Waterproof anti-crack inorganic thermal insulation mortar and preparation method thereof
By using waterproof and crack-resistant inorganic insulation mortar, the construction steps are simplified, the cost is reduced, and the stability and crack resistance of the material are improved, and the problems of long construction cycles and high costs in traditional construction processes are solved, achieving more efficient Construction and longer insulation effect.
Patent Information
- Application Number
- CN202411145547.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The construction process of traditional insulation mortar is cumbersome and expensive, especially the construction cycle of the waterproof mortar leveling step is long and the cost is high, which limits construction efficiency and cost control.
Use waterproof and crack-resistant inorganic insulation mortar, including silicate cement, fly ash, vitrified microbeads, sepiolite, mineral fibers, lignin, water repellent, waterproofing agent, crack-resistant fiber and other raw materials, through specific mixing and agitation process preparation, reduce construction steps and improve material stability and crack resistance.
It significantly shortens the construction cycle, reduces costs, improves construction efficiency, extends the hydration time of the material, enhances crack resistance, and ensures the long-term stability and durability of the exterior wall insulation layer.
Smart Images

Figure CN118878286A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building construction, and particularly relates to a waterproof and crack-resistant inorganic thermal insulation mortar and a preparation method thereof. Background Art
[0002] In the current field of construction, exterior wall insulation mortar construction is a key technical link, which is of great significance to improving the thermal insulation performance and overall quality of buildings. However, the traditional thermal insulation mortar construction process has many shortcomings, especially in terms of the cumbersomeness and cost of the construction steps. The traditional thermal insulation mortar construction is roughly divided into four steps: the first is to roughen the mortar to provide a basis for subsequent construction; the second is to level the waterproof mortar to ensure the flatness and waterproof performance of the wall, but it is also the most labor-intensive and time-consuming part of the entire construction process, with high labor and raw material costs; the third step is the thermal insulation mortar construction to achieve the exterior wall insulation function; the last step is to fully hang the alkali-resistant mesh and finish the anti-cracking mortar to ensure the stability and durability of the insulation layer.
[0003] However, with the rapid development of the construction industry and higher requirements for construction efficiency and cost control, the limitations of traditional insulation mortar construction technology have become increasingly prominent, especially the waterproof mortar leveling step, which not only has a long construction period but also high cost. There are certain limitations in construction and use. For this reason, a waterproof and crack-resistant inorganic insulation mortar is designed. Summary of the invention
[0004] The object of the present invention is to provide a waterproof and crack-resistant inorganic thermal insulation mortar and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A waterproof and crack-resistant inorganic thermal insulation mortar, comprising the following raw materials in parts by weight:
[0007] 90-95 parts of silicate cement, 5-10 parts of fly ash, 10-20 parts of vitrified microspheres, 5-15 parts of sepiolite, 1-3 parts of mineral fiber, 0.5-2 parts of lignin, 0.5-2 parts of water repellent, 0.5-2 parts of waterproofing agent, 2-5 parts of anti-cracking fiber, appropriate amount of additives, and appropriate amount of water are used as the mixing medium.
[0008] Preferably, the additives include 0.1-0.5 parts of thickener, 0.5-1.5 parts of cellulose and 0.1-0.5 parts of retarder.
[0009] Preferably, the waterproofing agent is one or more of a silicone waterproofing agent and an acrylate waterproofing agent, and the anti-cracking fiber is one or more of a polypropylene fiber and a glass fiber.
[0010] A method for preparing waterproof and crack-resistant inorganic thermal insulation mortar comprises the following steps:
[0011] a. Mix silicate cement, fly ash, mineral fiber and lignin evenly;
[0012] b. Add vitrified microspheres, sepiolite, water repellent, waterproofing agent, anti-cracking fiber and thickener to the mixture in step a and continue stirring;
[0013] c. When the ambient temperature is greater than 25 degrees, add additional cellulose and retarder to the mixture in step b and continue stirring. If the temperature is not greater than 25 degrees, no additional addition is made;
[0014] d. Gradually add an appropriate amount of water during the stirring process until a uniform mortar mixture is formed, and control the stirring speed and stirring time. The stirring speed is 500-1000 rpm and the stirring time is 10-20 minutes;
[0015] e. The mortar mixture obtained in step d is allowed to stand and mature to obtain a waterproof and crack-resistant inorganic thermal insulation mortar.
[0016] Application of the waterproof and crack-resistant inorganic thermal insulation mortar according to any one of the above in building construction.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) By using waterproof and crack-resistant inorganic thermal insulation mortar, there is no need for waterproof mortar leveling process, which optimizes the construction process and significantly reduces the construction steps, making the entire construction process more efficient and faster, greatly shortening the construction period, reducing construction costs, and improving construction efficiency, saving time and human resources.
[0019] (2) By adding materials such as glass beads and lignin, the hydration time of cement is extended and increased, making the new material more stable during the curing process. At the same time, its shrinkage ratio is reduced and its crack resistance is significantly improved, effectively avoiding cracks caused by material shrinkage or temperature changes, and ensuring the long-term stability and durability of the exterior wall insulation layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flowchart of the present invention;
[0021] Figure 2 It is a construction schematic diagram of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Embodiment 1:
[0024] See also Figure 1-Figure 2 As shown, a waterproof and crack-resistant inorganic thermal insulation mortar comprises:
[0025] 90 parts of silicate cement, 5 parts of fly ash, 10 parts of vitrified microspheres, 5 parts of sepiolite, 1 part of mineral fiber, 0.5 parts of lignin, 0.5 parts of water repellent, 0.5 parts of waterproofing agent, 2 parts of anti-cracking fiber, appropriate amount of additives, and appropriate amount of water are used as the mixing medium.
[0026] In one embodiment of the present invention, the additives include 0.1 parts of thickener, 0.5 parts of cellulose and 0.1 parts of retarder.
[0027] In one embodiment of the present invention, the waterproofing agent is one or more of a silicone waterproofing agent and an acrylate waterproofing agent, and the anti-cracking fiber is one or more of a polypropylene fiber and a glass fiber.
[0028] A method for preparing waterproof and crack-resistant inorganic thermal insulation mortar comprises the following steps:
[0029] a. Mix silicate cement, fly ash, mineral fiber and lignin evenly;
[0030] b. Add vitrified microspheres, sepiolite, water repellent, waterproofing agent, anti-cracking fiber and thickener to the mixture in step a and continue stirring;
[0031] c. When the ambient temperature is greater than 25 degrees, add additional cellulose and retarder to the mixture in step b and continue stirring. If the temperature is not greater than 25 degrees, no additional addition is made;
[0032] d. Gradually add an appropriate amount of water during the stirring process until a uniform mortar mixture is formed, and control the stirring speed and stirring time. The stirring speed is 500 rpm and the stirring time is 10 minutes;
[0033] e. The mortar mixture obtained in step d is allowed to stand and mature to obtain a waterproof and crack-resistant inorganic thermal insulation mortar.
[0034] like Figure 2 As shown, the application of any of the above-mentioned waterproof and crack-resistant inorganic thermal insulation mortar in building construction specifically includes the following steps:
[0035] 1. Construction preparation:
[0036] Before processing the wall or ceiling, firstly, the base layer must be thoroughly cleaned to ensure that there is no dust, oil or other impurities on the surface to ensure the quality of subsequent construction;
[0037] After cleaning, use a 2m long ruler to check the flatness of the base layer to ensure that the maximum deviation of the flatness of the entire base layer does not exceed 5mm, so as to ensure that the subsequent decoration or coating work can proceed smoothly and achieve the expected decorative effect and service life;
[0038] 2. Construction of inorganic thermal insulation mortar layer:
[0039] When constructing inorganic thermal insulation mortar, the ratio of inorganic thermal insulation mortar to water should be 1:0.4 to ensure the performance and quality of the mortar;
[0040] During construction, apply inorganic thermal insulation mortar directly on the cleaned base layer. The thickness of the mortar should be controlled within 30mm to ensure uniform application and avoid problems such as hollowing and cracks.
[0041] After the construction is completed, it should be maintained for no less than 24 hours, during which the mortar layer should be kept moist to ensure that it can fully solidify and achieve the expected thermal insulation effect and service life;
[0042] 3. Laying of alkali-resistant mesh cloth:
[0043] After the inorganic thermal insulation mortar layer is constructed, evenly apply a special adhesive on its surface to enhance the bonding force with the subsequently laid alkali-resistant mesh cloth;
[0044] Next, lay the alkali-resistant mesh cloth. During the laying process, make the mesh cloth fit closely with the mortar layer to avoid wrinkles, hollows, etc., to ensure the overall flatness and firmness. The overlap width should not be less than 50mm to ensure the effective connection between the mesh cloths and enhance the overall tensile strength and durability.
[0045] 4. Anti-crack mortar finishing:
[0046] When constructing the anti-cracking mortar, prepare it in a ratio of 1:0.25 between the anti-cracking mortar and water to ensure the performance and quality of the mortar;
[0047] Apply anti-cracking mortar evenly on the laid alkali-resistant mesh cloth. The thickness of the mortar should be controlled between 2-3mm, and the trowel should be used to finish the mortar to ensure that the surface is flat and smooth to achieve the expected decorative effect.
[0048] After the construction is completed, it should be maintained for no less than 24 hours, and external impact should be avoided during this period to ensure that the anti-cracking mortar can be fully cured, exert its anti-cracking and waterproof functions, and extend its service life;
[0049] During the above process, the construction temperature is between 5-35°C, and the relative humidity of the construction environment should not exceed 85%. Compared with the traditional construction process, the total construction period can be shortened by about 20%-30% after using the new material.
[0050] Embodiment 2:
[0051] The difference between this embodiment and the first embodiment is that a waterproof and crack-resistant inorganic thermal insulation mortar comprises the following raw materials in parts by weight: 95 parts of silicate cement, 10 parts of fly ash, 20 parts of vitrified microspheres, 15 parts of sepiolite, 3 parts of mineral fiber, 2 parts of lignin, 2 parts of water repellent, 2 parts of waterproofing agent, 5 parts of anti-cracking fiber, appropriate amount of additives, and appropriate amount of water as a mixing medium, the additives comprising 0.5 parts of thickener, 1.5 parts of cellulose and 0.5 parts of retarder, and the remaining steps are the same as those in the first embodiment, and the same parts are not repeated here.
[0052] Experimental example:
[0053] Material preparation: the waterproof and crack-resistant inorganic thermal insulation mortar prepared in Example 1, the waterproof and crack-resistant inorganic thermal insulation mortar prepared in Example 2, standard mortar test block mold, cement, water (for preparing comparison samples), waterproof testing equipment, crack resistance testing equipment, thermal insulation performance testing equipment;
[0054] Experimental steps:
[0055] Use standard mortar test block molds to prepare waterproof and crack-resistant inorganic thermal insulation mortar test blocks and ordinary mortar test blocks (as comparison samples), and perform standard curing on the test blocks to ensure that the test blocks reach the specified strength;
[0056] Use waterproof testing equipment to test the waterproof performance of the test block and record the water seepage situation;
[0057] Use anti-crack testing equipment to test the anti-crack performance of the test block and record the occurrence of cracks;
[0058] Use thermal insulation performance testing equipment to test the thermal insulation performance of the test block and record the thermal insulation effect;
[0059] The details are shown in the following table:
[0060] Waterproof Crack resistance Thermal insulation performance Embodiment 1 1mm / h 0mm <![CDATA[1.5m 2 ·K / W]]> Embodiment 2 1mm / h 0.1mm <![CDATA[1.4m 2 ·K / W]]> Ordinary mortar test block 5mm / h 0.5mm <![CDATA[0.8m 2 ·K / W]]>
[0061] By comparing the experimental data, we can clearly see that the waterproof and crack-resistant inorganic thermal insulation mortar has shown significant advantages in waterproof performance, crack resistance and thermal insulation performance, which is significantly better than ordinary mortar. Its excellent waterproof effect greatly reduces water seepage and effectively protects the building from water erosion. At the same time, the mortar's crack resistance is also excellent, with small cracks, which greatly enhances the structural stability of the building. In addition, it has good thermal insulation effect and high thermal resistance value, which helps to reduce energy consumption and improve the energy efficiency of buildings.
[0062] In the above experiment:
[0063] Mortar test block mold: standard size, 70.7mm×70.7mm×70.7mm cubic mold, made of cast iron;
[0064] Test block preparation: After accurately weighing the raw materials of waterproof and crack-resistant inorganic thermal insulation mortar and ordinary mortar according to the formula, add the raw materials into the mixer and mix them thoroughly. Next, fill the mixed mortar into the mold and tamp it with a tamping rod to ensure that the mortar is filled evenly without bubbles. Then, use a ruler to scrape the surface of the mold to ensure that the surface of the test block is flat. Finally, place the prepared test block under standard curing conditions for curing. The general conditions are a temperature of 20±3℃, a relative humidity of more than 90%, and a curing time of 28 days;
[0065] Waterproof test process:
[0066] During the test block preparation phase, the cured test block needs to be removed from the curing environment and its surface must be thoroughly cleaned to ensure the accuracy of the test results. Subsequently, according to the required waterproof level IPX8, the corresponding test parameters are set on the waterproof tester, including setting a specific water depth of 1 meter and determining the test time, which lasts for 30 minutes. Then, the test block is placed in the designated test area of the waterproof tester and ensured to be completely immersed in water. After starting the waterproof tester, observe the water seepage of the test block in the water and record it in detail.
[0067] Test process of crack resistance test:
[0068] During the test block preparation stage, you first need to remove the cured test block from the curing environment and clean its surface to ensure that the surface of the test block is clean and free of impurities, thereby ensuring the accuracy of the test results. Next, install the test block on the fixture of the crack resistance testing machine, and ensure that the test block is firmly fixed to avoid movement or falling off during the test. According to the test standard, set the loading rate, maximum loading force and other parameters on the testing machine, then start the testing machine and start loading until cracks appear on the test block or the preset maximum loading force is reached. During the test, record the loading force when cracks appear on the test block in detail, and also record the shape, length and other data of the cracks. Finally, evaluate the crack resistance of the test block based on the recorded data to determine whether it meets the predetermined performance requirements;
[0069] Thermal insulation performance test process:
[0070] During the test block preparation stage, you first need to remove the cured test block from the curing environment and thoroughly clean its surface to ensure that the surface of the test block is clean and free of impurities, thereby ensuring the accuracy of the thermal insulation performance test. Then, according to the test requirements, install the test block in the test area of the thermal insulation performance tester and ensure that its position is stable to avoid movement or falling off during the test. According to the test standard or actual needs, set the test temperature to 25°C and the test time to 4 hours, start the tester, start testing and record the thermal insulation performance data of the test block, including key indicators such as temperature changes on the surface of the test block and heat flow. Finally, evaluate the thermal insulation performance of the test block based on the test data to determine whether it meets the predetermined performance requirements.
[0071] in:
[0072] Portland cement is a hydraulic cementing material made from limestone, siliceous materials and aluminum materials through calcination, grinding and other processes. It is also called Portland cement. It has high strength and good durability. It is a commonly used basic material in construction projects. Portland cement can harden in water and gradually form a solid stone body, thus playing a role of bonding and solidification.
[0073] Fly ash is the solid residue produced when burning coal, mainly composed of silicon dioxide, aluminum oxide, calcium oxide and other components. In cement concrete, fly ash is used as an admixture to improve the workability, strength and durability of concrete. The addition of fly ash can also reduce the amount of cement used, reduce costs, and is beneficial to the environment;
[0074] As a highly efficient, environmentally friendly, green inorganic material, vitrified microspheres are mainly made of oxides of silicon, aluminum, calcium and other elements processed by special technology. This material has many excellent properties, the most notable of which are its excellent thermal insulation, sound insulation and fire resistance. Due to its unique physical structure and chemical properties, vitrified microspheres can effectively prevent the transfer of heat and the propagation of sound, so they are often used as the main material for building thermal insulation layers. When vitrified microspheres are added to concrete or mortar, their tiny bead-like structure can form a large number of tiny pores in the material. These pores effectively block the heat transfer path, thereby significantly improving the thermal insulation effect of the material. At the same time, due to the lightweight characteristics of vitrified microspheres, it can also reduce the density of concrete or mortar, further reducing the energy consumption of buildings. In addition, vitrified microspheres also have good chemical stability and durability, and can maintain their excellent performance in various harsh environments. This makes its application in the construction field more extensive and lasting;
[0075] Sepiolite is a fibrous hydrous magnesium silicate clay mineral with good adsorption properties and certain catalytic effects. In building materials, sepiolite can be used as a filler or reinforcing material to improve the mechanical properties and durability of the material. At the same time, sepiolite can also absorb harmful substances and improve indoor air quality;
[0076] Mineral fiber is a fiber material obtained from mineral rocks with a fibrous structure. Its main components are oxides such as silicon dioxide, aluminum oxide, and magnesium oxide. Mineral fiber has good dispersibility and reinforcing effect. It is often used as reinforcing ribs or fillers in building materials to improve the tensile strength and crack resistance of the material.
[0077] Lignin is one of the main components of plant cell walls and is a complex polymer compound. In building materials, lignin can be used as an additive to improve the adhesion, water resistance and durability of the materials. Lignin also has good biodegradability, which is beneficial to environmental protection.
[0078] Water repellent is a chemical substance that can reduce the surface tension of materials, making it difficult for water molecules to wet and penetrate the surface of materials. Adding water repellent to building materials can improve the waterproof performance of materials and reduce the erosion and damage of water to materials;
[0079] Waterproofing agent is an additive specially used to improve the waterproof performance of materials. It can form a dense waterproof film covering the surface of the material or penetrating into the material to prevent the penetration and diffusion of water molecules. The addition of waterproofing agent can significantly improve the waterproof effect and service life of building materials;
[0080] Anti-crack fiber is a fiber material used to enhance the anti-crack performance of materials. Adding anti-crack fiber to building materials can effectively inhibit the generation and development of cracks and improve the integrity and durability of materials. Common anti-crack fibers include polypropylene fiber, steel fiber, etc.
[0081] Thickener is a chemical substance that can increase the viscosity of a liquid or paste. In building materials, thickeners are often used to improve the consistency of mortar, paint, putty and other products, making them easier to construct and apply, while improving the adhesion and anti-sagging properties of the materials. There are many types of thickeners, including inorganic thickeners (such as bentonite, magnesium aluminum silicate, etc.) and organic thickeners (such as cellulose derivatives, polyurethane thickeners, etc.). In this formula, a polyurethane thickener is selected;
[0082] Polyurethane thickeners provide efficient thickening effects for water-based systems through their unique molecular structure (hydrophilic group at one end and hydrophobic group at the other end) and mechanism of action (the hydrophobic part of the molecule associates with emulsion particles, pigments and fillers to form a three-dimensional network structure). It is a slightly turbid milky white viscous liquid with excellent flow and leveling properties, uniform film-forming properties, glossiness and high thickening efficiency.
[0083] Cellulose is a natural or synthetic polymer compound with good dispersibility, thickening and water retention. In building materials, cellulose is often used as an additive to improve the workability, crack resistance and durability of materials such as mortar and concrete. Cellulose can form a three-dimensional network structure, absorb and fix a large amount of water, thereby slowing down the evaporation rate of water and improving the water retention performance of the material. At the same time, cellulose can also enhance the cohesion of the material and reduce the occurrence of cracks;
[0084] Retarder is a chemical substance that can slow down the hydration reaction of cement. In building materials, retarders are often used to adjust the setting time of cement concrete to adapt to different construction requirements and climatic conditions. Retarder can reduce the early strength development rate of cement paste, thereby extending the setting time of concrete and improving the operability of construction. At the same time, retarder can also reduce temperature cracks caused by excessive hydration heat in concrete.
[0085] The standard parts used in the present invention can all be purchased from the market, and the special-shaped parts can be customized according to the description and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. The machinery, parts and equipment all adopt conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0086] In the description of the present invention, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0087] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0088] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0089] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0090] In the drawings of the embodiments disclosed in the present invention, only the structures related to the embodiments disclosed in the present invention are involved, and other structures can refer to the general design. In the absence of conflict, the same embodiment and different embodiments of the present invention can be combined with each other.
[0091] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A waterproof and crack-resistant inorganic thermal insulation mortar, characterized in that: The invention comprises the following raw materials in parts by weight: 90-95 parts of silicate cement, 5-10 parts of fly ash, 10-20 parts of vitrified microspheres, 5-15 parts of sepiolite, 1-3 parts of mineral fiber, 0.5-2 parts of lignin, 0.5-2 parts of water repellent, 0.5-2 parts of waterproofing agent, 2-5 parts of anti-cracking fiber, appropriate amount of additives, and appropriate amount of water as a mixing medium.
2. The waterproof and crack-resistant inorganic thermal insulation mortar according to claim 1, characterized in that: The additives include 0.1-0.5 parts of thickener, 0.5-1.5 parts of cellulose and 0.1-0.5 parts of retarder.
3. The waterproof and crack-resistant inorganic thermal insulation mortar according to claim 1, characterized in that: The waterproofing agent is one or more of an organic silicon waterproofing agent and an acrylic waterproofing agent, and the anti-cracking fiber is one or more of a polypropylene fiber and a glass fiber.
4. A method for preparing waterproof and crack-resistant inorganic thermal insulation mortar, characterized in that: The following steps are involved: a. Mix silicate cement, fly ash, mineral fiber and lignin evenly; b. Add vitrified microspheres, sepiolite, water repellent, waterproofing agent, anti-cracking fiber and thickener to the mixture in step a and continue stirring; c. When the ambient temperature is greater than 25 degrees, add additional cellulose and retarder to the mixture in step b and continue stirring. If the temperature is not greater than 25 degrees, no additional addition is made; d. Gradually add an appropriate amount of water during the stirring process until a uniform mortar mixture is formed, and control the stirring speed and stirring time. The stirring speed is 500-1000 rpm and the stirring time is 10-20 minutes; e. The mortar mixture obtained in step d is allowed to stand and mature to obtain a waterproof and crack-resistant inorganic thermal insulation mortar.
5. Application of the waterproof and crack-resistant inorganic thermal insulation mortar according to any one of claims 1 to 4 in building construction.