Production method for preparing potassium chloride from carnallite

By adding the grading and material separation operation of the crystallizer bottom flow in the optical haloite processing process, the problem of fine particle size of potassium chloride products is solved, the crystallization efficiency and product quality are improved, energy consumption and equipment investment are reduced, and more efficient is achieved production of potassium chloride.

CN118877912APending Publication Date: 2024-11-01BLUESTAR LEHIGH ENG INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410923008.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing light halide processing technology, the potassium chloride product has fine particle size, resulting in poor flotation, low washing and purification efficiency, difficulty in filtration and dehydration, and large mechanical losses. The existing processes such as hot melt recrystallization and dry granulation have high energy consumption. , equipment investment or equipment is prone to corrosion.

Method used

The bottom flow of the crystallizer adds grading operations and material separation operations. Through the grading operations, the fine mud and fine crystals are removed. The material separation operations return the crystallized potassium chloride particles to the crystallizer, increase the crystallization growth point, improve crystallization efficiency, and achieve chlorination. Controllability of potassium particle size.

Benefits of technology

It significantly improves the particle size of potassium chloride products, improves flotation and washing efficiency, reduces production energy consumption, improves product quality and resource utilization, and reduces equipment investment and operation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877912A_ABST
    Figure CN118877912A_ABST
Patent Text Reader

Abstract

The invention relates to a production method for preparing potassium chloride from carnallite, and belongs to the field of inorganic salt production processes. According to the method disclosed by the invention, a production process for preparing potassium chloride by decomposing carnallite is utilized, grading operation and material distribution operation are added to the bottom flow of a crystallizer, and most fine silt and excessive fine grains are removed through the grading operation; a part of crystallized potassium chloride particles are returned to a crystallizer as seed crystals through material distribution operation, and the rest part enters flotation operation to obtain potassium chloride concentrate. According to the invention, most fine silt and excessive fine grains can be removed through grading operation, so that the stability of a crystallization environment is ensured. Through the material distribution operation, a part of crystallized potassium chloride particles can be returned to the crystallizer as seed crystals, and the potassium chloride crystals further grow on the original basis, so that the crystallization efficiency is improved, and the aim of controlling the crystallization granularity of the potassium chloride is fulfilled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic salt production technology, and in particular to a method for producing potassium chloride by utilizing carnallite ore. Background Art

[0002] Carnallite is a complex salt containing potassium chloride, magnesium chloride and crystal water, with a molecular formula of KCl·MgCl2·6H2O. Carnallite, as it is commonly known, actually refers to carnallite ore, which is a mixed salt of carnallite and sodium chloride (Na + ,K + Mg 2+ / / Cl - -H2O quaternary water salt system) or mixed salts of carnallite, sodium chloride and magnesium sulfate, potassium salt magnesium vanadium, etc. (Na + ,K + Mg 2+ / / Cl - ,SO4 2- -H2O system), and also insoluble fine mud with varying contents. In the process of processing carnallites to extract potassium chloride, fresh water needs to be added to decompose the carnallites. Due to the difference in solubility between potassium chloride and magnesium chloride, all magnesium chloride enters the liquid phase, part of potassium chloride enters the liquid phase, and most of potassium chloride enters the solid phase to form potassium chloride products.

[0003] Since there is an objective process of potassium chloride recrystallization when carnallites decompose, the potassium chloride product obtained by this method has a fine particle size, and the average particle size is only about 0.050mm. This fine-grained potassium chloride has a great impact on subsequent production, such as entrainment of fine-grained sodium chloride during flotation, resulting in poor sorting, large water consumption during washing and purification, resulting in low concentrate yield, difficulty in dehydration during filtration and drying, and large mechanical loss. Therefore, many units at home and abroad have conducted research and exploration on this and developed a variety of production processes for producing coarse-grained potassium chloride, such as hot melt recrystallization process, dry granulation process, carnallites cold decomposition crystallization process, etc. The hot melt recrystallization process is to first add fresh water to decompose carnallites at low temperature to obtain potassium chloride and sodium chloride, and then use the solubility difference of potassium chloride and sodium chloride under high temperature conditions, solid-liquid separation at high temperature to obtain undissolved sodium chloride, and then liquid phase cooling to precipitate potassium chloride, and then washing, filtering and drying to obtain granular potassium chloride products, but this process has the disadvantages of high energy consumption and easy corrosion of equipment. The dry granulation process is to add a small amount of organic binder, granulation aid, wetting agent, etc. to the potassium chloride powder after obtaining the powdered potassium chloride product, stir evenly, add them together to the granulator for granulation, and obtain large-particle potassium chloride products in the form of pellets after drying. The disadvantages of this process are large equipment investment, the need for external granulation aids, high energy consumption, and high operating costs.

[0004] Compared with the above two processes, the cold crystallization process has a more obvious advantage in that the investment and energy consumption increase is not obvious, and a potassium chloride product with a coarser particle size can be obtained without adding external additives. For example, the invention patents disclosed in Chinese patent documents CN102963912B and CN104058428B use a cold decomposition crystallization-flotation-washing process and a reverse flotation-cold decomposition crystallization process to obtain a granular potassium chloride product. However, these two processes still have the following disadvantages that cannot be overcome: ① Limited by the working principle of the crystallizer, the overflow desliming effect of the crystallizer is poor. When the fine mud content in the carnallite ore is high, since the crystallizer discharges fine crystals and fine mud by overflow, the effect of removing fine crystals and fine mud is very limited. A large amount of fine mud will affect the subsequent flotation operation, and then affect the quality of potassium chloride products.

[0005] ② Due to the working principle of the crystallizer, since the stirring force of the crystallizer is weak, the product particles will leave the crystallization zone after growing to a certain extent, and the particle size will no longer increase. Although the product particle size has increased significantly compared with the product particle size of the direct decomposition process, the particle size is still relatively fine. The product particle size must be further increased to effectively reduce the energy consumption and product loss of subsequent filtration and washing operations. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a production method for preparing potassium chloride by using carnallite with improved crystallization efficiency and crystallization stability in view of the deficiencies in the prior art.

[0007] The technical problem to be solved by the present invention is achieved by the following technical solution. The present invention is a production method for preparing potassium chloride by using carnallite, which is characterized in that: during the crystallization operation, the method adds a classification operation and a material separation operation to the bottom flow of the crystallizer, and removes most of the fine mud and excessive fine crystals through the classification operation; a part of the crystallized potassium chloride particles is returned to the crystallizer as crystal seeds through the material separation operation, and the rest enters the flotation operation to obtain potassium chloride concentrate.

[0008] In the present invention, the method for implementing the material separation operation can be manual material separation or the use of fully automatic or semi-automatic material separation tools for material separation. Any tool that can separate the material into two parts in the prior art can be applicable to the present invention. The material separation equipment disclosed in the present invention is preferred.

[0009] A further preferred technical solution of the above-mentioned production method is that during the classification operation, the classification particle size is controlled within the range of 0.074 mm to 0.15 mm.

[0010] The above-mentioned production method has a further preferred technical solution: the specific steps are as follows: Crush the carnallite to less than -10mm; add the crushed carnallite to the crystallizer, add an appropriate amount of fresh water, add the overflow from the thickener 1 to the crystallizer, add the return material from the distributor as a seed crystal to the crystallizer, and return the refined potassium filtrate from the filtration to the crystallizer; The crystallizer bottom flow enters the classification operation, and the classification particle size is controlled at 0.074mm~0.15mm. The coarse-grained material enters the material separation operation, and the fine-grained material enters the thickener I together with the crystallizer overflow; the material separation operation divides the material into two parts, one part is returned to the crystallizer as a seed, and the rest enters the flotation operation; The froth product of the flotation operation is the concentrate, which enters the filtration and dehydration operation, and the filtrate returns to the flotation operation; the product in the tank is the tailings slurry, which enters the thickener II, and the overflow of the thickener II returns to the flotation operation, and the underflow of the thickener II is the flotation tailings; The concentrated ore after filtration enters the washing process, and after adding fresh water for washing, it enters the filtering process again. The liquid phase is the refined potassium filtrate, which returns to the crystallizer, and the solid phase is dried to obtain the potassium chloride product.

[0011] A further preferred technical solution of the production method described above is that the equipment used for the classification operation is a screening equipment for classification according to particle size or a equipment for classification according to fluid dynamic characteristics.

[0012] A further preferred technical solution of the production method described above is that the material dividing equipment used in the material dividing operation is a three-way pipe fitting, the material inlet is located at the upper part, and the material outlets are arranged on both sides of the lower part.

[0013] The above production method has a further preferred technical solution that: the discharge port of the material dispensing equipment used in the material dispensing operation is provided with a regulating mechanism for regulating the discharge amount. The regulating mechanism may be a regulating valve.

[0014] A further preferred technical solution of the production method described above is that an adjusting baffle is provided in the three-way pipe fitting to adjust the discharge amount of the material outlet.

[0015] A further preferred technical solution of the production method described above is that the ratio of the material returned to the crystallizer accounts for 10% to 90% of the underflow material of the crystallizer.

[0016] A further preferred technical solution of the production method described above is that during the material splitting operation, the ratio of the material returned to the crystallizer accounts for 30% to 70% of the underflow material of the crystallizer.

[0017] A further preferred technical solution of the above-mentioned production method is: adding clean water to the crystallizer to control the potassium ion content in the crystallizer underflow to no more than 2.5%.

[0018] A further preferred technical solution of the production method described above is: adding an appropriate amount of clean water to the thickener I to control the potassium ion content of the thickener overflow to be no higher than 3.0%.

[0019] Compared with the prior art, the present invention has the following beneficial effects: By adding grading and material separation operations to the bottom flow of the crystallizer, most of the fine mud and excessive fine crystals can be removed through grading operations, ensuring the stability of the crystallization environment. The material separation operation can return a part of the crystallized potassium chloride particles to the crystallizer as seeds, so that the potassium chloride in the crystallizer has more growth points when crystallizing, and the potassium chloride crystals grow further on the original basis, thereby improving the crystallization efficiency and achieving the goal of controllable potassium chloride crystal size.

[0020] Through the technical solution of the present invention, a large amount of existing low-quality carnallite ores containing mud are put to use, thereby improving the utilization rate of potash ore resources; in the production process, since the particle size of the potassium chloride product is significantly increased, the efficiency of the flotation operation and the washing operation is significantly improved, the production energy consumption is reduced, the product quality is improved, and significant economic benefits are achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a process flow chart of the method of the present invention; Figure 2 A schematic diagram of the structure of a material distributor used for material distribution operations. DETAILED DESCRIPTION

[0022] The specific technical solutions of the present invention are further described below to help those skilled in the art further understand the present invention without limiting the rights thereof.

[0023] Embodiment 1, see attached Figure 1 -2, Experiment 1 of the production method of potassium chloride using carnallite ore: ① Crush the carnallite ore (containing 15.5% KCl, 48.2% NaCl, 17.5% MgCl2, and 1.8% water-insoluble matter) to less than 10 mm.

[0024] ② The crystallizer is pre-filled with mother liquor, the composition of which is Na + ,K + Mg 2+ / / Cl - -H2O quaternary water-salt system metastable phase diagram KCl, NaCl and carnallite three-phase co-saturation point mother liquor composition, the main component mass content is K + 1.78%,Na + 0.65%,Mg 2+ 6.64%, Cl - 20.97%.

[0025] ③ The crushed material is transported to the crystallizer, and at the same time, the overflow of thickener I, the seed crystals returned from the material separation operation, the refined potassium mother liquor and fresh water from the washing and filtration operation are added. The potassium ion content of the bottom flow liquid phase of the crystallizer is controlled to be no more than 2.5% by adjusting the amount of fresh water.

[0026] ④ The classification operation adopts a hydrocyclone, and the classification particle size is controlled to be 0.10mm. The fine-grained material enters the thickener I together with the crystallizer overflow, and the coarse-grained material enters the distributor.

[0027] ⑤ Add fresh water to thickener I and adjust the amount of fresh water to control the potassium ion content in the overflow to no more than 3.0%.

[0028] ⑥ The coarse-grained material enters the distributor, and the distributor separates 40% of the material as seeds and returns to the crystallizer.

[0029] ⑦ The remaining 60% of the material in the distributor operation enters the flotation operation, and the overflow of the thickener II is used for slurry adjustment. The flotation operation adopts a process flow of primary roughing and secondary concentrating. The product in the tank is tailings slurry, which enters the thickener II. The overflow of the thickener II returns to the flotation operation. The foam product of the flotation operation is the concentrate slurry, which enters the filtration and dehydration operation, and the filtrate returns to the flotation operation. The solid phase enters the washing operation.

[0030] ⑧ The amount of water added for washing operation is based on Na + ,K + Mg 2+ / / Cl - -H2O quaternary water-salt system calculated 110% of the theoretical amount of water, the washing time is 30min, after washing, the solid phase obtained by filtration is dried to obtain the potassium chloride product, and the liquid phase is the refined potassium mother liquor, which is returned to the crystallizer.

[0031] ⑨ The obtained potassium chloride product has an average particle size of 1.25 mm, a potassium chloride content of 96.5%, and a recovery rate of 75.0%.

[0032] Example 2, reference Figure 1 and 2 , a production method for preparing potassium chloride using carnallite ore Experiment 2: ① Crush the carnallite ore (containing KCl 18.4%, NaCl 38.2%, MgCl2 23.4%, and water-insoluble matter 1.3%) to less than 10 mm.

[0033] ② The crystallizer is pre-filled with mother liquor, the composition of which is Na + ,K + Mg 2+ / / Cl --H2O quaternary water-salt system metastable phase diagram KCl, NaCl and carnallite three-phase co-saturation point mother liquor composition, the main component mass content is K + 1.78%,Na + 0.65%,Mg 2+ 6.64%, Cl - 20.97%.

[0034] ③ The crushed material is transported to the crystallizer, and at the same time, the overflow of thickener I, the seed crystals returned from the material separation operation, the refined potassium mother liquor and fresh water from the washing and filtration operation are added. The potassium ion content of the bottom flow liquid phase of the crystallizer is controlled to be no more than 2.5% by adjusting the amount of fresh water.

[0035] ④ The grading operation uses a high-frequency vibrating screen to control the grading particle size to 0.074mm. The fine-grained material enters the thickener I together with the crystallizer overflow, and the coarse-grained material enters the distributor.

[0036] ⑤ Add fresh water to thickener I and adjust the amount of fresh water to control the potassium ion content in the overflow to no more than 3.0%.

[0037] ⑥ The coarse-grained material enters the distributor, and the distributor separates 50% of the material as seeds and returns to the crystallizer.

[0038] ⑦ The remaining 50% of the material in the distributor operation enters the flotation operation, and the overflow of the thickener II is used for slurry adjustment. The flotation operation adopts a process flow of primary roughing and secondary concentrating. The product in the tank is tailings slurry, which enters the thickener II. The overflow of the thickener II returns to the flotation operation. The foam product of the flotation operation is the concentrate slurry, which enters the filtration and dehydration operation, and the filtrate returns to the flotation operation. The solid phase enters the washing operation.

[0039] ⑧ The amount of water added for washing operation is based on Na + ,K + Mg 2+ / / Cl - -H2O quaternary water-salt system calculated 110% of the theoretical amount of water, the washing time is 30min, after washing, the solid phase obtained by filtration is dried to obtain the potassium chloride product, and the liquid phase is the refined potassium mother liquor, which is returned to the crystallizer.

[0040] ⑨ The obtained potassium chloride product has an average particle size of 1.25 mm, a potassium chloride content of 97.0%, and a recovery rate of 78.0%.

[0041] Example 3, reference Figure 1 and 2 , a production method for preparing potassium chloride using carnallite ore Experiment 3: ① Crush the carnallite ore (containing KCl 13.4%, NaCl 53.2%, MgCl2 15.6%, and water-insoluble matter 2.3%) to less than 10 mm.

[0042] ② The crystallizer is pre-filled with mother liquor, the composition of which is Na + ,K + Mg 2+ / / Cl - -H2O quaternary water-salt system metastable phase diagram KCl, NaCl and carnallite three-phase co-saturation point mother liquor composition, the main component mass content is K + 1.78%,Na + 0.65%,Mg 2+ 6.64%, Cl - 20.97%.

[0043] ③ The crushed material is transported to the crystallizer, and at the same time, the overflow of thickener I, the seed crystals returned from the material separation operation, the refined potassium mother liquor and fresh water from the washing and filtration operation are added. The potassium ion content of the bottom flow liquid phase of the crystallizer is controlled to be no more than 2.5% by adjusting the amount of fresh water.

[0044] ④ The spiral chute is used for grading operation, and the grading particle size is controlled to be 0.10mm. The fine-grained materials enter the thickener I together with the crystallizer overflow, and the coarse-grained materials enter the distributor.

[0045] ⑤ Add fresh water to thickener I and adjust the amount of fresh water to control the potassium ion content in the overflow to no more than 3.0%.

[0046] ⑥ The coarse-grained material enters the distributor, and the distributor separates 60% of the material as seeds and returns to the crystallizer.

[0047] ⑦ The remaining 40% of the material in the distributor operation enters the flotation operation, and the overflow of the thickener II is used for slurry adjustment. The flotation operation adopts a process flow of primary roughing and secondary concentrating. The product in the tank is tailings slurry, which enters the thickener II. The overflow of the thickener II returns to the flotation operation. The foam product of the flotation operation is the concentrate slurry, which enters the filtration and dehydration operation, and the filtrate returns to the flotation operation. The solid phase enters the washing operation.

[0048] ⑧ The amount of water added for washing operation is based on Na + ,K + Mg 2+ / / Cl - -H2O quaternary water-salt system calculated 110% of the theoretical amount of water, the washing time is 30min, after washing, the solid phase obtained by filtration is dried to obtain the potassium chloride product, and the liquid phase is the refined potassium mother liquor, which is returned to the crystallizer.

[0049] ⑨ The obtained potassium chloride product has an average particle size of 1.25 mm, a potassium chloride content of 95.5%, and a recovery rate of 72.0%.

[0050] Example 4, reference Figure 2 , a production method for preparing potassium chloride using carnallite ore Experiment 4: ① Classifier bottom flow rate 10m 3 / h enters the distributor from the feed port; ②Control and adjust the baffle to the appropriate position; ③The flow rate of outlet 1 is 4.0 3 / h, and transported back to the crystallizer by a pump; The rest of the methods are the same as the experiments.

[0051] Example 5, a production method for preparing potassium chloride using carnallite ore Experiment 5: ① Classifier bottom flow rate 10m 3 / h enters the distributor from the feed port; ② The distributor adopts a three-way pipe fitting, and outlet 1 is equipped with a control valve; ③ Adjust the control valve so that the flow rate of outlet 1 is 4.0 3 / h, and transported back to the crystallizer by a pump; The rest of the methods were the same as in Experiment 2.

Claims

1. A production method for preparing potassium chloride using carnallite, characterized in that: During the crystallization operation, the method adds classification operation and material separation operation to the bottom flow of the crystallizer, and removes most of the fine mud and excessive fine crystals through the classification operation; through the material separation operation, a part of the crystallized potassium chloride particles are returned to the crystallizer as seeds, and the rest enters the flotation operation to obtain potassium chloride concentrate.

2. The production method according to claim 1, characterized in that: During the grading operation, the grading particle size is controlled at 0.074mm~0.15mm.

3. The production method according to claim 1, characterized in that The specific steps are as follows: Crush the carnallite to less than -10mm; add the crushed carnallite to the crystallizer, add an appropriate amount of fresh water, add the overflow from the thickener 1 to the crystallizer, add the return material from the distributor as a seed crystal to the crystallizer, and return the refined potassium filtrate from the filtration to the crystallizer; The crystallizer bottom flow enters the classification operation, and the classification particle size is controlled at 0.074mm~0.15mm. The coarse-grained material enters the material separation operation, and the fine-grained material enters the thickener I together with the crystallizer overflow; the material separation operation divides the material into two parts, one part is returned to the crystallizer as a seed, and the rest enters the flotation operation; The froth product of the flotation operation is the concentrate, which enters the filtration and dehydration operation, and the filtrate returns to the flotation operation; the product in the tank is the tailings slurry, which enters the thickener II, and the overflow of the thickener II returns to the flotation operation, and the underflow of the thickener II is the flotation tailings; The concentrated ore after filtration enters the washing process, and after adding fresh water for washing, it enters the filtering process again. The liquid phase is the refined potassium filtrate, which returns to the crystallizer, and the solid phase is dried to obtain the potassium chloride product.

4. The production method according to claim 1, 2 or 3, characterized in that: The equipment used for classification operations is screening equipment for classification by particle size or equipment for classification by fluid dynamic characteristics.

5. The production method according to claim 1, characterized in that: The material dividing equipment used in the material dividing operation is a three-way pipe fitting, with the material inlet at the top and the material outlets at both sides of the bottom, and an adjusting baffle is provided inside.

6. The production method according to claim 1, characterized in that: During the material splitting operation, the ratio of the material returned to the crystallizer accounts for 10% to 90% of the underflow material of the crystallizer.

7. The production method according to claim 6, characterized in that: During the material splitting operation, the ratio of the material returned to the crystallizer is preferably 30% to 70% of the underflow material of the crystallizer.

8. The production method according to claim 1, characterized in that: Clean water is added to the crystallizer to control the potassium ion content in the bottom flow liquid phase of the crystallizer to no more than 2.5%.

9. The production method according to claim 1, characterized in that: Add an appropriate amount of clean water to the thickener I to control the potassium ion content of the thickener overflow liquid phase to be no higher than 3.0%.