursor solution; the structural aid is a soluble inorganic sodium salt, preferably sodium bromide, and X represents the structural aid, and the molar ratio of X:SiO2 is 0.1 to 0.4:1; (3) Crystallization; (4) Post-treatment to obtain nano ZSM-5 molecular sieve aggregates.
2. The method according to claim 1, characterized in that The average particle size of the silicon source fine powder is 0.05-30 μm, the first stirring time is 0.5-4 hours, the second stirring time is 0.5-4 hours, and the third stirring time is 0.5-4 hours.
3. The method according to claim 1, characterized in that: The silicon source is a solid silicon source with a SiO2 content higher than 90% by weight.
4. The method according to claim 1 or 3, characterized in that: The aluminum source is one or more of aluminum isopropoxide, aluminum trichloride, and aluminum sulfate; the silicon source is one or more of diatomaceous earth, white carbon black, and solid silica gel; the microporous template is one or more of tetrapropylammonium hydroxide and tetrapropylammonium bromide; and the soluble inorganic sodium salt is one or more of sodium bromide, sodium chloride, sodium nitrate, and sodium carbonate.
5. The method according to claim 1, characterized in that In the crystallization precursor solution, the molar ratio of R:SiO2 is 0.1-0.5:1, where R represents a template; the molar ratio of H2O:SiO2 is 6-24:1; and the molar ratio of Al2O3:SiO2 is 0.004-0.05:
1.
6. The method according to claim 5, characterized in that In the crystallization precursor solution, the molar ratio of H2O:SiO2 is 10-20:1, the molar ratio of X:SiO2 is 0.2-0.3:1, and the molar ratio of R:SiO2 is 0.2-0.4:
1.
7. The method according to claim 1, characterized in that The pH value of the crystallization precursor solution is 10-12.
8. The method according to claim 1, characterized in that The crystallization is static crystallization.
9. The method according to claim 1, characterized in that: The crystallization conditions are: crystallization at 150-190° C. for 16-72 hours.
10. The method according to claim 1, characterized in that The post-treatment comprises: filtering, washing, drying in sequence, and calcining at 500-600° C. for 4-8 hours.
11. A nano ZSM-5 molecular sieve aggregate, characterized in that: The nano ZSM-5 molecular sieve aggregate is a micro-mesoporous aggregate of nano ZSM-5 molecular sieve crystals exposed on the surface, and includes the following characteristics: (1) According to the crystallinity, the mass fraction of ZSM-5 molecular sieve in the micro-mesoporous aggregates of the surface-exposed nano ZSM-5 molecular sieve crystals is 55-75%; the relative crystallinity is tested according to ASTM D3906-03 standard; (2) The micro-mesoporous aggregates of the surface-exposed nano ZSM-5 molecular sieve crystals exist in a particle state, and the average size of the aggregate particles of the micro-mesoporous aggregates of the surface-exposed nano ZSM-5 molecular sieve crystals is 5 to 20 μm; (3) Nano ZSM-5 molecular sieve crystals are distributed on the surface of the micro-mesoporous aggregates of the surface-exposed nano ZSM-5 molecular sieve crystals, and the average grain size of the nano ZSM-5 molecular sieve crystals is 20-400 nm; (4) The micropore volume of the surface-exposed micro-mesoporous aggregates of ZSM-5 molecular sieve nanocrystals is 0.06-0.13 cm 3 / g, and the mesopore volume is 0.05-0.10cm 3 / g.
12. The nano ZSM-5 molecular sieve aggregate according to claim 11, characterized in that: The micro-mesoporous aggregates of surface-exposed ZSM-5 molecular sieve nanocrystals have solid-phase silicon source cores, the content of which is 25-45%. The content of which is measured by an X-ray diffraction relative crystallinity method is 100% minus the crystallinity of the ZSM-5 molecular sieve. The average diameter of the internal solid-phase silicon source cores is 3 to 18 μm.
13. The micro-mesoporous aggregates of surface-exposed ZSM-5 molecular sieve nanocrystals according to claim 11, characterized in that: The effectiveness factor of the micro-mesoporous aggregates of the surface-exposed ZSM-5 molecular sieve nanocrystals is 0.4-0.
9.
14. Nano ZSM-5 molecular sieve aggregates obtained by the method according to any one of claims 1 to 10.
15. Use of the nano ZSM-5 molecular sieve aggregates according to claim 11, 12, 13 or 14 in catalytic cracking reactions.
Citation Information
Patent Citations
Molecular sieve aggregate and its preparation method
CN102872909A
Hydrophobic silicon zeolite adsorbent without cohesive agent and its preparation
CN1105906A
Process for producing cavity type ZSM-5 modified zeolite molecular sieve
CN101428817A
Method for preparing nano ZSM-5 molecular sieve
CN102001680A
ZSM-5 / MCM-48 composite molecular sieve, preparation method and application thereof
CN104043477A