Commercial concrete production wastewater recycling process
By using preliminary precipitation, filtration and sustained-release flocculant treatment processes in concrete production wastewater treatment, and using graphene-loaded sustained-release flocculant composed of mesoporous titanium dioxide and other graphene, the problem of incomplete removal of impurities in the prior art is solved, and the problem of incomplete removal of impurities in the prior art is achieved. Efficient recycling and environmental protection effects of wastewater.
Patent Information
- Application Number
- CN202411151317.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing concrete production wastewater treatment methods cannot effectively remove impurities, limiting the recycling of wastewater, and the rapid precipitation effect of traditional chemical flocculants is not long-lasting, making it difficult to achieve long-term flocculation.
The process of initial precipitation, filtration and sustained release flocculant is adopted. The sustained release flocculant consists of graphene-loaded mesoporous titanium dioxide, organic titanium salt, composite inorganic salt, modified chitosan and branched polyethyleneimine, and is treated by oxidation. Adjust pH to neutral to achieve long-term flocculation and water purification.
Effectively remove impurities such as sand, gravel, soil, etc., reduce solid waste generation, improve the recycling value of wastewater, reduce environmental pollution risks, and reduce wastewater emissions and production costs.
Smart Images

Figure BDA0005003737440000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of wastewater treatment, and in particular to a process for recycling wastewater from commercial concrete production. Background Art
[0002] At present, a large amount of wastewater is generated during the production of commercial concrete. This wastewater contains mud, which will cause environmental pollution if discharged directly. Traditional wastewater treatment methods include sedimentation and filtration, but these methods have limited effects on mud treatment and it is difficult to achieve wastewater recycling.
[0003] Existing concrete production wastewater treatment solutions usually use chemical flocculants for rapid sedimentation, but the disadvantage of this method is that the treated wastewater still contains a lot of impurities and cannot achieve long-term flocculation, which limits the reuse effect of the wastewater, so it needs to be improved. Summary of the invention
[0004] In order to improve the treatment effect of wastewater, the present application provides a process for recycling wastewater from commercial concrete production.
[0005] The present application provides a process for recycling wastewater from commercial concrete production using the following technical solutions: A process for recycling wastewater from commercial concrete production, comprising the following steps: (1) Collecting commercial concrete production wastewater, performing preliminary sedimentation, removing large particle impurities, and obtaining primary treated wastewater; (2) passing the primary treated wastewater through a filtration device to further remove small particle impurities to obtain secondary treated wastewater; (3) adding a slow-release flocculant to the secondary treated wastewater to react with the slurry components, re-precipitating the secondary treated wastewater after the reaction, separating the precipitate to obtain tertiary treated wastewater, drying and crushing the precipitate to obtain recycled concrete filler; (4) After the tertiary treated wastewater is oxidized with an oxidant, the pH is adjusted to neutral to obtain regenerated wastewater.
[0006] By carrying out preliminary sedimentation, filtration, flocculation and oxidation treatment on the wastewater produced by commercial concrete, impurities such as sand, gravel and soil in the wastewater of commercial concrete can be effectively removed. At the same time, these separated impurities can be used as fillers to reduce the generation of solid waste; the slow-release flocculant has a long-lasting flocculation effect and can remain in the wastewater for a longer time, fully contact and react with the mud components in the wastewater, and effectively complex and adsorb harmful components in the wastewater, so that the wastewater meets the standards for recycling, improves the utilization value of recycled wastewater, reduces the discharge of wastewater, and reduces production costs and the risk of environmental pollution.
[0007] Preferably, the raw materials for preparing the slow-release flocculant include the following components in parts by weight: 3-5 parts of graphene-loaded mesoporous titanium dioxide, 8-10 parts of organic titanium salt, 6-8 parts of composite inorganic salt, 20-30 parts of modified chitosan, 15-25 parts of branched polyethyleneimine and 10-15 parts of cross-linking agent.
[0008] Graphene-loaded mesoporous titanium dioxide has good dispersibility and high specific surface area, and has high adsorption activity. It can effectively adsorb impurity components in concrete wastewater, improve the effect and utilization rate of slow-release flocculants, and reduce the dosage of slow-release flocculants; organic titanium salts and composite inorganic salts work synergistically to form colloidal particles, complex the particulate matter in concrete wastewater, form larger agglomerates for sedimentation, and effectively remove impurities in concrete wastewater; modified chitosan and branched polyethyleneimine are in situ polymerized on the surface of graphene-loaded mesoporous titanium dioxide, organic titanium salts and composite inorganic salts to form an inorganic-organic phase flocculant with a core-shell structure, and through the synergistic effect of organic phase gel, inorganic phase colloid and high specific surface area filler, it effectively complexes impurities in concrete wastewater and improves the recycling value of wastewater.
[0009] Preferably, the graphene-supported mesoporous titanium dioxide is prepared by the following steps: Tetrabutyl titanate, anhydrous ethanol and graphene oxide are mixed and dispersed to obtain a suspension, and a nitric acid aqueous solution is added under stirring to obtain a reaction solution. After standing, the pH of the reaction solution is adjusted to neutral, the temperature is increased to react, and after cooling, the reaction solution is washed and dried to obtain graphene-loaded mesoporous titanium dioxide.
[0010] Graphene oxide has good adsorption activity and large specific surface area, and can effectively adsorb and complex various impurities. By in situ synthesizing mesoporous titanium dioxide on the surface of graphene oxide, the dispersion performance of graphene oxide can be improved, and agglomeration can be reduced, thereby improving its adsorption performance. Mesoporous titanium dioxide has a rich and ordered pore structure, which can store organic titanium salts and composite inorganic salt particles, improve the efficiency of adsorption and complexation, and provide a sustained release effect, thereby improving the long-term flocculation performance and water purification performance of the sustained-release flocculant.
[0011] Preferably, the raw materials for preparing the organic titanium salt include titanium tetrachloride and dodecylmethyl dihydroxyethyl ammonium bromide.
[0012] The organic titanium salt obtained by the reaction of titanium tetrachloride and dodecylmethyl dihydroxyethyl ammonium bromide has good flocculation properties. The introduction of quaternary ammonium salts can enhance the adsorption effect of small molecular organic matter, and preliminary sterilization and disinfection of concrete wastewater can be performed, which can enhance the water purification performance of the slow-release flocculant.
[0013] Preferably, the composite inorganic salt includes aluminum sulfate, ferric chloride and calcium carbonate.
[0014] Through the synergistic effect of three inorganic salts, aluminum sulfate, ferric chloride and calcium carbonate, colloids are formed, which effectively flocculate the particulate matter in the concrete wastewater and enhance the water purification effect of the slow-release flocculant.
[0015] Preferably, the raw materials for preparing the modified chitosan include carboxymethyl chitosan and polyquaternium-7.
[0016] Carboxymethyl chitosan has good water solubility and reactivity, and is more susceptible to cross-linking reactions; polyquaternium-7 has quaternary ammonium groups and acrylamide groups. By modifying carboxymethyl chitosan, the charge density on the chitosan surface can be enhanced, and the adsorption capacity can be improved, so that the modified chitosan can effectively adsorb and wrap particles in the water, thereby improving the flocculation effect.
[0017] Preferably, the mass ratio of the carboxymethyl chitosan to polyquaternium-7 is 1:(0.28-0.46).
[0018] The modified chitosan prepared according to the above mass ratio has good flocculation performance.
[0019] Preferably, the raw materials for preparing the branched polyethyleneimine include polyethyleneimine, hexyl chloride and epoxysilane.
[0020] Polyethyleneimine is modified by using hexyl chloride and epoxysilane, and hydrophobic silane molecules are introduced into the side chains of polyethyleneimine, so that the obtained polyethyleneimine has a certain negative charge and can adsorb positively charged impurities. At the same time, the increase in the degree of branching will increase spatial steric hindrance, improve the dispersibility of polyethyleneimine, slow down the flocculation and sedimentation rate of the flocculant, and enable the slow-release flocculant to play a role for a longer period of time; branched polyethyleneimine has good reactivity, and through in-situ polymerization with modified chitosan on the surface of the inorganic phase and secondary coating, the slow-release performance can be further improved, the working time of the slow-release flocculant can be extended, and the water purification performance of the slow-release flocculant can be improved.
[0021] Preferably, the mass ratio of polyethyleneimine, hexyl chloride and epoxysilane is (4-6):0.25:1.
[0022] The branched polyethyleneimine prepared according to the above mass ratio has good reaction performance and adsorption performance.
[0023] Preferably, the slow-release flocculant is prepared by the following steps: The graphene-loaded mesoporous titanium dioxide is dispersed in deionized water, and a graphene dispersion is obtained after ultrasonic treatment. An organic titanium salt and a composite inorganic salt are added to the graphene dispersion, and a mixed dispersion is obtained after stirring. The modified chitosan and the branched polyethyleneimine are mixed and dispersed in deionized water to obtain an organic phase solution, a crosslinker is dissolved in deionized water to obtain a crosslinker solution, the organic phase solution and the crosslinker solution are added to the mixed dispersion under stirring conditions, a slow-release flocculant solution is obtained after reaction, acetone is added to the slow-release flocculant solution for precipitation to obtain a product, and the product is dried to obtain a slow-release flocculant.
[0024] The slow-release flocculant prepared according to the above steps has long-lasting flocculation performance and good water purification effect.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. Through the preliminary sedimentation, filtration, flocculation and oxidation treatment of commercial concrete production wastewater, impurities such as sand, gravel, and soil in the commercial concrete wastewater can be effectively removed. At the same time, these separated impurities can be used as fillers to reduce the generation of solid waste; the slow-release flocculant has a long-lasting flocculation effect, which can remain in the wastewater for a longer time, fully contact and react with the mud components in the wastewater, and effectively complex and adsorb harmful components in the wastewater, so that the wastewater meets the standards for recycling, improves the utilization value of recycled wastewater, reduces wastewater discharge, and reduces production costs and the risk of environmental pollution.
[0026] 2. Graphene-loaded mesoporous titanium dioxide has good dispersibility and high specific surface area, and has high adsorption activity. It can effectively adsorb impurities in concrete wastewater, improve the effect and utilization rate of slow-release flocculants, and reduce the dosage of slow-release flocculants; organic titanium salts and composite inorganic salts work synergistically to form colloidal particles, complex the particulate matter in concrete wastewater, form larger agglomerates for sedimentation, and effectively remove impurities in concrete wastewater; modified chitosan and branched polyethyleneimine undergo in-situ polymerization on the surface of graphene-loaded mesoporous titanium dioxide, organic titanium salts and composite inorganic salts to form an inorganic-organic phase flocculant with a core-shell structure, which effectively complexes impurities in concrete wastewater through the synergistic effect of organic phase gel, inorganic phase colloid and high specific surface area filler, thereby improving the recycling value of wastewater.
[0027] 3. Polyethyleneimine is modified by using chlorohexane and epoxysilane, and hydrophobic silane molecules are introduced into the side chains of polyethyleneimine, so that the obtained polyethyleneimine has a certain negative charge and can adsorb positively charged impurities. At the same time, the increase in the degree of branching will increase the steric hindrance, improve the dispersibility of polyethyleneimine, slow down the flocculation and sedimentation rate of the flocculant, and enable the slow-release flocculant to play a role for a longer period of time; branched polyethyleneimine has good reactivity, and through in-situ polymerization with modified chitosan on the surface of the inorganic phase and secondary coating, the slow-release performance can be further improved, the working time of the slow-release flocculant can be extended, and the water purification performance of the slow-release flocculant can be improved. DETAILED DESCRIPTION
[0028] The present application discloses a process for recycling wastewater from commercial concrete production. The raw materials used in the present application can be obtained from commercially available raw materials unless otherwise specified. The present application is further described in detail below in conjunction with the embodiments: Raw materials description: Tetrabutyl titanate (CAS No.: 5593-70-4), graphene oxide was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., titanium tetrachloride (CAS No.: 7550-45-0), dodecylmethyl dihydroxyethyl ammonium bromide (CAS No.: 57122-49-3), carboxymethyl chitosan (CAS No.: 83512-85-0), polyquaternium-7 (CAS No.: 26590-05-6), polyethyleneimine (CAS No.: 9002-98 -6), molecular weight of 20000, hexyl chloride (CAS No.: 544-10-5), epoxy silane is 3-(2,3-epoxypropoxy)propyltrimethoxysilane (CAS No.: 2530-83-8), cross-linking agent is glutaraldehyde (CAS No.: 111-30-8), chitosan (CAS No.: 9012-76-4), polyquaternium-6 (CAS No.: 26062-79-3), methyltriethoxysilane (CAS No.: 2031-67-6).
[0029] Example 1 Preparation of graphene-supported mesoporous titanium dioxide 10 kg of tetrabutyl titanate, 12 kg of anhydrous ethanol and 5 kg of graphene oxide were mixed and dispersed to obtain a suspension, and 24 L of a 1 mol / L nitric acid aqueous solution was added under stirring at a speed of 800 rpm. The addition was completed within 30 minutes to obtain a reaction solution. After standing for 4 hours, the pH of the reaction solution was adjusted to 7, and the temperature was raised to 100° C. to react for 4 hours. After cooling to below 30° C., the solution was centrifugally washed three times with deionized water and anhydrous ethanol respectively, and dried in an oven at 80° C. to obtain graphene-loaded mesoporous titanium dioxide.
[0030] Preparation of organic titanium salts 6.8 kg of titanium tetrachloride and 13.2 kg of dodecylmethyl dihydroxyethyl ammonium bromide were mixed and dispersed in 40 L of dichloromethane, and the mixture was stirred at a speed of 200 rpm for 12 hours. The solvent was removed by rotary evaporation to obtain an organic titanium salt.
[0031] Preparation of modified chitosan 39.06 kg of carboxymethyl chitosan and 10.94 kg of polyquaternium-7 were dispersed in 100 L of deionized water, stirred at 200 rpm for 1 hour, and then an initiator aqueous solution containing 0.5 kg of potassium persulfate was added dropwise within 30 minutes. The stirring reaction was continued for 2 hours, and acetone was added for precipitation to obtain a precipitate. The precipitate was dried in an oven at 60°C to obtain modified chitosan.
[0032] Preparation of branched polyethyleneimine 38.1 kg of polyethyleneimine was dispersed in 100 L of methanol to obtain a polyethyleneimine dispersion, 2.38 kg of hexyl chloride, 9.52 kg of epoxysilane and 4 kg of tetrabutylammonium bromide were added to the polyethyleneimine dispersion, and the mixture was stirred at 500 rpm in an 80°C water bath to react until the viscosity of the solution increased, and then 200 L of a 1 mol / L sodium hydroxide aqueous solution was added, and the mixture was continued to stir at 500 rpm in an 80°C water bath for 6 hours, and the solvent was removed by rotary evaporation to obtain branched polyethyleneimine.
[0033] Preparation of slow-release flocculants 3 kg of graphene-loaded mesoporous titanium dioxide was dispersed in 50 L of deionized water, and a graphene dispersion was obtained after ultrasonic treatment for 30 min. 8 kg of organic titanium salt and 6 kg of composite inorganic salt were added to the graphene dispersion, wherein the mass ratio of aluminum sulfate, ferric chloride and calcium carbonate in the composite inorganic salt was 1:1:1. The mixture was stirred at 200 rpm for 2 h to obtain a mixed dispersion. 20 kg of modified chitosan and 15 kg of branched polyethyleneimine were mixed and dispersed in 50 L of deionized water to obtain an organic phase solution. 10 kg of a cross-linking agent was dissolved in 20 L of deionized water to obtain a cross-linking agent solution. The organic phase solution and the cross-linking agent solution were added to the mixed dispersion within 2 h. The mixture was stirred at 500 rpm for reaction to obtain a slow-release flocculant solution. Acetone was added for precipitation to obtain a product. The product was dried in an oven at 60 ° C to obtain a slow-release flocculant.
[0034] Preparation of recycled wastewater (1) Collecting commercial concrete production wastewater, performing preliminary sedimentation, removing large particle impurities, and obtaining primary treated wastewater; (2) passing the primary treated wastewater through a filtration device to further remove small particle impurities to obtain secondary treated wastewater; (3) adding a slow-release flocculant to the secondary treated wastewater, and subjecting it to ultrasonic oscillation treatment at 20 kHz for 24 hours to react the slow-release flocculant with the mud component, re-precipitating the secondary treated wastewater after the reaction, separating the precipitate to obtain tertiary treated wastewater, and drying and crushing the precipitate to obtain recycled concrete filler; (4) The tertiary treated wastewater is oxidized with ozone, and then carbon dioxide is passed through the wastewater to adjust the pH to neutral to obtain regenerated wastewater.
[0035] Example 2 Preparation of graphene-supported mesoporous titanium dioxide 10 kg of tetrabutyl titanate, 12 kg of anhydrous ethanol and 5 kg of graphene oxide were mixed and dispersed to obtain a suspension, and 24 L of a 1 mol / L nitric acid aqueous solution was added under stirring at a speed of 800 rpm. The addition was completed within 30 minutes to obtain a reaction solution. After standing for 4 hours, the pH of the reaction solution was adjusted to 7, and the temperature was raised to 100° C. to react for 4 hours. After cooling to below 30° C., the solution was centrifugally washed three times with deionized water and anhydrous ethanol respectively, and dried in an oven at 80° C. to obtain graphene-loaded mesoporous titanium dioxide.
[0036] Preparation of organic titanium salts 6.8 kg of titanium tetrachloride and 13.2 kg of dodecylmethyl dihydroxyethyl ammonium bromide were mixed and dispersed in 40 L of dichloromethane, and the mixture was stirred at a speed of 200 rpm for 12 hours. The solvent was removed by rotary evaporation to obtain an organic titanium salt.
[0037] Preparation of modified chitosan 34.25 kg of carboxymethyl chitosan and 15.75 kg of polyquaternium-7 were dispersed in 100 L of deionized water, stirred at 200 rpm for 1 hour, and then an initiator aqueous solution containing 0.5 kg of potassium persulfate was added dropwise within 30 minutes. The stirring reaction was continued for 2 hours, and acetone was added for precipitation to obtain a precipitate. The precipitate was dried in an oven at 60°C to obtain modified chitosan.
[0038] Preparation of branched polyethyleneimine 41.38 kg of polyethyleneimine was dispersed in 100 L of methanol to obtain a polyethyleneimine dispersion, 1.72 kg of hexyl chloride, 6.9 kg of epoxysilane and 4 kg of tetrabutylammonium bromide were added to the polyethyleneimine dispersion, and the mixture was stirred at 500 rpm in an 80°C water bath to react until the viscosity of the solution increased, and then 200 L of a 1 mol / L sodium hydroxide aqueous solution was added, and the mixture was continued to stir at 500 rpm in an 80°C water bath for 6 hours, and the solvent was removed by rotary evaporation to obtain branched polyethyleneimine.
[0039] Preparation of slow-release flocculants 5 kg of graphene-loaded mesoporous titanium dioxide was dispersed in 50 L of deionized water, and a graphene dispersion was obtained after ultrasonic treatment for 30 min. 10 kg of organic titanium salt and 8 kg of composite inorganic salt were added to the graphene dispersion, wherein the mass ratio of aluminum sulfate, ferric chloride and calcium carbonate in the composite inorganic salt was 1:1:1, and the mixture was stirred at 200 rpm for 2 h to obtain a mixed dispersion. 30 kg of modified chitosan and 25 kg of branched polyethyleneimine were mixed and dispersed in 50 L of deionized water to obtain an organic phase solution, 15 kg of a cross-linking agent was dissolved in 20 L of deionized water to obtain a cross-linking agent solution, the organic phase solution and the cross-linking agent solution were added to the mixed dispersion within 2 h, and the mixture was stirred at 500 rpm for reaction to obtain a slow-release flocculant solution, acetone was added for precipitation to obtain a product, and the product was dried in an oven at 60 ° C to obtain a slow-release flocculant.
[0040] Preparation of recycled wastewater (1) Collecting commercial concrete production wastewater, performing preliminary sedimentation, removing large particle impurities, and obtaining primary treated wastewater; (2) passing the primary treated wastewater through a filtration device to further remove small particle impurities to obtain secondary treated wastewater; (3) adding a slow-release flocculant to the secondary treated wastewater, and subjecting it to ultrasonic oscillation treatment at 20 kHz for 24 hours to react the slow-release flocculant with the mud component, re-precipitating the secondary treated wastewater after the reaction, separating the precipitate to obtain tertiary treated wastewater, and drying and crushing the precipitate to obtain recycled concrete filler; (4) The tertiary treated wastewater is oxidized with ozone, and then carbon dioxide is passed through the wastewater to adjust the pH to neutral to obtain regenerated wastewater.
[0041] Example 3 Preparation of graphene-supported mesoporous titanium dioxide 10 kg of tetrabutyl titanate, 12 kg of anhydrous ethanol and 5 kg of graphene oxide were mixed and dispersed to obtain a suspension, and 24 L of a 1 mol / L nitric acid aqueous solution was added under stirring at a speed of 800 rpm. The addition was completed within 30 minutes to obtain a reaction solution. After standing for 4 hours, the pH of the reaction solution was adjusted to 7, and the temperature was raised to 100° C. to react for 4 hours. After cooling to below 30° C., the solution was centrifugally washed three times with deionized water and anhydrous ethanol respectively, and dried in an oven at 80° C. to obtain graphene-loaded mesoporous titanium dioxide.
[0042] Preparation of organic titanium salts 6.8 kg of titanium tetrachloride and 13.2 kg of dodecylmethyl dihydroxyethyl ammonium bromide were mixed and dispersed in 40 L of dichloromethane, and the mixture was stirred at a speed of 200 rpm for 12 hours. The solvent was removed by rotary evaporation to obtain an organic titanium salt.
[0043] Preparation of modified chitosan 36.5 kg of carboxymethyl chitosan and 13.5 kg of polyquaternium-7 were dispersed in 100 L of deionized water, stirred at 200 rpm for 1 hour, and then an initiator aqueous solution containing 0.5 kg of potassium persulfate was added dropwise within 30 minutes. The stirring reaction was continued for 2 hours, and acetone was added for precipitation to obtain a precipitate. The precipitate was dried in an oven at 60°C to obtain modified chitosan.
[0044] Preparation of branched polyethyleneimine 40 kg of polyethyleneimine was dispersed in 100 L of methanol to obtain a polyethyleneimine dispersion, 2 kg of hexyl chloride, 8 kg of epoxysilane and 4 kg of tetrabutylammonium bromide were added to the polyethyleneimine dispersion, and the mixture was stirred at 500 rpm in an 80° C. water bath to react until the viscosity of the solution increased, and then 200 L of a 1 mol / L sodium hydroxide aqueous solution was added, and the mixture was stirred at 500 rpm in an 80° C. water bath for 6 h, and the solvent was removed by rotary evaporation to obtain branched polyethyleneimine.
[0045] Preparation of slow-release flocculants 4 kg of graphene-loaded mesoporous titanium dioxide was dispersed in 50 L of deionized water, and a graphene dispersion was obtained after ultrasonic treatment for 30 min. 9 kg of organic titanium salt and 7 kg of composite inorganic salt were added to the graphene dispersion, wherein the mass ratio of aluminum sulfate, ferric chloride and calcium carbonate in the composite inorganic salt was 1:1:1, and the mixture was stirred at 200 rpm for 2 h to obtain a mixed dispersion. 25 kg of modified chitosan and 20 kg of branched polyethyleneimine were mixed and dispersed in 50 L of deionized water to obtain an organic phase solution, 12.5 kg of a cross-linking agent was dissolved in 20 L of deionized water to obtain a cross-linking agent solution, the organic phase solution and the cross-linking agent solution were added to the mixed dispersion within 2 h, and the mixture was stirred at 500 rpm for reaction to obtain a slow-release flocculant solution, acetone was added for precipitation to obtain a product, and the product was dried in an oven at 60 ° C to obtain a slow-release flocculant.
[0046] Preparation of recycled wastewater (1) Collecting commercial concrete production wastewater, performing preliminary sedimentation, removing large particle impurities, and obtaining primary treated wastewater; (2) passing the primary treated wastewater through a filtration device to further remove small particle impurities to obtain secondary treated wastewater; (3) adding a slow-release flocculant to the secondary treated wastewater, and subjecting it to ultrasonic oscillation treatment at 20 kHz for 24 hours to react the slow-release flocculant with the mud component, re-precipitating the secondary treated wastewater after the reaction, separating the precipitate to obtain tertiary treated wastewater, and drying and crushing the precipitate to obtain recycled concrete filler; (4) The tertiary treated wastewater is oxidized with ozone, and then carbon dioxide is passed through the wastewater to adjust the pH to neutral to obtain regenerated wastewater.
[0047] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, graphene-loaded mesoporous titanium dioxide is replaced by a mixture of graphene oxide and mesoporous titanium dioxide in a mass ratio of 1:1.
[0048] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the organic titanium salt is replaced by titanium tetrachloride.
[0049] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that in Example 6, the composite inorganic salt is replaced by a mixture of aluminum sulfate and ferric chloride in a mass ratio of 1:1.
[0050] Example 7 Example 7 is based on Example 3, and the only difference between Example 7 and Example 3 is that in Example 7, the composite inorganic salt is replaced by calcium carbonate.
[0051] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, the amount of carboxymethyl chitosan used is 43.48 kg, and the amount of polyquaternium-7 used is 6.52 kg.
[0052] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the amount of carboxymethyl chitosan used is 31.25 kg, and the amount of polyquaternium-7 used is 18.75 kg.
[0053] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, carboxymethyl chitosan is replaced by chitosan.
[0054] Embodiment 11 Example 11 is based on Example 3, and the only difference between Example 11 and Example 3 is that in Example 11, polyquaternium-7 is replaced by polyquaternium-6.
[0055] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, the amount of polyethyleneimine used is 35.29 kg, the amount of hexyl chloride used is 2.94 kg, and the amount of epoxysilane used is 11.77 kg.
[0056] Example 13 Example 13 is based on Example 3. The only difference between Example 13 and Example 3 is that in Example 13, the amount of polyethyleneimine used is 42.42 kg, the amount of hexyl chloride used is 1.52 kg, and the amount of epoxysilane used is 6.06 kg.
[0057] Embodiment 14 Example 14 is based on Example 3. The only difference between Example 14 and Example 3 is that in Example 14, epoxysilane is replaced by methyltriethoxysilane.
[0058] Comparative Example 1 Comparative Example 1 is based on Example 3. The only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the slow-release flocculant is replaced by a mixture of cationic polyacrylamide and polyaluminum chloride in a mass ratio of 1:1.
[0059] Performance testing The "GB8978-1996 Comprehensive Sewage Discharge Standard", "GB / T19923-2024 Urban Sewage Recycling Industrial Water Quality" and "JGJ63-2006 Concrete Water Standard" were selected as standards to detect the pH value, insoluble matter, soluble matter, chloride ion, sulfate ion and alkali content of the regenerated wastewater. Each sample was tested three times, and the average value was taken after measurement. The results are recorded in Table 1.
[0060] Table 1 Test results of recycled wastewater quality It can be seen from Table 1 that the pH value of Examples 1-3 is greater than 7.2, the insoluble matter content is less than 902 mg / L, the soluble matter content is less than 1160 mg / L, the chloride ion content is less than 342 g / L, the sulfate ion content is less than 308 mg / L, and the alkali content is less than 785 mg / L. It can be seen that the slow-release flocculant prepared in the present application has good flocculation effect and water purification effect, and the regenerated wastewater obtained by treatment has high recycling value.
[0061] It can be seen from Table 1 that the only difference between Example 4 and Example 3 is that in Example 4, the graphene-loaded mesoporous titanium dioxide is replaced by a mixture of graphene oxide and mesoporous titanium dioxide in a mass ratio of 1:1. Compared with Example 3, the purity of the regenerated wastewater in Example 4 is reduced; this is because the graphene-loaded mesoporous titanium dioxide is replaced by a mixture of graphene oxide and mesoporous titanium dioxide, and the two are not directly combined, and the effect of synergistically improving the adsorption performance is reduced. At the same time, the dispersion performance of graphene oxide is reduced, and it is easy to agglomerate, which in turn affects the performance of the slow-release flocculant, thereby reducing the purity of the regenerated wastewater.
[0062] As can be seen from Table 1, the only difference between Example 5 and Example 3 is that in Example 5, the organic titanium salt is replaced by titanium tetrachloride. Compared with Example 3, the purity of the regenerated wastewater in Example 5 is reduced. This is because the organic titanium salt is replaced by titanium tetrachloride, and the titanium tetrachloride lacks the modification treatment of dodecylmethyl dihydroxyethyl ammonium bromide and the quaternary ammonium salt group, and the adsorption effect on small molecular organic matter is reduced, thereby affecting the adsorption performance of the slow-release flocculant, and the purity of the regenerated wastewater is reduced.
[0063] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that in Example 6, the composite inorganic salt is replaced by a mixture of aluminum sulfate and ferric chloride in a mass ratio of 1:1, and in Example 7, the composite inorganic salt is replaced by calcium carbonate. Compared with Example 3, the purity of the regenerated wastewater in Examples 6 and 7 is reduced; this is because the types of inorganic salts in the composite inorganic salts are reduced, and different inorganic salt molecules have a complexing and flocculation effect on different types of impurities. Reducing the types affects the synergistic effect of the composite inorganic salts, thereby reducing the purity of the regenerated wastewater.
[0064] As can be seen from Table 1, the only difference between Examples 8 and 9 and Example 3 is that the mass ratio of carboxymethyl chitosan to polyquaternium salt-7 in Example 8 is 1:0.15, and the mass ratio of carboxymethyl chitosan to polyquaternium salt-7 in Example 9 is 1:0.6. Compared with Example 3, the purity of the regenerated wastewater in Examples 8 and 9 is reduced; this is because the mass ratio of carboxymethyl chitosan to polyquaternium salt-7 is not within the specified range, and too much or too little polyquaternium salt-7 will affect the reaction performance and molecular chain structure of the modified chitosan, thereby affecting the flocculation performance and stability of the slow-release flocculant, thereby reducing the purity of the regenerated wastewater.
[0065] As can be seen from Table 1, the only difference between Examples 10 and 11 and Example 3 is that: in Example 10, carboxymethyl chitosan is replaced by chitosan, and in Example 11, polyquaternium-7 is replaced by polyquaternium-6. Compared with Example 3, the purity of the regenerated wastewater in Examples 10 and 11 is reduced; this is because if carboxymethyl chitosan is replaced by chitosan, the reactivity and compatibility are reduced; if polyquaternium-7 is replaced by polyquaternium-6, the introduction of acrylamide groups is lacking, the adsorption performance and flocculation performance are reduced, and thus the purity of the regenerated wastewater is reduced.
[0066] As can be seen from Table 1, the only difference between Examples 12 and 13 and Example 3 is that the mass ratio of polyethyleneimine, hexyl chloride and epoxysilane in Example 12 is 3:0.25:1, and the mass ratio of polyethyleneimine, hexyl chloride and epoxysilane in Example 13 is 7:0.25:1. Compared with Example 3, the purity of the regenerated wastewater in Examples 12 and 13 is reduced; this is because the mass ratio of polyethyleneimine, hexyl chloride and epoxysilane is not within the specified range, the degree of branching of polyethyleneimine is different, and too high or too low a degree of branching will affect the effective working time and sustained release performance of the slow-release flocculant in the wastewater, thereby affecting the flocculation effect, so that the purity of the regenerated wastewater is reduced.
[0067] As can be seen from Table 1, the only difference between Example 14 and Example 3 is that in Example 14, epoxy silane is replaced by methyltriethoxysilane. Compared with Example 3, the purity of the regenerated wastewater in Example 14 is reduced. This is because the epoxy silane is replaced by methyltriethoxysilane, the reaction activity of methyltriethoxysilane is reduced, the branching degree of branched polyethyleneimine is reduced, and thus the dispersion performance and slow-release flocculation performance are reduced, which affects the working performance of the slow-release flocculant, thereby reducing the purity of the regenerated wastewater.
[0068] As can be seen from Table 1, the only difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, the slow-release flocculant is replaced by a mixture of cationic polyacrylamide and polyaluminum chloride in a mass ratio of 1:1. Compared with Example 3, the purity of the regenerated wastewater in Comparative Example 1 is greatly reduced; this is because the slow-release flocculant is replaced by a mixture of inorganic and organic flocculants, lacking the design of modification treatment and slow-release flocculation, the flocculant will act quickly, settle quickly, and it is difficult to exist in the water body for a long time, and the impurities in the wastewater cannot be fully and effectively removed, so that the purity of the regenerated wastewater is greatly reduced.
[0069] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A process for recycling wastewater from commercial concrete production. Features: The steps include: (1) Collect the wastewater from commercial concrete production, conduct preliminary sedimentation, remove large particle impurities, and obtain primary treated wastewater; (2) Passing the primary treated wastewater into a filtration device to further remove small particle impurities to obtain secondary treated wastewater; (3) adding a slow-release flocculant to the secondary treated wastewater to react with the slurry components, re-precipitating the secondary treated wastewater after the reaction, separating the precipitate to obtain tertiary treated wastewater, drying and crushing the precipitate to obtain recycled concrete filler; (4) After the tertiary treated wastewater is oxidized with an oxidant, the pH is adjusted to neutral to obtain regenerated wastewater.
2. A process for recycling wastewater from commercial concrete production according to claim 1, Features: The raw materials for preparing the slow-release flocculant include the following components in parts by mass: 3-5 parts of graphene-loaded mesoporous titanium dioxide, 8-10 parts of organic titanium salt, 6-8 parts of composite inorganic salt, 20-30 parts of modified chitosan, 15-25 parts of branched polyethyleneimine and 10-15 parts of crosslinking agent.
3. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The graphene-supported mesoporous titanium dioxide is prepared by the following steps: Tetrabutyl titanate, anhydrous ethanol and graphene oxide are mixed and dispersed to obtain a suspension, and a nitric acid aqueous solution is added under stirring to obtain a reaction solution. After standing, the pH of the reaction solution is adjusted to neutral, the temperature is increased to react, and after cooling, the reaction solution is washed and dried to obtain graphene-loaded mesoporous titanium dioxide.
4. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The raw materials for preparing the organic titanium salt include titanium tetrachloride and dodecylmethyl dihydroxyethyl ammonium bromide.
5. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The composite inorganic salt includes aluminum sulfate, ferric chloride and calcium carbonate.
6. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The raw materials for preparing the modified chitosan include carboxymethyl chitosan and polyquaternium-7.
7. A process for recycling wastewater from commercial concrete production according to claim 6, Features: The mass ratio of the carboxymethyl chitosan to polyquaternium salt-7 is 1:(0.28-0.46).
8. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The raw materials for preparing the branched polyethyleneimine include polyethyleneimine, hexyl chloride and epoxysilane.
9. A process for recycling wastewater from commercial concrete production according to claim 8, Features: The mass ratio of polyethyleneimine, hexyl chloride and epoxysilane is (4-6):0.25:
1.
10. A process for recycling wastewater from commercial concrete production according to claim 2, Features: The slow-release flocculant is prepared by the following steps: The graphene-loaded mesoporous titanium dioxide is dispersed in deionized water, and a graphene dispersion is obtained after ultrasonic treatment. An organic titanium salt and a composite inorganic salt are added to the graphene dispersion, and a mixed dispersion is obtained after stirring. The modified chitosan and the branched polyethyleneimine are mixed and dispersed in deionized water to obtain an organic phase solution, a crosslinker is dissolved in deionized water to obtain a crosslinker solution, the organic phase solution and the crosslinker solution are added to the mixed dispersion under stirring conditions, a slow-release flocculant solution is obtained after reaction, acetone is added to the slow-release flocculant solution for precipitation to obtain a product, and the product is dried to obtain a slow-release flocculant.
Citation Information
Patent Citations
Preparation method for magnetic mesoporous titanium dioxide / graphene oxide adsorbing material
CN103816869A
Industrial wastewater treatment agent and preparation method thereof
CN109626483A
Recycling process of highway construction waste mud
CN114212962A
Organic titanium salt flocculant and preparation method thereof
CN115403610A
Production process of polyaluminum chloride-based flocculant
CN115991529A