Waste catalyst recovery process
Through the full process of the microliquid membrane reactor core, the high energy consumption and low recovery rate of titanium element recovery in waste denitrification catalysts are solved, and the preparation of high-purity titanium dioxide is realized, with high efficiency, low energy consumption and good performance characteristics.
Patent Information
- Application Number
- CN202410911952.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, the method of separating and extracting titanium elements from waste denitrification catalysts has problems such as high energy consumption, complex process, low recovery rate of titanium elements and low product purity.
Adopt a full-process recycling process with microliquid membrane reactor as the core, including liquid-solid mixing module, vacuum spraying device, liquid-solid reaction module and membrane separator. The efficient recycling of titanium elements is achieved through alkaline dissolution and pickling treatment, and the preparation is carried out. High purity titanium dioxide.
It has achieved high efficiency and low energy consumption recovery of titanium elements. It has high purity, low silicon and aluminum content, uniform particle size distribution, and good physical and chemical properties. The vanadium and tungsten recovery rate can exceed 90% and the titanium dioxide yield is >98%.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure HDA0004933885290000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling waste denitration catalysts, and in particular to a waste catalyst powder recycling process. Background Art
[0002] Titanium dioxide has a wide range of uses, covering batteries, electronic components, catalysts and other fields. In the battery industry, titanium dioxide's high ionic conductivity and chemical stability make it a candidate material for high-performance batteries; in the field of optical and electronic device research and development, titanium dioxide is used to prepare optical devices and electronic components due to its special structure and optical properties; in the field of catalysts, titanium dioxide's high specific surface area and chemical stability make it have great potential in catalyst design and reaction control, and can be used as a catalyst or catalyst carrier.
[0003] With the increase in my country's efforts to prevent and control air pollution and the large-scale promotion of denitration technology, the amount of denitration catalyst used and the total amount of deactivated denitration catalyst have increased sharply year by year. At present, the main methods of separating and extracting V, W, Ti and other components from non-renewable deactivated denitration catalysts are chemical methods such as dry or wet methods to achieve resource utilization. However, the research work on resource utilization in China is mostly at the basic research stage, and a complete set of resource utilization technology has not yet been formed. Patent (CN 114573022A) discloses a method for preparing high-purity nano titanium dioxide using the enhanced mixing and reaction capacity of a three-stage emulsification device. The method uses water washing, acid hydrolysis, and alkaline hydrolysis to obtain high-purity sodium titanate, and then acid hydrolyzes the sodium titanate to obtain metatitanic acid, and finally roasts to obtain high-purity nano titanium dioxide. The method has a short process flow, is easy to be mass-produced and stabilized, and the obtained product has a high purity and good physical properties. However, this method requires a three-stage emulsification device, which has high requirements for equipment. The patent (CN 106011478A) discloses a sodium roasting-leaching method, in which the waste denitration catalyst is mixed with Na2CO3 and roasted to obtain a titanium-rich material, which is then acidified and hydrolyzed to obtain metatitanic acid. This method achieves the effective separation of V, W, Al, Si, etc. from Ti, and inhibits the occurrence of early hydrolysis, but the reaction requires high-temperature roasting and high-concentration acidification, resulting in high energy consumption, difficulty in waste liquid treatment, and low purity of the final product, and low recovery rate of titanium element. Therefore, it is of great significance to develop a process technology with simple process, low energy consumption, high product purity and good performance for the recovery and utilization of titanium element in waste denitration catalyst. Summary of the invention
[0004] In view of the problems of high energy consumption, complex process, low yield of titanium element and low purity of products in the current method of separating and extracting titanium element from waste denitration catalyst, a full-process recovery process design with micro-liquid membrane reactor as the core is carried out to achieve the separation of high-priced tungsten and vanadium components from titanium components and complete the preparation of high-purity titanium dioxide. The overall process flow is short and the energy consumption is low; at the same time, the product obtained by the present invention has high purity, low silicon and aluminum content, large specific surface area, uniform particle size distribution, and good physical and chemical properties.
[0005] The full-process recovery process of the present invention mainly includes a liquid-solid mixing module-vacuum spraying device, a liquid-solid reaction module-micro liquid membrane reactor (including a temperature control device), and a liquid-solid separation module-membrane separator.
[0006] The vacuum spraying device is used to mix the alkaline solution and the waste denitration catalyst powder so that they are in full and uniform contact, so as to improve the alkaline hydrolysis efficiency.
[0007] The micro-liquid membrane reactor (including the temperature control device) can suppress the occurrence of inhomogeneity in the reaction system, reduce the adverse effects of internal diffusion during the leaching of valuable metal ions, and improve the leaching rate of metal ions. The temperature control device can achieve continuous temperature increase.
[0008] The membrane separator is used for rapid and efficient liquid-solid separation.
[0009] The specific continuous operation steps of the full-process recovery process are:
[0010] A. Efficient separation and recovery of tungsten and vanadium
[0011] The spent denitrification catalyst sample powder is purged, washed, dried, crushed and sieved and placed in a vacuum spray device. Alkali solution is then added for full contact. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0012] B. Purification of high titanium slag phase
[0013] The Si, Al and other impurity components in the slag phase are further removed by alkaline leaching in a micro-liquid membrane reactor, and the silicon, aluminum and other impurity components in the leached slag are converted into corresponding soluble salts, and then a high-purity solid phase titanate intermediate is obtained by a membrane separator.
[0014] C. Preparation of high-purity ultrafine titanium dioxide carrier
[0015] A micro-liquid membrane reactor was used to separate the nucleation and crystallization processes of the titanium dioxide precursor, to achieve rapid acid hydrolysis of titanate, and metatitanic acid was calcined at 600°C in a muffle furnace for 4 hours to prepare titanium dioxide in batches.
[0016] In the steps, the alkali solution is NaOH, Na2CO3 or NH4OH, the concentration of the alkali solution is 10-50wt.%, the liquid-to-solid ratio is 5:1-20:1mL / g, the temperature is 90-150°C, the reaction time is 10-30min, and the stirring rate is 3000-6000rpm.
[0017] In the step, the acid leaching solution is HNO3, HCl, H2SO4 or H2C2O4, the acid solution has a concentration of 10-30wt.%, a temperature of 90-130°C, a reaction time of 5-30min, and a stirring rate of 2000-5000rpm.
[0018] Beneficial effects of the present invention:
[0019] The present invention provides a full-process device for separating and recovering titanium from waste denitration catalysts. The process design is centered on a micro-liquid membrane reactor to carry out engineering research on the resource utilization of deactivated catalysts. Based on the characteristics of the micro-liquid membrane reactor, forced micro-mixing strengthens the separation process, improves the leaching rate of metal ions, significantly reduces the leaching time, and the vanadium and tungsten recovery rate can exceed 90%. In addition, a micro-liquid membrane reactor is used to control the formation of primary ecological particles of titanium dioxide precursors, and a titanium dioxide carrier with uniform particle size distribution is obtained through the separation of nucleation and growth processes, with a titanium dioxide content of >98%. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a schematic diagram of the process of the present invention
[0021] Figure 2 is the XRD diffraction pattern of the metatitanic acid powder prepared in Example 1-3 of the present invention;
[0022] Figure 3 is a morphology photograph and particle size distribution diagram of titanium dioxide powder prepared in an embodiment of the present invention; DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0024] In the following examples, the main chemical components of the spent denitration catalyst used are shown in Table 1.
[0025] Table 1 Main chemical components of spent denitrification catalyst
[0026]
[0028] Example 1
[0029] A. The spent denitrification catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then a 30wt.% NaOH solution is added to fully contact the spent denitrification catalyst at a liquid-solid ratio of 5:1mL / g. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor, and the temperature is set at 140°C, the reaction time is 20min, and the stirring rate is 3500rpm to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0030] B. The high-titanium slag phase obtained in step A is further purified by adding 30wt.% NaOH solution and the high-titanium slag phase into a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1mL / g for sufficient reaction. The temperature is set at 130°C, the reaction time is 15min, and the stirring rate is 4000rpm. The impurity components such as silicon and aluminum in the leached slag are converted into corresponding soluble salts, and then high-purity solid-phase titanate is obtained through a membrane separator.
[0031] C. A 20wt% H2SO4 solution and the solid phase titanate powder obtained in step B were added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 10:1 mL / g. The reaction temperature was set at 120°C, the reaction time was 20 min, and the stirring rate was 3500 rpm to achieve rapid acid hydrolysis of the titanate. The obtained metatitanic acid was calcined at 600°C in a muffle furnace for 4 h to stabilize the batch and prepare high-end titanium dioxide.
[0032] Example 2
[0033] A. The spent denitrification catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then a 40wt.% NaOH solution is added to fully contact the spent denitrification catalyst at a liquid-solid ratio of 20:1mL / g. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor, and the temperature is set at 150°C, the reaction time is 15min, and the stirring rate is 4500rpm to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0034] B. The high-titanium slag phase obtained in step A is further purified by adding 30wt.% Na2CO3 solution and the high-titanium slag phase into a micro-liquid membrane reactor at a liquid-solid ratio of 5:1mL / g for sufficient reaction. The temperature is set at 130°C, the reaction time is 20min, and the stirring rate is 4000rpm. The impurity components such as silicon and aluminum in the leached slag are converted into corresponding soluble salts, and then high-purity solid phase titanate is obtained through a membrane separator.
[0035] C. A 20wt% HNO3 solution and the solid phase titanate powder obtained in step B were added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1 mL / g. The reaction temperature was set at 110°C, the reaction time was 20 min, and the stirring rate was 4000 rpm to achieve rapid acid hydrolysis of the titanate. The obtained metatitanic acid was calcined at 600°C in a muffle furnace for 4 h to stabilize the batch and prepare high-end titanium dioxide.
[0036] Example 3
[0037] A. The spent denitrification catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then 50wt.% Na2CO3 solution is added to fully contact the spent denitrification catalyst at a liquid-solid ratio of 15:1mL / g. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor, and the temperature is set at 150°C, the reaction time is 20min, and the stirring rate is 4000rpm to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0038] B. The high-titanium slag phase obtained in step A is further purified by adding 30wt.% NaOH solution and the high-titanium slag phase into a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1mL / g for sufficient reaction. The temperature is set at 130°C, the reaction time is 20min, and the stirring rate is 4000rpm. The impurity components such as silicon and aluminum in the leached slag are converted into corresponding soluble salts, and then high-purity solid phase titanate is obtained through a membrane separator.
[0039] C. A 25wt% HCl solution and the solid phase titanate powder obtained in step B were added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1 mL / g. The reaction temperature was set at 120°C, the reaction time was 20 min, and the stirring rate was 4000 rpm to achieve rapid acid hydrolysis of the titanate. The obtained metatitanic acid was calcined at 600°C in a muffle furnace for 4 h to prepare high-end titanium dioxide in batches for stabilization.
[0040] Example 4
[0041] A. The spent denitrification catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then a 40wt.% NaOH solution is added to fully contact the spent denitrification catalyst at a liquid-solid ratio of 15:1mL / g. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor, and the temperature is set at 130°C, the reaction time is 20min, and the stirring rate is 5000rpm to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0042] B. The high-titanium slag phase obtained in step A is further purified by adding 50wt.% NH4OH solution and the high-titanium slag phase into a micro-liquid membrane reactor at a liquid-solid ratio of 5:1mL / g for sufficient reaction. The temperature is set at 130°C, the reaction time is 20min, and the stirring rate is 5500rpm. The impurity components such as silicon and aluminum in the leached slag are converted into corresponding soluble salts, and then high-purity solid phase titanate is obtained through a membrane separator.
[0043] C. A 30wt% H2C2O4 solution and the solid phase titanate powder obtained in step B were added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1 mL / g. The reaction temperature was set at 130°C, the reaction time was 30 min, and the stirring rate was 4500 rpm to achieve rapid acid hydrolysis of the titanate. The obtained metatitanic acid was calcined at 600°C in a muffle furnace for 4 h to stabilize the batch and prepare high-end titanium dioxide.
[0044] Example 5
[0045] A. The spent denitrification catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then a 50wt.% NaOH solution is added to fully contact the spent denitrification catalyst at a liquid-solid ratio of 20:1mL / g. The evenly mixed liquid-solid mixture enters a micro-liquid membrane reactor, and the temperature is set to 150°C, the reaction time is 25min, and the stirring rate is 4500rpm to achieve efficient leaching of tungsten and vanadium metal ions. The leachate is then passed through a membrane separator to obtain a high-titanium slag phase.
[0046] B. The high-titanium slag phase obtained in step A is further purified by adding 30wt.% NaOH solution and the high-titanium slag phase into a micro-liquid membrane reactor at a liquid-solid ratio of 5:1mL / g for sufficient reaction. The temperature is set at 150°C, the reaction time is 20min, and the stirring rate is 5000rpm. The impurity components such as silicon and aluminum in the leached slag are converted into corresponding soluble salts, and then high-purity solid phase titanate is obtained through a membrane separator.
[0047] C. A 30wt% HNO3 solution and the solid phase titanate powder obtained in step B were added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 5:1 mL / g. The reaction temperature was set at 130°C, the reaction time was 30 min, and the stirring rate was 4000 rpm to achieve rapid acid hydrolysis of the titanate. The obtained metatitanic acid was calcined at 600°C in a muffle furnace for 4 h to stabilize the batch and prepare high-end titanium dioxide.
[0048] Table 2 Main indicators of metatitanic acid in the examples
[0049]
[0050] By comparing the XRF analysis data of the products of Examples 1-5 in Table 2, it can be seen that the method of the present invention can recover a metatitanic acid product having a titanium dioxide content of >98%, a silicon content of <0.02%, and an aluminum content of <0.01% from the waste denitration catalyst by alkaline hydrolysis and acid washing of the waste denitration catalyst powder. At the same time, through analysis and calculation, the specific surface area of the metatitanic acid in all the embodiments is between 150 and 280 m 2 / g, particle size is less than 10μm, and titanium dioxide yield is >90%.
[0051] The full-process recovery process method with a micro-liquid membrane reactor as the core adopted in the present invention is conducive to recovering the titanium element in the waste denitration catalyst in the form of a metatitanic acid product. Figure 2 The XRD diffraction pattern of the metatitanic acid prepared in Example 1-3 is shown in FIG. Figure 2 It can be seen that in Examples 1-3, the XRD characteristic peak positions of the products are consistent with those of anatase phase titanium dioxide, but due to the presence of crystalline water and surface hydroxyl groups in hydrated titanium dioxide, the crystal plane peaks of metatitanic acid are somewhat broadened compared to the characteristic peaks of anatase phase titanium dioxide, and the degree of crystallinity is lower.
[0052] The metatitanic acid powder prepared by the present invention includes titanium dioxide and other components which are basically derived from waste denitration catalysts. Therefore, the metatitanic acid of the present invention can be directly used to prepare titanium dioxide as a carrier of denitration catalysts or further remove impurities to prepare titanium element products such as high-purity titanium dioxide, thereby reducing the input cost of raw materials for preparing denitration catalysts on the one hand, and reducing the waste of metal elements in waste denitration catalysts on the other hand, which is more economical and environmentally friendly.
Claims
1. A process for recovering a waste denitration catalyst, characterized in that: The steps are: A. Efficient separation and recovery of tungsten and vanadium The spent denitration catalyst sample powder obtained by purging, washing, drying, crushing and sieving is placed in a vacuum spray device, and then alkali solution is added for contact, and the liquid-solid mixture after uniform mixing enters a micro-liquid membrane reactor for reaction to achieve leaching of tungsten and vanadium metal ions, and the leaching liquid is then passed through a membrane separator to obtain a high-titanium slag phase; the alkali solution is a solution of NaOH, Na2CO3 or NH4OH, the alkali solution has a concentration of 10-50wt.%, a liquid-solid ratio of 5:1-20:1mL / g, a temperature of 90-150°C, a reaction time of 10-30min, and a stirring rate of 3000-6000rpm; B. Purification of high titanium slag phase The impurity components in the slag phase are further removed by alkaline leaching in a micro-liquid membrane reactor, and the impurity components in the leached slag are converted into corresponding soluble salts, and then solid phase titanate is obtained by a membrane separator; the leaching liquid is a solution of HNO3, HCl, H2SO4, and H2C2O4, the concentration of the leaching liquid is 10-30wt.%, the temperature is 90-130°C, the reaction time is 5-30min, and the stirring rate is 2000-5000rpm; C. Preparation of high-purity ultrafine titanium dioxide carrier An acid solution with a concentration of 20wt%-30wt% and the solid phase titanate powder obtained in step B are added to a micro-liquid membrane reactor at a liquid-to-solid ratio of 5-10:1mL / g, the reaction temperature is set at 110-130°C, the reaction time is 20-30min, and the stirring rate is 4000-5000rpm to achieve rapid acid hydrolysis of the titanate, and the obtained metatitanic acid is calcined to obtain titanium dioxide.