Recycling process of waste vanadium-titanium denitration catalyst
Through high-pressure water rinsing and multi-step chemical treatment, the recycling efficiency and compound types of waste vanadium titanium denitrification catalysts have been successfully improved, and the high-purity extraction of various compounds has been achieved, solving the problems of low recycling efficiency and limited compound types in the prior art. , enhances the economic value of waste catalysts.
Patent Information
- Application Number
- CN202410868477.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art has low efficiency in recycling and reuse of waste denitrification catalysts, limited types of compounds, and difficult to achieve economic recycling.
After rinsing and crushing with high-pressure water, the waste vanadium titanium denitrification catalyst is reacted in dilute sulfuric acid and NaHSO3, the pH and temperature are controlled, and filtration and precipitation are carried out through multiple steps to produce titanium dioxide, tungsten trioxide, molybdenum trioxide, vanadium pentoxide and other compounds. , and crystals of sodium sulfate and sodium chloride were obtained by evaporation, thereby improving the recovery efficiency and purity of the compound.
High-purity extraction of various compounds has been achieved, the economic value of waste vanadium titanium denitrification catalyst has been improved, the problem of separation of tungsten and molybdenum has been solved, and the recycling cost has been reduced.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of environmental protection recycling, and specifically relates to a recycling process for waste vanadium-titanium denitration catalysts. Background Art
[0002] With the rapid development of industrialization, large-scale emissions of nitrogen oxides have caused many air pollution problems such as acid rain, photochemical smog, and haze. Selective oxidation-reduction technology (SCR) has been widely used in the field of denitrification. Currently, about 140,000 tons of SCR denitrification catalysts are discarded each year, which can be converted into a volume of up to 250,000 cubic meters. The regeneration or resource utilization of discarded denitrification catalysts has become a problem that needs to be solved urgently. Waste denitrification catalysts can usually be regenerated 2 to 3 times, and then they can only be completely scrapped. How to achieve the recycling of discarded denitrification catalysts is an urgent need for technicians in this field; Patent application number CN201510014516.6 discloses an acid leaching reduction method for comprehensive utilization of waste denitration catalysts. The waste denitration catalysts are crushed, and then hydrochloric acid or sulfuric acid is added to the waste denitration catalysts. At the same time, a reducing agent is added to heat the leaching, and the obtained acid leaching filtrate is filtered. The pH of the acid leaching filtrate is adjusted with alkaline solution to obtain a crude vanadium product. Finally, the crude vanadium precipitate is dissolved in a nitric acid solution of a certain concentration, boiled to cause an oxidation reaction, and a vanadium pentoxide product is generated in the solution. Although this method has a simple process and realizes the comprehensive utilization of waste denitration catalysts, its recovery efficiency is limited, the types of compounds recycled and reused are small, and the recovery process still needs further improvement. Summary of the invention
[0003] The purpose of the present invention is to provide a recycling process for waste vanadium titanium denitration catalysts, which can improve the recovery efficiency and the types of recycled compound products, give the waste vanadium titanium denitration catalysts economic value, and realize the recycling of waste vanadium titanium denitration catalysts.
[0004] The present invention provides the following technical solutions: A process for recycling waste vanadium-titanium denitration catalyst, the steps are as follows: S1. The waste vanadium titanium denitrification catalyst is washed with high-pressure water to remove dust and impurities. The high washing pressure is 100-110 MPa and the washing time is 10-15 min. Then, it is crushed into 20-80 meshes by a crusher. The speed of the crusher is 20-30 r / min and the crushing time is 0.5-1 h. S2, adding the crushed waste vanadium titanium denitration catalyst to dilute sulfuric acid and NaHSO3; controlling the pH to 3-4 and the temperature to 80-90°C, and then reacting for 3-4 hours, filtering to obtain filtrate 1 and filter residue 2; the mass ratio of the waste vanadium titanium denitration catalyst to NaHSO3 is 1:190-200; Add sodium hydroxide to the filter residue 2 at room temperature until it is completely dissolved, the mass ratio of sodium hydroxide to the filter residue 2 being 1:5, and then filter to obtain titanium dioxide and filtrate 2; S3, add dilute sulfuric acid to the filtrate 2 to adjust the pH value to 4-5, react for 1-2 hours to generate a precipitate, filter the precipitate to obtain tungsten trioxide or molybdenum trioxide, and filtrate 3.
[0005] S4. Add sodium hydroxide to the filtrate 1 in a volume ratio of 1:1 to the filtrate 1, wait for a precipitate to be generated, filter to obtain a filtrate 4 and a filter residue 3; put the filter residue 3 into a sodium hydroxide solution in a mass ratio of 1:5 to the filter residue 3, then introduce oxygen into the sodium hydroxide solution to react for 1 to 2 hours, wait for the filter residue 3 to be completely dissolved; add ammonium chloride to react for 1 to 2 hours to generate a precipitate, filter to obtain a filtrate 5 and a precipitate respectively, and roast the precipitate at 500 to 600° C. for 20 to 40 minutes to obtain vanadium pentoxide.
[0006] Preferably, the waste vanadium titanium denitrification catalyst is washed with high-pressure water to remove dust and impurities, the high washing pressure is 105 MPa, and the washing time is 12 minutes; then it is crushed into 50 mesh using a crusher, the crusher speed is 25 r / min, and the crushing time is 0.7 hours.
[0007] Preferably, the crushed waste vanadium titanium denitrification catalyst is added with dilute sulfuric acid and NaHSO3; the pH is controlled to be 3.5, the temperature is 85°C, and then the reaction is carried out for 3.5 hours, and the filtrate 1 and the filter residue 2 are obtained by filtering; the mass ratio of the waste vanadium titanium denitrification catalyst to NaHSO3 is 1:195.
[0008] Preferably, dilute sulfuric acid is added to the filtrate 2 to adjust the pH value to 4.5, and the reaction is carried out for 1.5 hours to generate a precipitate, which is filtered to obtain tungsten trioxide or molybdenum trioxide and filtrate 3.
[0009] Preferably, sodium hydroxide is added to the filtrate 1 in a volume ratio of 1:1 to the filtrate 1, and a precipitate is generated, and the filtrate 4 and the filter residue 3 are obtained by filtering; the filter residue 3 is put into a sodium hydroxide solution in a mass ratio of 1:5 to the filter residue 3, and then oxygen is introduced into the sodium hydroxide solution for reaction for 1.5 hours, and the filter residue 3 is completely dissolved; ammonium chloride is added to react for 1.5 hours to generate a precipitate, and the filtrate 5 and the precipitate are respectively obtained by filtering, and the precipitate is roasted at 550° C. for 30 minutes to obtain vanadium pentoxide.
[0010] Preferably, filtrate 3 is evaporated and crystallized at 120-150°C for 1-2 hours to obtain sodium sulfate crystals. filtrate 4 is evaporated and crystallized at 120-150°C for 1-2 hours to obtain sodium sulfate crystals. filtrate 5 is evaporated and crystallized at 120-150°C for 1-2 hours to obtain sodium chloride crystals.
[0011] Beneficial effects of the present invention: 1. The present invention realizes the recovery and purification of titanium dioxide, tungsten trioxide, molybdenum trioxide, sodium chloride, sodium sulfate and other compounds with high purity through the synergistic effect of various process parameters; 2. The present invention purifies vanadium pentoxide from waste vanadium titanium denitration catalysts, and the vanadium pentoxide has high purity; at the same time, titanium dioxide can be used as a raw material for synthesizing titanium dioxide in the chlorination process, greatly improving the economic value of waste vanadium titanium denitration catalysts.
[0012] 3. The present invention solves the problem of difficulty in separating tungsten and molybdenum, and reduces the recycling cost by recycling tungsten trioxide and molybdenum trioxide together. DETAILED DESCRIPTION Example 1
[0013] A process for recycling waste vanadium-titanium denitration catalyst, the steps are as follows: First, 10 kg of the waste vanadium titanium denitrification catalyst was washed with high-pressure water to remove dust and impurities, the high washing pressure was 100 MPa, and the washing time was 10 minutes; then it was crushed into 20 meshes using a crusher, the crusher speed was 20 r / min, and the crushing time was 0.5 h; The crushed waste vanadium titanium denitration catalyst was added with dilute sulfuric acid and NaHSO3; the pH was controlled to be 3 and the temperature was 80°C, and then reacted for 3 hours, and filtered to obtain filtrate 1 and filter residue 2; the mass ratio of the waste vanadium titanium denitration catalyst to NaHSO3 was 1:190; sodium hydroxide was added to the filter residue 2 at room temperature until it was completely dissolved, and the mass ratio of sodium hydroxide to filter residue 2 was 1:5, and then filtered to obtain 0.63 kg of titanium dioxide (HPLC was 96%) and filtrate 2; Dilute sulfuric acid was added to filtrate 2 to adjust the pH value to 4, and the reaction was continued for 1 hour to generate a precipitate, which was filtered to obtain 1.61 kg of tungsten trioxide and molybdenum trioxide (HPLC: 90%) and filtrate 3. Filtrate 3 was evaporated and crystallized at 120°C for 1 hour to obtain 0.26 kg of sodium sulfate crystals (HPLC: 86%).
[0014] Sodium hydroxide was added to the filtrate 1 in a volume ratio of 1:1 to the filtrate 1, and a precipitate was formed, which was filtered to obtain a filtrate 4 and a filter residue 3; the filtrate 4 was evaporated and crystallized at 120° C. to obtain 0.28 kg of sodium sulfate crystals (HPLC: 86%).
[0015] The filter residue 3 was put into a sodium hydroxide solution, the mass ratio of the sodium hydroxide solution to the filter residue 3 was 1:5, and then oxygen was introduced into the sodium hydroxide solution for reaction for 1 hour until the filter residue 3 was completely dissolved; ammonium chloride was added for reaction for 1 hour to generate a precipitate, which was filtered to obtain a filtrate 5 and a precipitate respectively, and the precipitate was roasted at 500°C for 20 minutes to obtain 2.91 kg of vanadium pentoxide (HPLC: 95%). The filtrate 5 was evaporated and crystallized at 120°C for 1 hour to obtain 0.55 kg of sodium chloride crystals (HPLC: 91%). Example 2
[0016] A process for recycling waste vanadium-titanium denitration catalyst, the steps are as follows: 10 kg of waste vanadium titanium denitrification catalyst was washed with high-pressure water to remove dust and impurities, the high washing pressure was 105 MPa, and the washing time was 12 minutes; then it was crushed into 50 meshes using a crusher, the crusher speed was 25 r / min, and the crushing time was 0.7 hours; The crushed waste vanadium titanium denitration catalyst was added with dilute sulfuric acid and NaHSO3; the pH was controlled to be 3.5 and the temperature was 85°C, and then the reaction was carried out for 3.5 hours, and the filtrate 1 and the filter residue 2 were obtained by filtration; the mass ratio of the waste vanadium titanium denitration catalyst to NaHSO3 was 1:195; sodium hydroxide was added to the filter residue 2 at room temperature until it was completely dissolved, and the mass ratio of sodium hydroxide to the filter residue 2 was 1:5, and then 0.68 kg of titanium dioxide (HPLC was 97%) and the filtrate 2 were obtained by filtration; Dilute sulfuric acid was added to filtrate 2 to adjust the pH value to 4.5, and the reaction was continued for 1.5 hours to generate a precipitate, which was filtered to obtain 1.63 kg of tungsten trioxide and molybdenum trioxide (HPLC: 91%) and filtrate 3. Filtrate 3 was evaporated and crystallized at 145°C for 1.5 hours to obtain 0.28 kg of sodium sulfate crystals (HPLC: 88%).
[0017] Sodium hydroxide was added to the filtrate 1 in a volume ratio of 1:1, and a precipitate was formed, which was filtered to obtain a filtrate 4 and a filter residue 3; the filtrate 4 was evaporated and crystallized at 120-150° C. for 1-2 h to obtain 0.31 kg of sodium sulfate crystals (HPLC: 87%).
[0018] The filter residue 3 was put into a sodium hydroxide solution, the mass ratio of the sodium hydroxide solution to the filter residue 3 was 1:5, and then oxygen was introduced into the sodium hydroxide solution for reaction for 1.5 hours until the filter residue 3 was completely dissolved; ammonium chloride was added for reaction for 1.5 hours to generate a precipitate, and the filtrate 5 and the precipitate were obtained by filtration, and the precipitate was roasted at 550°C for 30 minutes to obtain 3.08 kg of vanadium pentoxide (HPLC: 95%). The filtrate 5 was evaporated and crystallized at 145°C for 1.5 hours to obtain 0.58 kg of sodium chloride crystals (HPLC: 92%). Example 3
[0019] A recycling process for waste vanadium titanium denitration catalysts, comprising the following steps: washing 10 kg of waste vanadium titanium denitration catalysts with high-pressure water to remove dust and impurities, wherein the high washing pressure is 108 MPa and the washing time is 13 minutes; then crushing the waste vanadium titanium denitration catalysts into 75 meshes using a crusher, the crusher speed is 28 r / min, and the crushing time is 0.8 hours; The crushed waste vanadium titanium denitration catalyst was added with dilute sulfuric acid and NaHSO3; the pH was controlled to be 3.8 and the temperature was 88°C, and then the reaction was carried out for 3.7 hours, and the filtrate 1 and the filter residue 2 were obtained by filtration; the mass ratio of the waste vanadium titanium denitration catalyst to NaHSO3 was 1:198; sodium hydroxide was added to the filter residue 2 at room temperature until it was completely dissolved, and the mass ratio of sodium hydroxide to the filter residue 2 was 1:5, and then 0.54 kg of titanium dioxide (HPLC was 94%) and the filtrate 2 were obtained by filtration; Dilute sulfuric acid was added to filtrate 2 to adjust the pH value to 4.7, and the reaction was continued for 1.8 hours to generate a precipitate, which was filtered to obtain 1.61 kg of tungsten trioxide and molybdenum trioxide (HPLC: 91%) and filtrate 3. Filtrate 3 was evaporated and crystallized at 147°C for 1.8 hours to obtain 0.25 kg of sodium sulfate crystals (HPLC: 86%).
[0020] Sodium hydroxide was added to filtrate 1 in a volume ratio of 1:1. After a precipitate was formed, filtrate 4 and filter residue 3 were obtained by filtration. Filtrate 4 was evaporated and crystallized at 147° C. for 1.8 h to obtain 0.26 kg of sodium sulfate crystals (HPLC: 88%).
[0021] The filter residue 3 was put into a sodium hydroxide solution, the mass ratio of the sodium hydroxide solution to the filter residue 3 was 1:5, and then oxygen was introduced into the sodium hydroxide solution for reaction for 1.8 hours until the filter residue 3 was completely dissolved; ammonium chloride was added for reaction for 2 hours to generate a precipitate, which was filtered to obtain a filtrate 5 and a precipitate respectively, and the precipitate was roasted at 580°C for 37 minutes to obtain 2.87 kg of vanadium pentoxide (HPLC: 93%). The filtrate 5 was evaporated and crystallized at 147°C for 1.8 hours to obtain 0.53 kg of sodium chloride crystals (HPLC: 92%). Example 4
[0022] A recycling process for waste vanadium titanium denitration catalysts, comprising the following steps: washing 10 kg of waste vanadium titanium denitration catalysts with high-pressure water to remove dust and impurities, wherein the high washing pressure is 110 MPa and the washing time is 15 min; then crushing the waste vanadium titanium denitration catalysts into 80 meshes using a crusher, the crusher speed is 30 r / min, and the crushing time is 1 h; Add dilute sulfuric acid and NaHSO3 to the crushed waste vanadium titanium denitration catalyst; control the pH to 4 and the temperature to 90°C, then react for 4 hours, filter to obtain filtrate 1 and filter residue 2; the mass ratio of waste vanadium titanium denitration catalyst to NaHSO3 is 1:200; add sodium hydroxide to filter residue 2 at room temperature until it is completely dissolved, the mass ratio of sodium hydroxide to filter residue 2 is 1:5, and then filter to obtain 0.59 kg of titanium dioxide (HPLC is 93%) and filtrate 2; Dilute sulfuric acid was added to filtrate 2 to adjust the pH value to 5, and the reaction was continued for 2 hours to generate a precipitate, which was filtered to obtain 1.63 kg of tungsten trioxide and molybdenum trioxide (HPLC: 90%) and filtrate 3. Filtrate 3 was evaporated and crystallized at 150°C for 2 hours to obtain 0.26 kg of sodium sulfate crystals (HPLC: 86%).
[0023] Sodium hydroxide was added to filtrate 1 in a volume ratio of 1:1. After a precipitate was formed, filtrate 4 and filter residue 3 were obtained by filtration. Filtrate 4 was evaporated and crystallized at 150° C. for 2 h to obtain 0.28 kg of sodium sulfate crystals (HPLC: 86%).
[0024] The filter residue 3 was put into a sodium hydroxide solution, the mass ratio of the sodium hydroxide solution to the filter residue 3 was 1:5, and then oxygen was introduced into the sodium hydroxide solution for reaction for 2 hours until the filter residue 3 was completely dissolved; ammonium chloride was added for reaction for 2 hours to generate a precipitate, and the filtrate 5 and the precipitate were obtained by filtration, and the precipitate was roasted at 600°C for 40 minutes to obtain 2.89 kg of vanadium pentoxide (HPLC: 94%). The filtrate 5 was evaporated and crystallized at 150°C for 2 hours to obtain 0.55 kg of sodium chloride crystals (HPLC: 90%).
[0025] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for recycling waste vanadium-titanium denitration catalyst, characterized in that: Here are the steps: S1. The waste vanadium titanium denitrification catalyst is washed with high-pressure water to remove dust and impurities. The high washing pressure is 100-110 MPa and the washing time is 10-15 min. Then, it is crushed into 20-80 meshes by a crusher. The speed of the crusher is 20-30 r / min and the crushing time is 0.5-1 h. S2, adding the crushed waste vanadium titanium denitration catalyst to dilute sulfuric acid and NaHSO3; controlling the pH to 3-4 and the temperature to 80-90°C, and then reacting for 3-4 hours, filtering to obtain filtrate 1 and filter residue 2; the mass ratio of the waste vanadium titanium denitration catalyst to NaHSO3 is 1:190-200; Add sodium hydroxide to the filter residue 2 at room temperature until it is completely dissolved, the mass ratio of sodium hydroxide to the filter residue 2 being 1:5, and then filter to obtain titanium dioxide and filtrate 2; S3, add dilute sulfuric acid to the filtrate 2 to adjust the pH value to 4-5, react for 1-2 hours to generate a precipitate, filter the precipitate to obtain tungsten trioxide or molybdenum trioxide, and filtrate 3; S4. Add sodium hydroxide to the filtrate 1 in a volume ratio of 1:1 to the filtrate 1, wait for a precipitate to be generated, filter to obtain a filtrate 4 and a filter residue 3; put the filter residue 3 into a sodium hydroxide solution in a mass ratio of 1:5 to the filter residue 3, then introduce oxygen into the sodium hydroxide solution to react for 1 to 2 hours, wait for the filter residue 3 to be completely dissolved; add ammonium chloride to react for 1 to 2 hours to generate a precipitate, filter to obtain a filtrate 5 and a precipitate respectively, and roast the precipitate at 500 to 600° C. for 20 to 40 minutes to obtain vanadium pentoxide.
2. A process for recycling waste vanadium-titanium denitration catalyst according to claim 1, characterized in that: The waste vanadium-titanium denitrification catalyst was washed with high-pressure water to remove dust and impurities. The high washing pressure was 105MPa and the washing time was 12min. Then it was crushed into 50 meshes by a crusher. The speed of the crusher was 25r / min and the crushing time was 0.7h.
3. A process for recycling waste vanadium-titanium denitration catalyst according to claim 1, characterized in that: The crushed waste vanadium titanium denitrification catalyst was added with dilute sulfuric acid and NaHSO3; the pH was controlled to be 3.5 and the temperature was 85°C, and then reacted for 3.5 hours, and filtered to obtain filtrate 1 and residue 2; the mass ratio of the waste vanadium titanium denitrification catalyst to NaHSO3 was 1:
195.
4. A process for recycling waste vanadium-titanium denitration catalyst according to claim 1, characterized in that: Add dilute sulfuric acid to the filtrate 2 to adjust the pH value to 4.5, react for 1.5 hours to generate a precipitate, filter the precipitate to obtain tungsten trioxide or molybdenum trioxide and filtrate 3.
5. A process for recycling waste vanadium-titanium denitration catalyst according to claim 1, characterized in that: Sodium hydroxide was added to the filtrate 1 in a volume ratio of 1:1 to the filtrate 1, and a precipitate was generated, which was filtered to obtain a filtrate 4 and a filter residue 3; the filter residue 3 was put into a sodium hydroxide solution in a mass ratio of 1:5 to the filter residue 3, and then oxygen was introduced into the sodium hydroxide solution to react for 1.5 hours until the filter residue 3 was completely dissolved; ammonium chloride was added to react for 1.5 hours to generate a precipitate, and the filtrate 5 and the precipitate were respectively obtained by filtering, and the precipitate was roasted at 550° C. for 30 minutes to obtain vanadium pentoxide.
6. A process for recycling waste vanadium-titanium denitration catalyst according to claim 4, characterized in that: The filtrate 3 is evaporated and crystallized at 120-150° C. for 1-2 hours to obtain sodium sulfate crystals.
7. A process for recycling waste vanadium-titanium denitration catalyst according to claim 5, characterized in that: The filtrate 4 is evaporated and crystallized at 120-150° C. for 1-2 hours to obtain sodium sulfate crystals.
8. A process for recycling waste vanadium-titanium denitration catalyst according to claim 5, characterized in that: The filtrate 5 is evaporated and crystallized at 120-150°C for 1-2 hours to obtain sodium chloride crystals.
9. A process for recycling waste vanadium-titanium denitration catalyst according to any one of claims 6 to 8, characterized in that: Evaporative crystallization was carried out at 145°C for 1.5 h.
