Preparation of composite flocculant based on volcanic minerals and application of composite flocculant in phosphorus removal

The preparation of composite silicon-aluminum-iron flocculants using volcanic rock minerals solves the problems of high cost and easy deactivation of existing flocculants, providing an efficient and low-cost water treatment solution, especially excelling in phosphorus removal.

CN118878036APending Publication Date: 2024-11-01CHINA RAILWAY URBAN CONSTR GRP THE 1ST ENG CORP LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411160263.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing flocculants are expensive and ineffective, making it difficult to meet increasingly stringent water treatment requirements. Polysilicate flocculants are prone to deactivation during storage, affecting their application.

Method used

A composite silicon-aluminum-iron flocculant was prepared by using volcanic rock minerals as raw materials through acid leaching and alkalization processes, including calcination, acid leaching and alkalization steps, optimizing the metal ion compounding to form a structurally stable flocculant.

Benefits of technology

A low-cost, environmentally friendly flocculant with excellent flocculation performance was prepared, which can effectively remove phosphorus from water, improve water treatment efficiency, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878036A_ABST
    Figure CN118878036A_ABST
Patent Text Reader

Abstract

The invention relates to preparation of a composite flocculant based on volcanic rock minerals and application of the composite flocculant in phosphorus removal. The preparation method comprises the following steps: an acid leaching process: taking hydrochloric acid, heating, pouring volcanic rock powder, starting stirring, continuously heating, keeping the temperature, continuously stirring, taking out a beaker, standing, and filtering to obtain yellow liquid, namely volcanic rock acid leaching liquid; and an alkalization process: placing the volcanic rock pickle liquor on an electromagnetic heating stirrer, slowly dropwise adding a sodium hydroxide solution into a beaker, continuously stirring, taking out, standing and curing at room temperature, and observing oil yellow liquid, namely the composite silicon-aluminum-iron flocculating agent. Volcanic rock is adopted as a raw material to prepare the composite silicon-aluminum-iron flocculating agent, and the preparation method of the composite flocculating agent is low in price, environmentally friendly, economical and effective.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and in particular relates to the preparation of a composite flocculant based on volcanic rock minerals and its application in phosphorus removal. Background Art

[0002] Water is known as the source of life. It is not only an important cornerstone for ensuring people's normal life, but also carries the potential for urban development. At present, the treatment of some polluted water sources in my country has not achieved good results. Such problems seriously threaten the safety of residents' drinking water. Long-term drinking or use of polluted water will endanger residents' health. At present, my country's residents' water mainly comes from rivers, lakes and groundwater. What is worrying is that among the seven major water systems, up to 40% of the river sections are not suitable for drinking water sources, especially in industrially developed towns, where river pollution is particularly serious, of which 78% of urban river sections are not suitable for drinking water sources. The main cause of this problem is the discharge of domestic sewage and industrial and agricultural production wastewater. When these wastewaters are discharged into the water body beyond its self-purification capacity, water pollution problems will be caused, which will eventually threaten the safety of residents' drinking water and endanger people's health. The World Health Organization's survey report shows that water pollution is related to 80% of human diseases. Drinking water contaminated by microorganisms can spread a variety of water-borne infectious diseases, such as diarrhea, cholera, dysentery, typhoid and poliomyelitis, which causes 485,000 deaths from diarrhea every year. Current research shows that the main factor affecting the growth of microorganisms in water is phosphorus in water. When the phosphorus content in water is too high, algae and microorganisms in water will multiply in large numbers, consume dissolved oxygen in water, and cause the death of other organisms in water, eventually polluting the water and endangering people's lives and health. Therefore, removing phosphorus from water while removing suspended pollutants in water has become an important issue of concern in the process of water environment management.

[0003] At present, the main water treatment methods in life are divided into three types: physical, chemical and biological. The physical method refers to the use of physical methods to separate pollutants in water, mainly including filtration, membrane filtration, activated carbon adsorption, etc.; the chemical method uses chemical principles to remove pollutants in water, mainly including flocculation, ion exchange, etc.; the biological method is to decompose organic matter in water through the action of microorganisms, thereby achieving the purpose of controlling water pollution, mainly including biofilm reactors and biological contact oxidation methods.

[0004] Compared with other water treatment methods, flocculation is widely used because of its simple process and high efficiency. However, although there are many types of flocculants on the market, their effects are uneven. With the increasing pollution of water resources, the treatment effects of many flocculants have begun to fail to meet the requirements of water treatment. Therefore, it is necessary to study a new type of flocculant to overcome the shortcomings of traditional flocculants in the field of water treatment, so as to adapt to the continuous increase in the scale of water treatment in the future and the improvement of the requirements for treated water quality indicators.

[0005] With the development and progress of society, the public's concept of protecting the environment has become stronger and stronger. Faced with the deteriorating water resources, the government has also successively issued relevant regulations and policies to strengthen the prevention and control of water pollution and water pollution control. At present, conventional flocculants have begun to fail to meet the needs of sewage treatment. Some flocculants with excellent flocculation performance are expensive, and their application in actual sewage treatment procedures increases production costs. Therefore, a low-cost flocculant product with good flocculation performance is needed to deal with the problems arising in the current development of the water treatment field.

[0006] Polysilicate is an old flocculant, but its development is far behind that of conventional aluminum-based and iron-based flocculants. One of the main reasons is that polysilicate flocculants will further polymerize and become inactivated during storage. Due to its poor stability, the application of polysilicate flocculants in the field of water treatment is limited. Experimental studies have found that the introduction of metal cations on the basis of polysilicate flocculants can greatly improve the disadvantage of polysilicate being easily polymerized and inactivated. Polysilicate-based flocculants are flocculants generated by polymerizing metal salt solutions with polysilicate solutions. Different metal salts introduced into polysilicate can make the generated flocculants have different water treatment effects. Due to its unique network structure and high molecular weight characteristics, polysilicate, after combining with metal salt ions, gives the finished flocculant similar structural advantages, and effectively overcomes the defect of polysilicate being easily inactivated, thus showing excellent performance in the water treatment process. Volcanic rocks, as a widely existing mineral resource in mines, are rich in key elements such as silicon, aluminum, and oxygen. Their high content of beneficial components indicates great application potential. The use of volcanic rocks to prepare polysilicate-based flocculants not only has a solid scientific basis, but also reflects the environmental protection concept of resource recycling. It is worth noting that the existence form of silicon in volcanic rocks is particularly stable, which provides favorable conditions for the preservation of the form of silicon after extraction. Under physical and chemical effects, silicon extracted from volcanic rocks is compounded with elements such as aluminum and iron to form a more stable complex than synthetic flocculants such as traditional silicates. This stability directly improves the overall efficiency of the flocculant. Therefore, optimizing the morphological distribution of silicon compounds in volcanic rocks to promote good compounding and efficient flocculation between metal ions has become the key to improving water treatment effects. The optimization of this process is not only related to the further improvement of flocculant performance, but also has important significance for water resource protection and water environment management. By precisely controlling the extraction and compounding conditions, it is expected to develop new flocculants with better performance, lower cost and environmental friendliness, bringing revolutionary changes to the field of water treatment. At present, there are few studies on the preparation of flocculants from volcanic rocks, which deserves special attention. Summary of the invention

[0007] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is: how to prepare a flocculant with low cost and good flocculation performance.

[0008] In order to solve the above technical problems, the present invention adopts the following technical scheme: a method for preparing a composite flocculant based on volcanic rock minerals, comprising the following steps: acid leaching process: take hydrochloric acid with a concentration of 3 to 4 mol / L, heat it to 50 to 90°C, pour it into volcanic rock powder, then start stirring and continue heating to 90 to 120°C, maintain the temperature and continue stirring for 2 to 3 hours, take out the beaker and let it stand overnight, and the yellow liquid obtained after filtration is the required volcanic rock acid leaching solution, and the mass ratio of volcanic rock powder to hydrochloric acid volume is 1:10 to 1:15.

[0009] Alkalization process: Take the volcanic rock acid extract, place it on an electromagnetic heating stirrer, slowly add 2-3 mol / L sodium hydroxide solution into the beaker, control the polymerization temperature to 20-100°C, continue stirring for 0.17-4h, then take it out and let it stand and mature at room temperature for 24-36h. An oily yellow liquid is observed, which is the composite silicon-aluminum-iron flocculant. The volume ratio of sodium hydroxide solution to volcanic rock acid extract is: 1.2-1.6.

[0010] Furthermore, the volcanic rock is calcined at 200-600° C. for 1-2 hours, taken out after calcination, cooled to room temperature, and ground into powder for later use.

[0011] A composite flocculant based on volcanic rock minerals is used in phosphorus removal. The composite silicon-aluminum-iron flocculant is used for water treatment, and the dosage of the composite silicon-aluminum-iron flocculant is 0.5mL / L-5mL / L.

[0012] Compared with the prior art, the present invention has at least the following advantages:

[0013] (1) A composite silicon-aluminum-iron flocculant was prepared using volcanic rock as raw material, and a low-cost, environmentally friendly, and cost-effective composite flocculant preparation method mechanism was obtained. Volcanic rock is a natural resource. The flocculant prepared using it as raw material has the advantages of low cost, environmental friendliness, and renewability. Its preparation process is simple, the raw materials are easily available, and it can be mass-produced, reducing the cost of water treatment. Through laboratory tests and field tests, the treatment effect and stability of the composite flocculant were evaluated, and its feasibility in practical applications was determined.

[0014] (2) The structure-activity relationship between the structure of the composite silicon-aluminum-iron flocculant and the flocculation effect of typical pollutants was revealed. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The effect of calcination temperature on flocculation performance.

[0016] Figure 2 The effect of acid leaching temperature on flocculation performance.

[0017] Figure 3 This is the effect of the type of alkalizer on the flocculation effect.

[0018] Figure 4 The effect of alkali dosage on flocculation performance.

[0019] Figure 5 The effect of polymerization time on flocculation performance.

[0020] Figure 6 The effect of polymerization temperature on flocculation effect.

[0021] Figure 7The effect of alkali dosage on the flocculation effect of PSAC.

[0022] Figure 8 The effect of polymerization temperature on the flocculation effect of PSAC.

[0023] Fig. 9 This is the effect of silicate on the flocculation effect of PSAC.

[0024] Fig.10 The effect of aging time on the flocculation effect of PSAC.

[0025] Fig.11 The effect of pH on the flocculation effect of PSAC.

[0026] Fig.12 Comparison of PSAC flocculation performance under different water quality conditions.

[0027] Fig.13 The distribution of aluminum forms in flocculants at different temperatures.

[0028] Fig.14 The distribution of aluminum forms in the presence of different amounts of alkali and silicon-containing / silicon-free flocculants.

[0029] Fig.15 SEM, EDS and element ratio diagram of volcanic rock.

[0030] Fig.16 SEM, EDS and element ratio diagram of PSAC.

[0031] Fig.17 SEM and element ratio diagram of PSAC-desiliconization.

[0032] Fig.18 These are the FTIR graphs of volcanic rock, PSAC, and PSAC-desiliconized materials, where the horizontal axis is the wave number and the vertical axis is the transmittance.

[0033] Fig.19 It is the XPS spectrum before and after flocculation, where the abscissa is the binding energy and the ordinate is the relative intensity.

[0034] Fig. 20 This is a peak diagram of silicon, aluminum, iron, oxygen, and phosphorus elements, where the horizontal axis is binding energy and the vertical axis is relative intensity. DETAILED DESCRIPTION

[0035] The present invention is described in further detail below.

[0036] A composite flocculant based on volcanic rock minerals, the preparation process of which includes calcination of volcanic rock, acid leaching process and alkalization process.

[0037] When exploring the preparation process of composite silicon-aluminum-iron flocculants, we focused on the fine control of the two core steps of acid leaching and alkalization, in order to maximize the extraction and efficient utilization of effective components in volcanic rocks. The acid leaching process, as the beginning of the preparation process, can not only effectively strip key metal elements such as aluminum, iron, and silicon from volcanic rocks, but also ensure the reasonable distribution of silicon elements in the system through fine control, laying a solid foundation for subsequent polymerization reactions. The key to this process is to accurately set parameters such as the type, concentration, treatment temperature, and time of the acid solution to achieve deep mining and component optimization of the raw materials. Subsequently, the introduction of the alkalization step is to further sublimate the acid leaching product. At this stage, by cleverly adjusting the type, amount, reaction temperature, and pH value of the alkali solution, we significantly enhanced the hydrolysis activity of metal ions, promoted the interaction and deep polymerization between elements such as aluminum, iron, and silicon, and formed a composite flocculant with stable structure and superior performance. This process not only optimizes the compounding effect between the components, but also promotes the formation of the optimal polymerization morphology, so that the flocculant exhibits stronger flocculation ability and wider adaptability in subsequent applications. It is worth noting that in response to the common impurity problem in volcanic rock raw materials, we introduced a pretreatment step of high-temperature calcination at the beginning of preparation. This innovative measure effectively removed the adverse components in the raw materials, improved the acid leaching efficiency of the effective components, and laid a good raw material foundation for the preparation of high-quality composite silicon-aluminum-iron flocculants. In summary, the preparation process of composite silicon-aluminum-iron flocculants is a complex system engineering that combines science and artistry. By precisely controlling the two key steps of acid leaching and alkalization, we have successfully mastered the compounding mechanism with iron, silicon, aluminum and other main metal elements, which not only surpassed the limitations of traditional silica-based control technology, but also achieved the enrichment of flocculant components and significant improvement in performance. This breakthrough in preparation technology has undoubtedly brought more efficient and environmentally friendly solutions to water treatment and related fields, showing broad application prospects and market potential.

[0038] The calcination process is to calcine the volcanic rock at 200-600° C. for 1-2 hours, take it out after calcination, cool it to room temperature, and grind it into powder for standby use; the acid leaching process is to take 200-300 ml of hydrochloric acid with a concentration of 3-4 mol / L, heat it to 50-90° C., pour 20-30 g of volcanic rock powder into it, then start stirring and continue heating to 90-120° C., keep the temperature and continue stirring for 2-3 hours, take out the beaker and let it stand overnight, and the yellow liquid obtained after filtration is the required volcanic rock acid leaching solution; the alkalization process is to take 10 ml of the acid leaching solution and put it in a beaker, put it on an electromagnetic heating stirrer, slowly add 4-16 ml of 2-3 mol / L sodium hydroxide solution into the beaker, control the polymerization temperature to 20-100° C., continue stirring for 0.17-4 hours, take it out, and let it stand and mature for 24-36 hours at room temperature.

[0039] Embodiment 1: A method for preparing a composite flocculant based on volcanic rock minerals, comprising the following steps:

[0040] Calcination: Calcine the volcanic rock at 200°C for 1 hour. After calcination, take it out and cool it to room temperature, then grind it into powder for later use.

[0041] Acid leaching process: Take 200ml of 3mol / L hydrochloric acid, heat it to 50℃, pour in 20g of volcanic rock powder, then start stirring and continue heating to 50℃, maintain the temperature and continue stirring for 2h, take out the beaker and let it stand overnight, and the yellow liquid obtained after filtering is the required volcanic rock acid leaching solution.

[0042] Alkalization process: Take 10 ml of volcanic rock acid extract, place it on an electromagnetic heating stirrer, slowly add 12 ml of 3 mol / L sodium hydroxide solution into the beaker, control the polymerization temperature to 20°C, continue stirring for 0.17h, then take it out and let it stand and mature at room temperature for 24h. An oily yellow liquid is observed, which is the composite silicon-aluminum-iron flocculant (PSAC).

[0043] The steps of Example 2 to Example 11 are the same as those of Example 1, and the only difference is the amount of raw materials and process parameters, as shown in Table 1.

[0044]

[0045] 1. Experimental Methods

[0046] Coagulation experiments were used to explore the influence of preparation conditions on the flocculation performance of flocculants. In the experiment, the water from Yuehu Lake of Hunan University of Science and Technology was taken as the target treatment object. Because it is a natural surface water body, there are certain fluctuations in the initial water quality parameters in the experiment. The specific coagulation experimental method and experimental parameters are as follows: Take 1L of Yuehu water sample and use an automatic coagulator for the experiment. Set the rapid stirring time to 1min, and the rapid stirring rate to 300r / min. Set the slow stirring time to 15min, and the slow stirring rate to 70r / min. After the coagulation and stirring are completed, let it stand for 30min, and take the clarified water sample 3-4cm below the supernatant surface to determine its residual turbidity. Filter the supernatant with a 0.45μm syringe filter, and use a double-beam UV spectrophotometer to measure UV at a wavelength of 254nm. 254 .

[0047] 2. Study on factors affecting preparation conditions

[0048] In the preparation process of composite silicon-aluminum-iron flocculant, the acid leaching liquid needs to be alkalized to make it have flocculation ability. Therefore, the synthesis conditions of the flocculant have a great influence on the coagulation effect of the flocculant. Therefore, in the preparation process, it is necessary to explore and determine the optimal preparation conditions of the composite silicon-aluminum-iron flocculant through single-factor experiments. The volcanic rock calcination temperature, acid leaching temperature, alkali type, alkali dosage, polymerization time and polymerization temperature in the preparation process are selected to explore the influence of preparation conditions on the coagulation effect of the composite silicon-aluminum-iron flocculant. In the determination stage, the turbidity and UV in the water are used. 254 The removal effect is used as the evaluation criterion for the coagulation effect of composite silicon-aluminum-iron flocculant.

[0049] (1) Effect of calcination temperature

[0050] The flocculant is prepared by calcining volcanic rocks to remove impurities contained in them so that more effective components can be leached out during acid leaching. The variables selected in the experiment are calcination temperatures, which are set to uncalcined, 200°C, 400°C, and 600°C respectively. The acid leaching temperature and acid leaching time are set to 90°C and 2h, and the polymerization time and polymerization temperature are set to 10min and 60°C. 12mL of 2mol / L sodium hydroxide solution is added dropwise as an alkalization condition. Coagulation experiments were carried out, and the selected dosages were 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. The composite silicon-aluminum-iron flocculant prepared from volcanic rocks calcined at different temperatures was observed to remove turbidity and UV in water. 254 The ability of volcanic rock was analyzed to obtain the influence of calcination of volcanic rock on the coagulation effect of composite silicon-aluminum-iron flocculant.

[0051] like Figure 1 As shown in the figure, the PSAC flocculants prepared from calcined and uncalcined volcanic rocks have an effect on turbidity and UV in water. 254 All of them have good removal effects. The PSAC flocculants made of volcanic rocks calcined at different temperatures have a good effect on turbidity and UV in water. 254 There is no significant difference in the removal effect. As the amount of flocculant added gradually increases, the turbidity and UV 254 The removal effect shows a trend of first increasing and then decreasing. Figure 1 As shown in (a), under the same dosage conditions, the change of calcination temperature has no obvious effect on the removal of turbidity in water by PSAC flocculant. Within a certain dosage range, as the dosage of flocculant increases, the turbidity in water decreases significantly. When the dosage reaches 1.5mL / L, the removal effect reaches the best. As the dosage continues to increase, the residual turbidity in the water begins to rise, and an obvious anti-stabilization phenomenon occurs. Figure 1As shown in (b), the PSAC flocculants prepared at different calcination temperatures all had a significant effect on UV absorption in water when the dosage was 2 mL / L. 254 The removal effect is the best, and the residual UV 254 The concentration of PSAC was controlled in the range of 0.02 to 0.04, and the PSAC flocculants prepared by uncalcined and calcined at 400℃ had the highest effect on UV in water. 254 When the dosage of flocculant is greater than 2mL / L, the removal effect of UV 254 The removal effect began to decline, and an obvious anti-stabilization phenomenon appeared.

[0052] It can be seen that calcining volcanic rocks cannot effectively remove impurities in the material. Considering the removal effect of pollutants in water and the concept of energy saving and environmental protection, it is chosen not to calcine volcanic rocks as the preparation condition for preparing PSAC flocculants in subsequent experiments.

[0053] (2) Effect of acid leaching temperature

[0054] Heating during acid leaching can increase the leaching rate of effective components in volcanic rocks, and improve the flocculation performance by increasing the concentration of effective components in the composite silicon-aluminum-iron flocculant. The variables selected in the experiment are the acid leaching temperature, which are set to 50°C, 70°C, and 90°C respectively. The acid leaching time is set to 2h, and the polymerization time and polymerization temperature are set to 10min and 60°C. 12mL of 2mol / L sodium hydroxide solution is added as the alkalinization condition. A coagulation experiment was carried out, and the dosage selected in the experiment was 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. Observe the composite silicon-aluminum-iron flocculant prepared from the acid leaching solution obtained at different acid leaching temperatures to remove turbidity and UV in water. 254 The ability of acid leaching temperature was analyzed to obtain the influence of the flocculation performance of PSAC flocculant.

[0055] like Figure 2 As shown in the figure, the effect of different acid leaching temperatures on the removal of turbidity in water is slightly different. 254 There are great differences in the removal effect. When the acid leaching temperature is 50℃, the prepared PSAC flocculant has no obvious flocculation effect. Figure 2As shown in (a), when the dosage is in the range of 0.5 to 2.5 mL / L, the PSAC flocculant prepared under 90°C acid leaching conditions has a slightly better turbidity removal effect. As the dosage continues to increase, an obvious anti-stabilization phenomenon occurs. When the dosage exceeds 2.5 mL / L, the PSAC flocculant prepared under 70°C acid leaching conditions begins to surpass the turbidity removal effect, and the flocculation effect does not appear anti-stabilization with the increase of the head volume, and the residual turbidity in the water fluctuates within a certain range. Figure 2 (b) shows the effects of two flocculants on UV 254 Although the final removal effects of the two samples were similar, there were significant differences in the dosage. The optimal dosage of PSAC prepared under 90°C acid leaching conditions was 1.5 mL / L, after which the anti-stabilization phenomenon began to occur. The optimal dosage of PSAC prepared under 70°C acid leaching conditions was 4 mL / L. Moreover, the two samples had different effects on UV at different dosages. 254 The removal effects of PSAC vary greatly. As for the overall effect, the PSAC prepared under 90℃ acid leaching conditions has better effect.

[0056] It can be seen that at different acid leaching temperatures, the concentration of effective components in the acid leaching solution will be different, resulting in differences in the flocculation effect of the prepared PSAC flocculant. Considering the dosage and the removal effect of pollutants in water, the acid leaching temperature of 90°C was finally selected as the optimal preparation condition for preparing PSAC flocculants in subsequent experiments.

[0057] (3) Influence of alkalizing agent type

[0058] In the experiment, calcium oxide and sodium hydroxide were selected as alkalizing agents to prepare PSAC flocculants. The variable selected in the experiment was the type of alkalizing agent, and 8mL and 12mL of 2mol / L sodium hydroxide solution and 2mol / L calcium oxide suspension were added respectively. The acid leaching temperature and acid leaching time were set to 90℃ and 2h, and the polymerization time and polymerization temperature were set to 10min and 60℃. A coagulation experiment was carried out, and the dosage selected in the experiment was 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. Observe the composite silicon-aluminum-iron flocculants prepared with different alkalizing agents to remove turbidity and UV in water. 254 The ability of alkalizing agents was analyzed to obtain the influence of different alkalizing agents on the flocculation performance of composite silicon-aluminum-iron flocculant.

[0059] like Figure 3 As shown in the figure, PSAC flocculants alkalized with CaO and NaOH have good removal effects on turbidity in water, but have poor removal effects on UV 254However, there are large differences in the removal effects. Overall, the PSAC flocculant alkalized with NaOH has a better overall removal effect on pollutants in water. Figure 3 As shown in (a), 8mL CaO and 8mL NaOH alkaline PSAC flocculants can achieve the best turbidity removal effect at a dosage of 1.5mL / L. As the dosage continues to increase, the turbidity removal effect of 8mL NaOH alkaline PSAC flocculant will show an obvious trend of first increasing and then weakening. The turbidity removal effects of the other three flocculants fluctuate within a certain range with the increase in dosage, and the residual turbidity is controlled within the range of 0.7 to 2NTU. Figure 3 (b) shows the effects of four PSAC flocculants on UV 254 The removal effects of 8mL NaOH alkalized flocculants and 8mL CaO alkalized flocculants showed obvious inverse stability with the increase of dosage. In the dosage range of 0-2.2mL, the removal effects of NaOH alkalized flocculants on UV 254 The removal effect of PSAC flocculant with 12mL NaOH and CaO was better than that of the alkaline flocculant with CaO. 254 The removal effect of UV will gradually stabilize with the increase of dosage. 254 The removal effect is the best, and the residual UV in the water 254 The concentration is less than 0.02.

[0060] It can be seen that the alkalizer has an effect on the removal of UV in water by PSAC flocculant. 254 The effect on the removal of turbidity is more obvious, but the effect on the turbidity removal effect is smaller. 254 Based on the removal effect and the dosage, NaOH was selected to alkalize the acid leaching solution as the optimal preparation condition for preparing PSAC flocculant in subsequent experiments.

[0061] (4) Effect of alkali dosage

[0062] Alkalization is an important step in the preparation of silicon-aluminum-iron flocculants. Appropriate alkalization can promote the hydrolysis reaction of metal ions in the flocculant. The variable selected in the experiment is the dosage of sodium hydroxide solution, and 4mL, 8mL, 12mL, and 16mL of 2mol / L sodium hydroxide solution are added dropwise. The acid leaching temperature and acid leaching time are set to 90℃ and 2h, and the polymerization time and polymerization temperature are set to 10min and 60℃. A coagulation experiment was carried out, and the dosage selected in the experiment was 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. Observe the effect of composite silicon-aluminum-iron flocculants prepared with different alkali dosages on removing turbidity and UV in water. 254 The ability of alkali dosage was analyzed to obtain the influence of alkali dosage on the flocculation performance of PSAC flocculant.

[0063] like Figure 4 As shown in the figure, the amount of alkali used has a great influence on the removal effect of PSAC flocculant on pollutants in water. The flocculation performance of PSAC alkalized with 4mL NaOH shows great volatility with the increase of the dosage, such as Figure 4 As shown in (a), PSAC-4mL first reaches the best turbidity removal effect with the increase of dosage, but then the phenomenon of anti-stabilization will soon appear. With the continued increase of dosage, the turbidity removal effect begins to number and gradually stabilizes. This may be caused by incomplete alkalization of PSAC. Although the turbidity removal effect of PSAC-8mL will also show the phenomenon of anti-stabilization with the increase of dosage, the overall turbidity removal effect is relatively stable. When the dosage is 1.5mL / L, the best turbidity removal effect is achieved and the residual turbidity is controlled below 1NTU. The turbidity removal effects of the other two flocculants show a trend of first increasing and then stabilizing. The turbidity removal effects of both are best when the dosage is 5mL / L. Figure 4 As shown in (b), PSAC-16mL has the worst flocculation effect. PSAC-4mL and PSAC-8mL flocculants can flocculate UV in water at a lower dosage. 254 It has a good removal effect and can remove UV in water 254 The content was controlled below 0.02. PSAC-12mL also achieved similar removal effects in the experiment, but the required dosage reached 5mL / L, which was much larger than the dosage required for the other two flocculants.

[0064] It is known that the amount of alkali has a significant effect on the flocculation performance of the PSAC flocculant. The impurity removal effect of incompletely alkalized PSAC is unstable, and there is a large fluctuation with the increase of dosage. Within a certain range, the higher the degree of alkalization, the better the flocculation performance of PSAC and the better the removal effect of pollutants in water. Based on the removal effect of pollutants in water and the dosage factor, the alkalization condition of NaOH-8mL was selected as the optimal preparation condition for the subsequent synthesis of PSAC.

[0065] (5) Influence of polymerization time

[0066] The variable selected in the experiment is the polymerization time, which is set to 0h, 10min, 0.5h, 1h, 2h, and 4h respectively. The acid leaching temperature and acid leaching time are set to 90℃ and 2h respectively. 8mL of 2mol / L sodium hydroxide solution is added dropwise, and the polymerization temperature is set to 60℃. The coagulation experiment is carried out according to 2.4.1. The dosage selected in the experiment is 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. Observe the effect of the composite silicon-aluminum-iron flocculant prepared under different polymerization times on removing turbidity and UV in water. 254 The ability of polymerization time was analyzed to obtain the influence of the flocculation performance of the composite silicon-aluminum-iron flocculant.

[0067] like Figure 5 The results of the treatment of target water samples by flocculants prepared with different polymerization times show that PSAC flocculants can remove turbidity and UV 254 With the increase of dosage, the polymerization time has a certain influence on flocculation. The appropriate polymerization time can obtain the ideal flocculation effect. When the polymerization time is 0.5h, the flocculation effect is better. Figure 5 As shown in (a), at the same dosage, the change of polymerization time has little effect on the turbidity removal effect of PSAC flocculant. As the dosage increases, the turbidity of the water body will decrease significantly. When the dosage is greater than 3mL / L, the PSAC flocculants prepared at various polymerization times have a good removal effect on the turbidity in the water, and the residual turbidity in the water is basically maintained at about 1-1.5NTU. Figure 5 As shown in (b), at the same dosage, when the polymerization time is 1h and 0.5h, the effect of UV 254 The removal effect of the flocculant with a polymerization time of 0.5h was significantly better than that of other polymerization times, but the difference was not obvious enough. When the dosage was greater than 2.5mL / L, the flocculant with a polymerization time of 0.5h removed UV 254 The effect is slightly better than the polymerization effect with a polymerization time of 1h.

[0068] Considering the removal effect of pollutants and the factors of energy saving and environmental protection, a polymerization time of 0.5 h was selected as the optimal preparation condition for preparing PSAC flocculant in subsequent experiments.

[0069] (6) Effect of polymerization temperature

[0070] The variable selected in the experiment is the polymerization temperature, which is set to 20℃, 40℃, 60℃, 80℃, and 100℃ respectively. The acid leaching time and acid leaching temperature are set to 90℃ and 2h, 8mL of 2mol / L sodium hydroxide solution is added dropwise, and the polymerization time is set to 0.5h. The coagulation experiment was carried out according to 2.4.1. The dosage selected in the experiment was 0.5mL / L, 1mL / L, 1.5mL / L, 2mL / L, 2.5mL / L, 3mL / L, 3.5mL / L, 4mL / L, 4.5mL / L, and 5mL / L. Observe the effect of the composite silicon-aluminum-iron flocculant prepared at different polymerization temperatures on removing turbidity and UV in water. 254 The ability of polymerization temperature was analyzed to obtain the influence of the flocculation effect of PSAC flocculant.

[0071] like Figure 6 As shown in the figure, with the increase of dosage, the PSAC flocculant has a great influence on the turbidity and UV 254 The removal effect of PSAC flocculants prepared at different polymerization temperatures was not significantly different, but UV 254 The removal effect of α-hydroxy-2-nitrogen sulfide varies greatly with the change of polymerization temperature, such as Figure 6 As shown in (a), the PSAC prepared at 20°C first achieved the best turbidity removal effect when the dosage was 2ml / L, and the residual turbidity in the water was controlled below 1NTU. When the dosage was 2.5ml / L, the turbidity removal effect of the PSAC prepared at 20°C showed an anti-stabilization phenomenon, while the PSAC prepared at polymerization temperatures of 40°C, 60°C, 80°C, and 100°C all achieved good turbidity removal effects. When the dosage was 3mL / L, the residual turbidity in the water rebounded in a small range, and then gradually stabilized with the increase in dosage. Figure 6 As shown in (b), when the dosage is in the range of 1 to 1.5 mL / L, the effects of various flocculants on UV 254 There is no significant difference in the removal effect of UV in water when the dosage continues to increase and the PSAC flocculant prepared at a polymerization temperature of 60°C 254 The removal effect is the best, and the best UV removal is achieved when the dosage is 2.5mL / L. 254 It is known that too high or too low polymerization temperature will weaken the effect of PSAC flocculant on UV 254 removal effect.

[0072] It can be seen that when the polymerization temperature increases, the flocculation performance of PSAC is promoted. Considering the removal effect of pollutants, the polymerization temperature of 60 °C was selected as the optimal polymerization temperature for preparing PSAC flocculant in subsequent experiments.

[0073] 3. Study on actual water purification effect

[0074] (1) Effect of alkali dosage

[0075] Select PSAC flocculants with different amounts of NaOH added, and conduct dosage experiments according to the Al2O3 content calculated in 4.3.5 to obtain the optimal dosage range and the effect of alkali dosage on flocculation performance. The polluted water sample used in this experiment is actual sewage from a certain place, which is used to test the actual treatment effect of PSAC flocculants. The initial pH, turbidity, and UV of the sewage were measured. 254 , algae base number and total phosphorus were 7.16, 15.76NTU, and 0.209cm -1 , 0.047, 0.457mg / L. The dosage of PSAC flocculant was selected as 39mg / L, 78mg / L, 156mg / L, 312mg / L, and the removal of pollutants in water bodies with different dosages was analyzed. The results are as follows Figure 7 shown.

[0076] Figure 7 The figure shows the removal effect of pollutants in water by two flocculants with different amounts of NaOH added at different dosages. It can be seen that the removal effect of PSAC-8mL on pollutants in water is significantly better than that of PSAC-4mL. Figure 7 (a) and Figure 7 (b) As the dosage increases from 39 to 312 mg / L, the residual turbidity in the water shows a trend of first decreasing, then increasing, and then slightly decreasing. This proves that the turbidity removal effect of PSAC-4mL is not very stable. When the dosage is 78 mg / L, the turbidity removal effect is the best, and the residual turbidity is 1.01 NTU. 254 , algae, and total phosphorus have the same removal trend, and the best removal effect is achieved when the dosage is 78 mg / L, and the removal rates are 65.5%, 95.8%, and 93.4% respectively. 254 The removal rates of total phosphorus and algae decreased sharply, and only the removal rate of algae decreased slightly. When the dosage was 312 mg / L, PSAC-4mL had a significant effect on UV 254 The removal effect of total phosphorus dropped to 0, and PSAC only had a removal effect on algae in the water.

[0077] Combination Figure 7 (a) and Figure 7 (c) PSAC-8mL has a significant effect on turbidity and UV254 The removal effect of algae and total phosphorus was significantly better than that of PSAC-4mL. In the process of gradually increasing the dosage from 39 to 312 mg / L, the removal effect of pollutants in water first increased and then gradually weakened. When the dosage reached 78 mg / L, the removal effect reached the best, at which time the residual turbidity was 0.85 NTU and UV 254 The removal rates of algae and total phosphorus were 93.1%, 94.7% and 91.2% respectively. The removal rate of pollutants by PSAC-8mL did not fluctuate significantly with the increase of dosage, and the removal effect was relatively stable. However, at a dosage of 312 mg / L, the removal effect of total phosphorus would still drop to 0.

[0078] Combining the flocculation effects of the two PSACs, the effect of alkali dosage on turbidity and UV 254 The removal effect of algae and total phosphorus is greatly affected. The flocculation effect of incompletely alkalized PSAC is unstable. This is because less alkali is added and OH in the flocculant is - The decrease in concentration leads to a decrease in the hydrolysis degree of aluminum ions and their complexes in the solution, thus affecting the flocculation effect, which is verified by the above experimental results. From the overall effect, at the optimal dosage, the removal effect of PSAC-8mL on pollutants in water is significantly better than that of PSAC-4mL.

[0079] (2) Effect of polymerization temperature

[0080] PSAC flocculants with different polymerization temperatures were selected, and the dosage experiment was carried out according to the calculated Al2O3 content to obtain the optimal dosage experimental range and the influence of polymerization temperature on the actual flocculation effect. The polluted water sample used in this experiment was actual sewage from a certain place, which was used to test the actual treatment effect of PSAC flocculants. The initial pH, turbidity, and UV of the sewage were measured. 254 , algae base number and total phosphorus were 7.93, 16.13 NTU, and 0.062 cm -1 , 0.043, 0.41mg / L. The dosage of PSAC flocculant was selected as 39mg / L, 78mg / L, 156mg / L, 312mg / L, and the removal of pollutants in water bodies with different dosages was analyzed. The results are shown below.

[0081] Figure 8 The figure shows the removal effect of pollutants in water by PSAC prepared at 5 different polymerization temperatures at different dosages. It can be seen that PSAC prepared at different polymerization temperatures has a good removal effect on pollutants in water. Figure 8 (a) and Figure 8(b) As the dosage of PSAC-normal temperature gradually increased from 39 to 312 mg / L, the residual turbidity in the water showed a trend of first decreasing and then increasing. The turbidity removal effect reached the best at 156 mg / L, when the turbidity of the water body decreased from the initial 16.13 NTU to 1.38 NTU. In the same group of experiments, as the dosage gradually increased, PSAC-normal temperature had a significant effect on the UV 254 The removal effects of algae and total phosphorus have basically the same trend of change, and the removal rates of various pollutants reach the highest at a dosage of 156 mg / L, which are 92.7%, 96.5% and 75.6% respectively. When the dosage continues to increase to 312 mg / L, the removal effect of PSAC-normal temperature on various pollutants in water begins to decline. At a dosage of 312 mg / L, there is no removal effect on total phosphorus.

[0082] Combination Figure 8 (a) and Figure 8 (c) As the dosage increases from 39-312 mg / L, the residual turbidity in the water shows a trend of gradually decreasing and then increasing. At a dosage of 78 mg / L, PSAC-40℃ has the best turbidity removal effect, and its turbidity drops from the initial 16.13 NTU to 1.29 NTU. 254 The removal effect of UV 254 The removal rates of total phosphorus and algae gradually increased. When the dosage was 78 mg / L, the removal rates reached the maximum, which were 74.2% and 92.7% respectively. As the dosage continued to increase, the removal effect of pollutants in the water began to decline. The dosage used for the best algae removal effect is different from that of UV. 254 and total phosphorus, the removal rate of algae in water reached the maximum of 91.8%, and the dosage of PSAC-40℃ was 156mg / L.

[0083] Combination Figure 8 (a) and Figure 8 (d) From the above, PSAC-60℃ has a more prominent effect on the removal of pollutants in water. As the dosage gradually increases from 39 to 312 mg / L, the turbidity removal effect first becomes better and then stabilizes. The turbidity removal effect is best at a dosage of 78 mg / L, at which time the residual turbidity in the water is 0.88 NTU and the turbidity removal rate is 94.5%. With the increase in dosage, UV 254 The removal effects of algae and total phosphorus showed roughly the same trend, which was first steadily improved. When the dosage was greater than 78 mL / L, the removal effect of pollutants began to decline. When the dosage was 78 mg / L, the removal effect of pollutants in water was the best. At this time, UV 254 , algae and total phosphorus removal rates were 76.6%, 94.1% and 90.2% respectively, and residual UV 254The absorbance is 0.011 cm -1 , the residual algae base number is 0.005, and the residual total phosphorus is 0.07 mg / L. As the dosage continues to increase, UV 254 Although the removal rate of algae began to decline, it still had a good removal effect, and the removal rate of total phosphorus would drop to 0 when the dosage was 312 mg / L.

[0084] Combination Figure 8 (a) and Figure 8 (e) PSAC-80℃ UV 254 The removal effect of PSAC-80℃ on UV-ray in water was poor. When the dosage increased from 39 to 312 mg / L, the residual turbidity in the water showed a trend of decreasing first and then increasing. When the dosage was 156 mg / L, the turbidity removal effect was the best, and the turbidity dropped from the initial 16.13 NTU to 0.49 NTU. 254 The removal trend is roughly the same as that of algae. As the dosage increases, the removal of UV 254 The removal effect of algae increased steadily until the dosage increased to 156 mg / L, the removal rate reached the maximum, at this time UV 254 The removal rates of phosphide and algae were 58.9% and 93.0% respectively. The removal effect of PSAC-80℃ on total phosphorus was similar to that of UV 254 There is a difference in the removal effect between PSAC and algae. When the dosage of PSAC is 78 mg / L, the best phosphorus removal rate is 51.2%. As the dosage continues to increase, the removal effect of total phosphorus begins to gradually decrease, until the dosage increases to 312 mg / L, there is no removal effect on total phosphorus in water.

[0085] Combination Figure 8 (a) and Figure 8 (f) As the dosage of PSAC-100℃ increases from 39 to 312 mg / L, the turbidity removal effect shows a trend of first strengthening and then weakening. In the dosage range of 39 to 78 mg / L, the turbidity removal effect of PSAC-100℃ is slightly better than that of the other four PSAC flocculants. This is because the change in polymerization temperature increases the proportion of Al in PSAC and improves the degree of polymerization of PSAC. At a dosage of 78 mg / L, the turbidity removal effect is optimal, and the residual turbidity in the water is reduced to 0.82 NTU. PSAC-100℃ has a significant effect on UV 254 The removal trends of algae and total phosphorus are roughly the same. With the increase of dosage, the removal effect shows a trend of first strengthening and then weakening. When the dosage is 78 mg / L, the removal effect is the best, and the removal rates are 50.8%, 96.5% and 73.2% respectively. The algae removal effect of PSAC-100℃ will only decrease slightly with the continuous increase of dosage, but UV254 The removal effect of total phosphorus dropped to 0 at a dosage of 312 mg / L.

[0086] Effect of polymerization temperature of PSAC on turbidity and UV in water 254 The removal effect of PSAC-60℃ flocculant on pollutants is the best among the five flocculants, and it has a great influence on the removal effect of algae and total phosphorus. Within a certain range, the increase of polymerization temperature can enhance the flocculation performance of PSAC. Too high or too low polymerization temperature will lead to the weakening of the actual flocculation performance of PSAC. 254 The removal trends of total phosphorus and algae are roughly the same, and the actual flocculation effect will not fluctuate greatly with the increase of dosage.

[0087] (3) Influence of silica content

[0088] Remove the silica in PSAC to obtain PSAC-desiliconized flocculant. According to the Al2O3 content calculated in 4.3.5, the dosage experiment is carried out to obtain the optimal dosage experimental range and explore the effect of silica on the flocculation effect of PSAC. The polluted water sample used in this experiment is the actual sewage from a certain place, which is used to test the actual treatment effect of PSAC flocculant. The initial pH, turbidity, and UV of the sewage are measured. 254 , algae base number and total phosphorus were 7.15, 16.53NTU, 0.073cm -1 , 0.044, 0.443mg / L. The dosage of PSAC-containing silicon and PSAC-desiliconized flocculants was selected as 39mg / L, 78mg / L, 156mg / L, 312mg / L, and the removal of pollutants in water bodies with different dosages was analyzed. The results are shown below.

[0089] Fig. 9 The figure below shows the removal effect of pollutants in water under different dosages of two flocculants. It is not difficult to see that the overall removal effect of PSAC-containing silicon flocculant on pollutants in water is better than that of PSAC-desiliconized flocculant. Fig. 9 As shown in (a), there is a big difference in the removal effect of the two flocculants on turbidity in water. When the dosage increases from 39 to 312 mg / L, the removal effect of PSAC-containing silicon on turbidity in water will first increase and then weaken, while the removal effect of PSAC-desiliconized on turbidity in water will gradually increase until it stabilizes. The overall turbidity removal effect of PSAC-containing silicon is better than that of PSAC-desiliconized. When the two flocculants achieve the best turbidity removal effect, the dosage used is also inconsistent. PSAC-containing silicon achieves the best turbidity removal effect when the dosage is 78 mg / L, and the residual turbidity drops to 0.55 NTU, while PSAC-desiliconized achieves the best removal effect when the dosage is 156 mg / L, and the residual turbidity drops to 1.1 NTU.

[0090] like Fig. 9 As shown in (b), PSAC-silicon removal has a better removal effect on algae and UV 254 The removal effect of total phosphorus is relatively poor. As the dosage increases from 39 mg / L to 312 mg / L, the flocculation effect first increases and then gradually stabilizes. When the dosage is 312 mg / L, the removal effect of pollutants is the best. At this time, UV 254 The removal rates of algae and total phosphorus were 50.9%, 95.5% and 57.1% respectively. Fig. 9 (c) It can be seen that during the flocculation process, PSAC-containing silicon has an effect on UV 254 The removal trends of algae and total phosphorus were basically the same, which increased first and then weakened with the increase of dosage. Only the removal effect of total phosphorus changed greatly with the increase of dosage. When the dosage was 78 mg / L, the removal effect of pollutants in water was the best. The residual UV in water was 254 0.003cm -1 , algae base number is 0.004, residual total phosphorus is 0.083mg / L, UV 254 The removal rates of algae and total phosphorus were 93.2%, 98.9% and 82% respectively.

[0091] From the above experimental results, it can be seen that the presence of silicate will affect the flocculation performance of PSAC to a certain extent. Combined with SEM characterization and aluminum morphology speculation, silicate can increase the degree of polymerization of PSAC materials and increase the surface area of ​​the materials, making the Al in PSAC materials b The increase in proportion will enhance the adsorption, bridging, net capturing and sweeping capabilities of PSAC materials.

[0092] (4) Effect of aging time

[0093] Select PSAC flocculants prepared with different maturation times, and conduct dosage experiments according to the Al2O3 content calculated in 4.3.5 to obtain the optimal dosage experimental range and the effect of maturation on the PSAC flocculation effect, and determine the stability of the PSAC material. The polluted water sample used in this experiment is actual sewage from a certain place, which is used to test the actual treatment effect of the PSAC flocculant. The initial pH, turbidity, and UV of the sewage were measured. 254 , algae base number and total phosphorus were 7.64, 16.4 NTU, and 0.064 cm -1 , 0.045, 0.45mg / L. The dosage of PSAC flocculant was selected as 39mg / L, 78mg / L, 156mg / L, 312mg / L, and the removal of pollutants in water bodies with different dosages was analyzed. The results are shown below.

[0094] Fig.10The removal effect of pollutants in water by four PSAC flocculants with different aging times and different dosages is shown in Figure 1. Fig.10 (a) and Fig.10 (b) It can be seen that the dosage increased from 39 mg / L to 312 mg / L, and the PSAC-24h had a significant effect on the turbidity and UV 254 The removal effects of algae and total phosphorus showed a trend of first strengthening and then weakening. When the dosage reached 156 mg / L, the pollutant removal effect was the best, and the turbidity removal rate reached 93.9%. The removal rates of other pollutants were 70.9%, 95.6% and 86.7% respectively.

[0095] Depend on Fig.10 (a) It can be seen that the turbidity removal effect of PSAC-72h is significantly better than that of other flocculants, and when the anti-stabilization phenomenon occurs, the residual turbidity in the water only fluctuates in a small range, indicating that its turbidity removal effect is stable. The optimal dosage of PSAC-72h is 78mg / L, at which time the residual turbidity in the water drops to 0.483NTU, and the turbidity removal rate reaches 97%. Fig.10 (c) It can be seen that at each dosage, PSAC-72h can effectively remove pollutants in water and has a good effect on UV 254 The removal effect of UV was relatively stable, and only the removal rate of total phosphorus fluctuated greatly with the increase of dosage. 254 , algae and total phosphorus removal effects were optimal, and residual UV 254 Absorbance is 0.001cm -1 , the residual algae base number was 0.001, the residual total phosphorus was 0.08 mg / L, and the removal rates were 99.2%, 98.9% and 82.2% respectively. As the dosage of Daming Lake continued to increase, the removal effect of pollutants would decline, especially the removal effect of total phosphorus. When the dosage reached 312 mg / L, the removal rate of total phosphorus dropped to 0.

[0096] Depend on Fig.10 (a) It can be seen that when the aging time is 5 days and 7 days, the turbidity removal effect of PSAC on water begins to weaken, and as the dosage gradually increases from 39 to 312 mg / L, the turbidity removal effect fluctuates greatly. The longer the aging time, the more obvious the fluctuation of the turbidity removal effect. The two flocculants prepared with different aging times achieve the best turbidity removal effect when the dosage is 78 mg / L. The residual turbidity in the water is reduced to 1.167 NTU and 1.170 NTU, respectively, and the turbidity removal rates are 92.9% and 92.8%, respectively. It can be inferred that the aging time has little effect on the turbidity removal mechanism of PSAC. Fig.10 (d) and Fig.10 (e) It can be seen that the two PSAC flocculants with aging time of 5 days and 7 days have a significant effect on UV 254The removal effects of algae and total phosphorus have the same changing trend. With the increase of the dosage from 39 to 312 mg / L, they all show a trend of first strengthening and then weakening. At 78 mg / L, the best removal effect of pollutants in water is achieved, and under the condition of the optimal dosage, the flocculation effect is more considerable.

[0097] From the above experiments, we can see that the flocculation effect of PSAC flocculant will change with the aging time. This may be because there is still a certain amount of silicate in PSAC that has not polymerized with metal ions. It polymerizes and inactivates itself during the aging process, causing the spatial structure of PSAC to change and the chain structure used for flocculation to decrease, resulting in a decrease in the flocculation performance of PSAC. When the aging time is 72h, the turbidity and UV 254 , algae and total phosphorus have a high removal rate. When the aging time is short or long, PSAC still performs well at the optimal dosage, overcoming the characteristic of single polysilicate flocculant that is easy to aggregate and deactivate.

[0098] (5) pH influence

[0099] The preparation conditions of PSAC flocculant are 8mL sodium hydroxide alkalization, polymerization temperature of 60℃, and aging time of 72h. The dosage experiment is carried out according to the Al2O3 content calculated in 4.3.5. The polluted water sample used in this experiment is the actual sewage from a certain place, which is used to test the actual treatment effect of PSAC flocculant. The initial pH, turbidity, UV 254 , algae base number and total phosphorus were 7.52, 17.5NTU, 0.05cm -1 , 0.03, 0.3mg / L. The dosage of PSAC flocculant was selected as 78mg / L, and the raw water pH was adjusted to 5, 6, 7, 8, 9, 10. The removal of pollutants in water by PSAC flocculant in different pH water environments was analyzed, and the results are shown below.

[0100] Fig.11 The figure shows the removal effect of PSAC flocculant on pollutants in water under different pH conditions. Fig.11 (a) It can be seen that with the increase of pH, the residual turbidity fluctuates, first decreasing and then gradually increasing. When pH = 5-6, the turbidity removal effect of PSAC is weak, and the residual turbidity in the water is 4.80NTU and 4.45NTU, respectively. When pH = 7-8, the turbidity removal effect in the water is better, and the residual turbidity begins to drop significantly. At this time, the residual turbidity in the water drops to 0.64NTU and 0.87NTU, and the turbidity removal rates are 96.3% and 95%, respectively. When the pH continues to increase, the turbidity removal effect begins to gradually weaken, and the residual turbidity in the water increases slightly. It can be seen that in neutral and alkaline water bodies, PSAC has a better effect on turbidity removal in water. From Fig.11 (b) It can be seen that PSAC has a significant effect on UV 254 The flocculation removal trends of algae and total phosphorus were basically the same. With the increase of pH, the removal rate showed a trend of first increasing and then decreasing. When pH = 7-8, the removal rate of UV 254 The removal effects of algae and total phosphorus were the best, with removal rates of 97%, 96.6% and 100% (pH = 7), 94.7%, 98.3% and 100% respectively. 254 Absorbance is 0.002cm -1 , residual algae base number is 0.001, residual total phosphorus is 0 mg / L (pH=7), residual UV 254 Absorbance is 0.003cm -1 , the residual algae base number is 0.001, and the residual total phosphorus is 0 mg / L (pH = 8). When the pH continues to increase, the UV 254 , algae and total phosphorus removal effects rebounded, but the effect was still better than the removal effect of water pollutants under pH = 5-6 conditions.

[0101] From the above results, it can be seen that the PSAC flocculant has better flocculation performance in neutral and alkaline environments, and has a better effect on removing pollutants in water. This is because the flocculation performance of PSAC mainly depends on the hydrolysis reaction of aluminum ions and their complexes. In neutral and alkaline water bodies, the OH- concentration is relatively high, which can promote the hydrolysis reaction and enhance the flocculation performance of PSAC.

[0102] (6) Analysis of different water qualities

[0103] Wastewater of different water quality was selected to test the PSAC flocculant. The preparation conditions of the PSAC flocculant were 8mL of sodium hydroxide for alkalization, polymerization temperature of 60°C, and aging time of 72h. The dosage experiment was carried out according to the Al2O3 content calculated in 4.3.5. The polluted water samples used in this experiment were actual sewage from a certain place and sewage from a sewage treatment plant, which were used to test the actual treatment effect of the PSAC flocculant. The initial pH, turbidity, and UV of the sewage were measured. 254 and total phosphorus were 7.93, 16.13 NTU, and 0.066 cm -1 , 0.42mg / L. Sewage plant sewage initial pH, turbidity, UV 254 and total phosphorus were 6.93, 44.76NTU, and 0.179cm -1 , 0.95mg / L. The dosage of PSAC flocculant was selected as 39mg / L, 78mg / L, 156mg / L, and 312mg / L. The removal of pollutants in water bodies by PSAC in different water qualities was analyzed, and the applicable scope of PSAC was explored. The results are shown below.

[0104] Fig.12The figure below shows the effect of PSAC flocculant on the removal of pollutants in water when treating sewage of different water qualities. It can be seen that PSAC has a good effect on the treatment of the two types of sewage. Fig.12 From (a), we can see that as the dosage increases from 39 to 312 mg / L, the residual turbidity in the sewage has a trend of first weakening and then strengthening. When the dosage is 78 mg / L and 156 mg / L, the turbidity removal effect is better. At this time, the residual turbidity of the water body is reduced to 0.88 NTU and 1.07 NTU, and the turbidity removal rate is 94.5% and 93.4%, respectively. Fig.12 (b) It can be seen that UV 254 The removal effect of total phosphorus has the same trend as turbidity, and the removal effect increases first and then decreases. When the dosage is 78 mg / L, the removal effect of UV 254 The removal effect of total phosphorus is better than that of 156 mg / L. 254 The removal rates of total phosphorus and total phosphorus were 97.2% and 96.8% respectively. 254 Absorbance is 0.005 cm -1 , the residual total phosphorus is 0.03 mg / L.

[0105] Depend on Fig.12 (a) It can be seen that as the dosage increases from 39 to 312 mg / L, the turbidity removal effect in sewage treatment plant wastewater first increases and then gradually stabilizes. When the dosage is 156 mg / L, the turbidity removal effect is better than other dosages. At this time, the residual turbidity in the water drops to 2.67 NTU, and the removal rate reaches 94%. Fig.12 (c) It can be seen that PSAC has a significant effect on UV in sewage treatment plant wastewater. 254 The change trend of the removal effect of total phosphorus was inconsistent. As the dosage increased from 39 to 312 mg / L, UV 254 The removal effect of total phosphorus showed a trend of gradual strengthening, while the removal effect of total phosphorus first strengthened and then weakened. 254 The removal effects of total phosphorus and total phosphorus were relatively the best, with removal rates of 55.9% and 90.5% respectively. 254 The absorbance is 0.079 cm -1 , the residual total phosphorus is 0.09 mg / L.

[0106] From the above results, it can be seen that when PSAC flocculants treat different sewage, the flocculation effect will change due to the influence of different water quality conditions. However, it shows good pollutant removal effect in two different sewages. It can be inferred that PSAC flocculants have good flocculation performance and relatively stable flocculation performance. In the actual sewage treatment process, it can meet the basic treatment needs.

[0107] 4. Characterization of flocculants

[0108] It mainly characterizes the existing forms of aluminum in PSAC and its microscopic physical and chemical structure. Al-Ferron time-by-time complex colorimetry is often used to analyze the Al form and form transformation in aluminum salt flocculants. This experiment uses this method to analyze the Al form of PSAC flocculants and its morphological changes. Other applied characterization methods used include scanning electron microscopy (SEM), Fourier transform infrared spectroscopy (FTIR), X-diffraction spectroscopy (XRD), and X-ray photoelectron spectroscopy (XPS), which mainly analyze and study the phase composition, microstructure, and physical and chemical properties in PSAC.

[0109] (1) Effect of polymerization temperature

[0110] For the five PSAC products prepared at different polymerization temperatures, the values ​​of Al forms in the PSAC products were measured by experimental methods, the three forms of Al were distinguished, the experiments were repeated to reduce the error and ensure the accuracy of the experimental results of Al forms of PSAC flocculants. a , Al b , Al c , Al T The value of Al in PSAC flocculant was calculated. a , Al b , Al c The percentage is as follows Fig.13 As shown. Fig.13 As shown, Al in PSAC a The content of Al is relatively high. The change of polymerization temperature has a significant effect on the distribution of Al forms in PSAC. In PSAC prepared by polymerization at room temperature, Al c The proportion of Al a The proportion of Al c The proportion of Al a The proportion of Al b The proportion of Al a and Al c The proportion of Al b The proportion is high, reaching 47%. This shows that the change of temperature has an impact on the Al content in PSAC. a and Al b When the polymerization temperature is low, most of the aluminum in PSAC is oligomeric aluminum. As the polymerization temperature increases to 60°C and above, the distribution of Al morphology in PSAC flocculants begins to change significantly. b The proportion of Ala This is because the increase in temperature causes the form of aluminum in PSAC to change, and the increase in temperature can promote the Al a To Al b Conversion.

[0111] It can be seen that the polymerization temperature will affect the distribution of aluminum forms in PSAC. As the temperature increases, the Al b The increase in the content of PSAC promotes the flocculation performance of the PSAC flocculant.

[0112] (2) Effect of alkali dosage and silicon element

[0113] For four PSAC products with different amounts of alkali added and containing silicon and removing silicon, the values ​​of Al forms in PSAC products were measured by experimental methods. The three forms of Al were distinguished by experimental analysis methods. Repeated experiments were performed to reduce errors and ensure the accuracy of the experimental results of Al forms of PSAC flocculants. a , Al b , Al c , Al T The value of Al in PSAC flocculant was calculated. a , Al b , Al c The percentage is as follows Fig.14 shown.

[0114] like Fig.14 As shown in the figure, the amount of alkali has a significant effect on the form of aluminum in PSAC flocculant. Most of the aluminum in PSAC is in the form of Al a In the form of hydrolysis, only a small amount of Al 3+ With OH in water - Al in PSAC alkalized with 4 mL NaOH a The highest proportion was 82%, and the Al in PSAC alkalized with 8 mL NaOH b The results showed that the c A small increase, accounting for 17%, is because with the increase of alkali dosage, OH in the solution - As the concentration increases, the free Al in the PSAC flocculant 3+ and Al a Will continue with OH - Polymerization reaction occurs to generate Al b , Al c , during the flocculation process, Al b Give full play to the adsorption and bridging ability, Al cBy giving full play to the net capture and sweeping capabilities, these two ingredients can enhance the flocculation effect of PSAC flocculant.

[0115] like Fig.14 As shown in the figure, by comparing the distribution of aluminum forms in the two PSAC samples with and without silicon, it can be seen that under the same alkali dosage, there is a significant difference in the aluminum forms between the two. a The highest proportion, reaching 47%, Al c The lowest proportion is 17%. Al is also present in desiliconized PSAC. a The highest proportion is 55%, Al c The lowest proportion is 22%. Al in silicon-containing PSAC b The proportion is significantly higher than that of desiliconized PSAC. b The content difference is 13%. It can be inferred that the silicon-containing PSAC contains more silicate, which can increase the molecular weight of PSAC and promote Al a To Al b The conversion of Al b To Al c Conversion.

[0116] (3) Scanning electron microscopy analysis

[0117] In the experiment, the three materials of volcanic rock, PSAC-containing silicon, and PSAC-desiliconized were placed in a vacuum drying oven for two hours. The temperature of the drying oven was set to 60°C. After drying, the materials were taken out and fully ground with a mortar. The ground powder was sealed and stored in a drying dish. The dry powder material was evenly applied on the conductive glue in a linear shape and then pre-treated with gold spraying. The microstructure of the material was observed and scanned with a scanning electron microscope to obtain the corresponding SEM image. The electron micrograph of the material obtained by the SEM image can intuitively observe the surface of the material, understand the appearance and structural characteristics of the material, and study its physical and chemical properties.

[0118] Experimental results analysis

[0119] like Fig.15 As shown in (a)-(b), the surface of volcanic rock particles is uneven, the particle size is uneven, and there are impurities distributed on the surface. The uneven surface structure of volcanic rock increases the contact area, which can ensure that the volcanic rock can be fully infiltrated during acid leaching, improve the leaching rate of effective components in the volcanic rock, and avoid the waste of resources due to incomplete acid leaching. Fig.15(c)-(d) are the energy spectra of volcanic rock materials and the proportion of some elements. Elements such as carbon, oxygen, silicon, aluminum, and magnesium are distributed in volcanic rock materials, among which carbon, oxygen, and silicon are the most abundant, and the content of aluminum is higher than that of other metal elements, which shows that it is feasible to prepare flocculants using volcanic rocks.

[0120] Fig.16 (a)-(b) are SEM electron micrographs of PSAC magnified 500 times and 1000 times. From the figure, it can be seen that the surface of PSAC is rough, the particles are uneven, the overall morphology is irregular, and there are many small holes unevenly distributed on the surface, with a complex surface structure. This is due to the polysilicic acid in the material, which makes the PSAC molecules have a high molecular weight and complex structure, providing a large number of attachment sites for metal cations such as aluminum and iron. A large number of metal cations such as aluminum and iron are attached to these sites to form the rough appearance structure of PSAC. Such a structure makes the surface area of ​​PSAC larger, and has a strong adsorption bridging and net capture and sweeping ability. Fig.16 (c)-(d) are the EDS spectra of PSAC flocculants and the proportion of some elements. It can be seen from the figure that PSAC contains oxygen, silicon, aluminum, iron and other elements, and these elements are evenly distributed on the surface of the flocculant. It proves that oxygen, silicon, aluminum, iron and other elements are tightly aggregated together through heating and stirring, and are effective components of PSAC flocculants, which enhances the flocculation ability. Fig.15 (d) and Fig.16 (d) Analysis shows that the proportion of aluminum, iron and other elements in PSAC has increased significantly, which proves that the process of extracting effective components from volcanic rocks and preparing PSAC flocculants by acid leaching is feasible.

[0121] Fig.17 The SEM image and element ratio of PSAC-desiliconization. Fig.17 (a)-(b) clearly show that compared with PSAC flocculant, the surface roughness of PSAC-desiliconized flocculant material is reduced, and cubic particles can be clearly observed. These cubic particles are likely to be aluminosilicate substances formed by silicon, oxygen and aluminum elements that have not been removed, such as Fig.17 As shown in (d), after the silicon removal step, the proportion of silicon in the flocculant is significantly reduced, and the flocculant contains mostly oxygen, aluminum, and iron. These elements combine to form the main components of the flocculant and provide the main function in the flocculation process.

[0122] (4) Fourier transform infrared spectroscopy (FIIR) characterization

[0123] Fourier infrared spectroscopy characterization is a characterization method that uses continuous wavelength infrared light to pass through the sample to determine the type of group in the test sample from the resonance effect produced. Different groups have different absorption frequencies and produce different resonance effects. The Fourier infrared spectrometer is used to scan the sample in the range of 400-4000cm -1 The FTIR spectra collected by internal scanning can be used to compare and analyze the molecular structure and functional groups of flocculants. The mineral materials of the samples to be tested, and the two flocculant samples containing silicon and desiliconized are placed in a vacuum drying oven at 60°C for two hours. After drying, the samples are ground into powders of uniform size, mixed with potassium bromide: sample powder = 100:1, and pressed into tablets. The FTIR spectra are collected within the scanning range using a Fourier transform infrared spectrometer to compare and analyze the functional group structures of the samples.

[0124] Experimental results analysis

[0125] Fourier infrared spectrum of volcanic rock mineral materials Fig.18 As shown. In the spectrum, at 3610cm -1 The OH stretching vibration peak and HOH bending vibration peak of water molecules appear at 1633cm -1 The smaller absorption peak at 1029cm is the bending vibration peak of HOH, which proves that there is less crystal water and structural water in the volcanic rock material. -1 There is a more obvious absorption peak at 700cm, which is the vibration peak formed by Si-O, Al-O, and Fe-O in the material. -1 The peak at 467 cm represents the Si-O-Al / Mg absorption peak; -1 、541cm -1 The two peaks are Si-O plane vibration absorption peaks.

[0126] The Fourier infrared spectra of PSAC flocculant material and PSAC-desiliconized flocculant material are shown in Fig.18 In the spectrum, the PSAC flocculant material and the PSAC-desiliconized flocculant material have the peaks at 3413 cm -1 and 3415cm -1 Obvious absorption peaks appeared at 1633cm, which are caused by the stretching vibration of -OH groups in the hydrolysis products of aluminum ions and iron ions in the flocculant material. -1 Obvious HOH bending vibration peaks appear everywhere. These peaks are absorption peaks generated by the bending vibration of water molecules. This indicates that water molecules enter the flocculant during the preparation process and exist in the flocculant in the form of adsorbed water. It also indicates the existence of hydroxyl complexes in PSAC. -1 and 1103cm in PSAC-desiliconization -1The Si-O-Fe and Si-O-Al stretching vibration peaks appeared at 1029 cm -1 This indicates that the bonds between these elements were broken and reorganized during the preparation process, forming new tetrahedral structures of Si-O-Fe and Si-O-Al. The appearance of this new peak proves that the polymerization preparation of PSAC flocculant is successful. -1 610cm at PSAC desiliconization -1 The absorption peak that appears at indicates that the Fe-O vibration peak, the Fe-OH characteristic absorption peak and the Al-OH bending vibration peak are superimposed at this position to form a strong absorption peak, which indicates that there is an interaction between the hydroxyl complexes of aluminum ions and iron ions, which enhances the flocculation ability of PSAC.

[0127] (5) XPS characterization

[0128] X-ray photoelectron spectroscopy is to irradiate the sample to be tested with X-rays, and the electrons on the sample surface are excited. After passing through the transmission lens, the photoelectron spectrum can be obtained by counting the excited electrons and analyzing the kinetic energy of the photoelectrons. It is helpful to analyze the loading form of the specified elements on the surface of the composite material before and after flocculation. The sample to be tested is placed in a vacuum drying oven at 60℃ for two hours. After drying, it is taken out and ground into a uniform powder in a mortar and placed in a centrifuge tube for testing.

[0129] Experimental results analysis

[0130] Fig.19 This is the X-ray spectrum of PSAC flocculant and its flocs, which clearly shows the presence of elements in PSAC and flocs, including iron (Fe), phosphorus (P), magnesium (Mg), silicon (Si), aluminum (Al), oxygen (O), and carbon (C). The phosphorus, oxygen, silicon, aluminum, and iron elements in PSAC and the previous flocs are analyzed below.

[0131] Fig. 20 (a) is the peak spectrum of Si 2p in PSAC and its flocs. In PSAC, there are three convolution peaks in the Si 2p spectrum with binding energies of 103.34eV, 102.819eV, and 100.28eV, respectively. These three peaks correspond to the Si-OC mixed bond, Si-OH bond, and Si-O-Si bond in the PSAC material. After flocculation, the binding energy peaks appear at 97.88eV, 101.39eV, and 98.41eV, respectively, which indicates that the three bond positions in PSAC have changed during the flocculation process.

[0132] Fig. 20(b) is the peak spectrum of Al 2p in PSAC and its flocs. There are two convolution peaks in the PSAC spectrum, with the peak positions at 75.06eV and 74.68eV respectively. The binding energy at 75.06eV and 74.68eV represents the Al-OH bond and Al-O bond in the material. After flocculation, the binding energy peak of Al shifted from the original 75.06eV and 74.68eV to 74.88eV and 74.61 respectively, and the peak size also changed. The binding energy changed, indicating that the aluminum element in PSAC changed during the flocculation process.

[0133] Fig. 20 (c) is the peak spectrum of O1s in PSAC and its flocs.

[0134] It can be seen that a binding energy peak appears at a binding energy of 532.37 eV, which corresponds to the surface hydroxyl groups in the PSAC material. After flocculation, the binding energy position of the oxygen element shifts, the peak area decreases, and its peak position shifts from the original 532.37 eV to 532.22 eV.

[0135] Fig. 20 (d) is the peak spectrum of P1p in PSAC and its flocs. There are two convolution peaks in the PSAC spectrum, but the convolution peak at the binding energy peak of 14.131eV does not belong to phosphorus and its derivatives. This may be because the zinc element in the volcanic rock is mixed into the PSAC during the preparation process, forming the Zn 3s peak here. The binding energy peak corresponding to the phosphorus element should be at 133.99eV. The binding energy peak here corresponds to the phosphate substance in PSAC, which also shows the presence of phosphorus in the volcanic rock. After flocculation is completed, the original binding energy peak at 133.99eV shifts to 134.26eV. Both binding energy peaks correspond to the PO bond in the material.

[0136] Fig. 20 (e) is the peak spectrum of Fe 2p in PSAC and its flocs. A convolution peak can be seen in the spectrum of the PSAC material, and its corresponding peak position is 711eV, which proves that the iron (III) in the PSAC material mainly exists in the form of oxidation. After flocculation, the area and position of the peak change, the peak position shifts from 711eV to 728.88eV, and the binding energy peak area becomes larger.

[0137] Through the characterization and analysis of the physicochemical structures of volcanic rocks and different PSAC products and flocs, the following conclusions can be drawn:

[0138] (1) The Al(III) morphology was determined by the Al-Ferron complexation colorimetric method. It can be concluded that the change of polymerization temperature will affect the distribution of aluminum morphology in PSAC. The increase of polymerization temperature will promote the distribution of Al(III) in PSAC. a To Al b The amount of alkali and the presence of silica also affect the distribution of aluminum forms. The increase in the amount of alkali leads to the increase of Al a To Al b and Al c The presence of silicate promotes Al a To Al b The conversion of Al b To Al c Conversion.

[0139] (2) SEM structural characterization shows that the surface of the volcanic rock material is uneven, with a large specific surface area and impurities attached to it. The surface of the PSAC obtained after acid leaching is rougher and the specific surface area is significantly increased. The surface roughness of the PSAC prepared by the desiliconization step is reduced and the surface pores are reduced. EDS results show that the various elements on the PSAC are closely combined, proving that the process of extracting effective components from volcanic rocks to prepare PSAC is successful.

[0140] (3) The FIIR characterization results show that there are chemical bonds or groups such as Al-OH, Fe-OH, Si-OH, Si-O, Al-O, Fe-O, Si-O-Al and Si-O-Si in volcanic rocks, and there are a small amount of crystal water and structural water. During the preparation of PSAC, new Al-O-Si and Fe-O-Si bonds were formed. In both flocculants, there are absorption peaks formed by the superposition of Fe-O, Fe-OH and Al-OH, which indicates that there is an interaction between the hydroxyl complexes of aluminum ions and iron ions.

[0141] (4) XRD characterization results show that volcanic rock materials contain a variety of mineral materials, which are mainly rich in silicon, oxygen, aluminum, iron, magnesium and other elements. The material composition of PSAC materials is complex. The characterization results show that PSAC materials are mainly a complex product composed of silicon, oxygen, aluminum, iron and magnesium elements. The products composed of these elements participate in the flocculation process as effective components of PSAC.

[0142] (5) XPS characterization results show that there are hydroxyl groups on the surface of PSAC, and the Fe-O, Al-OH, Si-O, PO and other bonds inside the material participate in the entire flocculation process, resulting in changes in its binding energy.

[0143] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a composite flocculant based on volcanic rock minerals, characterized in that: The steps include: Acid leaching process: Take hydrochloric acid with a concentration of 3-4 mol / L, heat it to 50-90°C, then pour in the volcanic rock powder, start stirring and continue heating to 90-120°C, keep the temperature and continue stirring for 2-3 hours, take out the beaker and let it stand overnight, and the yellow liquid obtained after filtering is the required volcanic rock acid leaching solution. The mass ratio of volcanic rock powder to hydrochloric acid is 1:10-1:15; Alkalization process: Take the volcanic rock acid extract, place it on an electromagnetic heating stirrer, slowly add 2-3 mol / L sodium hydroxide solution into the beaker, control the polymerization temperature to 20-100°C, continue stirring for 0.17-4h, then take it out and let it stand and mature at room temperature for 24-36h. An oily yellow liquid is observed, which is the composite silicon-aluminum-iron flocculant. The volume ratio of sodium hydroxide solution to volcanic rock acid extract is: 1.2-1.

6.

2. A method for preparing a composite flocculant based on volcanic rock minerals, characterized in that: The volcanic rock is calcined at 200-600°C for 1-2 hours. After the calcination is completed, the rock is taken out and cooled to room temperature, and then ground into powder for later use.

3. Application of a composite flocculant based on volcanic rock minerals in phosphorus removal, characterized in that: The composite silicon-aluminum-iron flocculant according to claim 1 is used for water treatment, and the dosage of the composite silicon-aluminum-iron flocculant is 0.5mL / L-5mL / L.

Citation Information

Patent Citations

  • Method for preparing polyaluminum ferric silicate composite coagulant from coal ash

    CN108609711A

  • Preparation method of poly aluminum-ferric-silicate flocculant for coking wastewater pretreatment

    CN110980903A

  • Method for preparing polysilicate aluminum ferric flocculant from coal gangue

    CN116022801A