A method for preparing a multiphase porous stacked thermal shielding ceramic
By preparing multiphase porous stacked thermal shielding ceramics, the problem of high thermal conductivity and infrared transmittance of existing thermal barrier ceramics at high temperatures is solved by utilizing the stacked structure of dense and porous phase ceramics, thus achieving high-efficiency thermal shielding performance and good interface matching.
Patent Information
- Application Number
- CN202411137578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-08-19
AI Technical Summary
Existing thermal barrier ceramic materials have thermal conductivity limited by the limiting phonon thermal conductivity at high temperatures, and high transmittance in the infrared band, resulting in strong thermal radiation penetration and poor thermal shielding effect.
A method for preparing thermal shielding ceramics with a multiphase porous stacked structure is adopted. By selecting porous and dense phase ceramics with different crystal structure types and combining the sintering thermodynamics/kinetic process design, a dense-porous-dense stacked structure is formed. The high refractive index of the dense phase ceramic reflects infrared rays, while the low phonon thermal conductivity and porosity of the porous layer reduce heat conduction, thereby achieving infrared backscattering and improving thermal shielding performance.
With a thermal conductivity of less than 0.8 W/(m·K) in the range of 25 to 1300℃, a spectral transmittance of less than 10% in the 0.3 to 10 μm band, and an equivalent thermal conductivity of less than 1 W/(m·K) in the range of 25 to 1300℃, it exhibits high fracture toughness and good interface matching, breaking through the performance bottleneck of existing thermal barrier ceramics.
Smart Images

Figure CN118878324B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of thermal protection ceramic materials, specifically relating to a method for preparing a multiphase porous stacked structure thermal shielding ceramic. Background Technology
[0002] High-temperature thermal shielding ceramic materials are crucial for protecting the normal operation of energy and power equipment such as turbine engines, gas turbines, and industrial high-temperature furnaces, and improving their efficiency. Currently, research on thermal barrier ceramics mainly focuses on reducing their phonon thermal conductivity, developing various thermal barrier ceramic systems including niobates, zircons, hafnium ions, tannates, and cerates, and employing methods such as atomic or multi-atom doping and high-entropy strategies to reduce the phonon thermal conductivity of materials. However, the photon radiation thermal conductivity of these materials becomes very significant at high temperatures; furthermore, these materials are generally infrared transparent or translucent. According to Planck's law, the radiative heat flux density of a blackbody is proportional to the fourth power of its temperature, therefore, the increase in heat flux radiation penetration at the hot end becomes exceptionally significant at high temperatures. Therefore, researching multifunctional composite thermal shielding ceramic materials with low phonon thermal conductivity, photon thermal conductivity, and resistance to infrared radiation penetration is a current challenge and bottleneck.
[0003] Matthew J. Kelly et al. (Int. J. Appl. Ceram. Technol., 2016, 3: 81–93) prepared Al2O3 / 7YSZ multilayer ceramic coatings by thermal spraying. Compared with YSZ, the composite coating improved reflectivity by 28% and reduced infrared radiation penetration. However, both Al2O3 and 7YSZ are dense phases, and infrared reflection can only be enhanced through the layer interface, limiting the performance improvement. The thermal conductivity of the ceramic is still greater than 1 W / (m·K). Moreover, this multilayer structure design requires a refractive index difference between the two phases greater than 0.4 to achieve good results, making it difficult to extend to other ceramic systems. Nicholls, JR, et al. (Surf. Coat. Technol., 151–152, pp. 383–391) improved the infrared reflectivity and reduced infrared radiation penetration of materials by preparing ceramic / metal multilayer structures. However, in actual service, the metal layer is prone to oxide growth, leading to structural failure. Therefore, there is an urgent need to develop integrated thermal barrier ceramic materials with high strength and toughness, low thermal conductivity, and resistance to thermal radiation penetration, as well as their preparation methods. Summary of the Invention
[0004] The purpose of this invention is to address the problem that existing thermal barrier ceramic materials suffer from limited thermal conductivity due to their limiting phonon thermal conductivity, high infrared transmittance, resulting in strong thermal radiation penetration at high temperatures and poor thermal shielding performance. The invention provides a method for preparing a multiphase porous stacked structure thermal shielding ceramic.
[0005] A method for preparing a multiphase porous stacked structure heat-shielding ceramic is specifically carried out according to the following steps:
[0006] I. Select suitable porous phase ceramics and dense phase ceramics;
[0007] The porous ceramic and dense ceramic mentioned in step one have different crystal structure types. The difference between the sintering densification temperature of the porous ceramic and the dense ceramic is greater than 100℃. The dense ceramic is a high refractive index phase with n1>1.85, while the porous ceramic is a low refractive index phase with n2<1.8 and n1-n2>0.2. Both the porous ceramic and the dense ceramic have a thermal conductivity of less than 2W / (m·K).
[0008] II. Preparation of slurry and casting:
[0009] ① First, mix the porous ceramic powder, solvent, dispersant and binder, and ball mill for a period of time. Then add the plasticizer and continue ball milling for a period of time. Finally, add n-butanol and continue ball milling for a period of time to obtain the porous ceramic slurry.
[0010] The volume fraction of the porous phase ceramic slurry mentioned in step 2① is 50% to 65%;
[0011] The mass ratio of the porous ceramic powder, dispersant, plasticizer, and binder mentioned in step 2① is 1:0.01:0.01:(0.05~0.1);
[0012] ② Mix the dense phase ceramic powder, solvent, dispersant and binder, ball mill for a period of time, then add plasticizer and continue ball milling for a period of time to obtain dense phase ceramic slurry;
[0013] The volume fraction of the dense phase ceramic slurry mentioned in step 2② is 50% to 65%;
[0014] The mass ratio of the dense phase ceramic powder, dispersant, plasticizer, and binder mentioned in step 2② is 1:0.01:0.01:(0.05~0.1);
[0015] ③ Adjust the height of the casting blade to cast the porous phase ceramic slurry into a porous phase ceramic film; dry the porous phase ceramic film to obtain a porous layer ceramic substrate.
[0016] ④ Adjust the height of the casting knife to cast the dense phase ceramic slurry into a dense phase ceramic film; dry the dense phase ceramic film to obtain a dense phase ceramic film substrate.
[0017] III. High-temperature sintering:
[0018] ① A dense phase ceramic cast film substrate and a porous layer ceramic substrate are sequentially cross-laminated, and then held at 50-100℃ and 10MPa uniaxial pressure for 30-90 minutes to obtain a laminated ceramic preform.
[0019] The absolute value of the difference between the refractive index of the porous phase ceramic and the refractive index of the dense phase ceramic mentioned in step 3①, |n2-n1|, is greater than 8 when multiplied by the total number of layers in the stack.
[0020] ② The laminated ceramic preform is kept at 500-600℃ for 4-12 hours for debinding treatment to obtain the laminated ceramic preform after debinding treatment;
[0021] ③ The preform of the laminated ceramic after debinding is heated to the sintering temperature and sintered at the sintering temperature to obtain a multiphase porous laminated thermal shielding ceramic with a total thickness of more than 500 μm.
[0022] The principle of this invention:
[0023] This invention combines the design of multiphase ceramic component structure with the design of sintering thermodynamics / kinetics to prepare a multiphase porous layered thermal shielding ceramic. The sintering densification temperature of the dense phase ceramic component is lower than that of the porous phase ceramic component. By controlling the sintering temperature between the densification temperatures of the dense and porous phases, a "sandwich" structure of dense-porous-dense interlayered phases can be generated during the sintering process of the multilayer ceramic. The high refractive index of the dense phase ceramic is beneficial for reflecting thermal infrared radiation, achieving high-temperature radiation penetration resistance and improving thermal insulation performance. The low phonon thermal conductivity of the porous layer ceramic further reduces the heat conduction process and improves thermal insulation performance through porosity and pore structure regulation. The refractive index difference between the dense and porous phase ceramics is greater than 0.2, and the pore size in the porous layer is 0.3–5 μm, with a ratio to the thermal infrared radiation band between 0.1 and 10, which is beneficial for achieving infrared backscattering and thus reducing the thermal radiation penetration effect. Furthermore, by rationally controlling the thickness ratio of the porous layer and the dense layer, as well as the number of stacked layers, a highly efficient combined heat conduction and heat radiation shielding function can be achieved. This multiphase ceramic exhibits a thermal conductivity of less than 0.8 W / (m·K) at 25–1300℃. The multiphase porous stacked structure heat shielding ceramic with a total thickness of 500 μm has a spectral transmittance of less than 10% in the 0.3–10 μm wavelength range, and the combined equivalent thermal conductivity of heat conduction and heat radiation in the 25–1300℃ range is less than 1 W / (m·K).
[0024] Advantages of this invention:
[0025] I. The present invention discloses a method for preparing a multiphase porous stacked thermal shielding ceramic, which, compared with existing thermal barrier ceramics, breaks through the bottlenecks of high infrared transmittance and high phonon thermal conductivity after ion doping of thermal barrier ceramics such as niobate, zirconate, hafnium salt, tannate, and cerate; compared with existing multilayer ceramics, its dense-porous stacked multilayer structure design breaks through the limitations of large refractive index differences and the bottleneck problem of high-temperature oxidation of metal layers, further improving the high-temperature thermal shielding performance, and has better interface matching and higher strain tolerance;
[0026] Second, the process of this invention is simple, the ceramic structure is highly controllable, the formability is complete, the interlayer thermal expansion matching is good, the strain tolerance is large, the thermal stability is strong, and the fracture toughness is high, thus the multiphase porous stacked thermal shielding ceramic provided by this invention has a very good application prospect.
[0027] III. The multiphase porous stacked thermal shielding ceramic prepared by this invention has a thermal conductivity of less than 0.8 W / (m·K) at 25–1300℃, a spectral transmittance of less than 10% in the 0.3–10 μm wavelength band for a total thickness of 500 μm, an equivalent thermal conductivity of less than 1 W / (m·K) for the sum of thermal conduction and thermal radiation in the 25–1300℃ range, and a fracture toughness greater than 1.5 MPa·m. 1 / 2 The transverse shrinkage rate of ceramic sintering is less than 30%. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the multiphase porous stacked thermal shielding ceramic structure described in this invention. In the figure, 1 is a dense phase ceramic casting film substrate, and 2 is a porous layer ceramic substrate.
[0029] Figure 2 XRD patterns of Y3NbO7 dense phase ceramics and GdTaO4 porous phase ceramics;
[0030] Figure 3 Cross-sectional scan of the Y3NbO7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in Example 1. Detailed Implementation
[0031] Specific Implementation Method 1: This implementation method describes a method for preparing a multiphase porous stacked structure heat-shielding ceramic, which is specifically completed according to the following steps:
[0032] I. Select suitable porous phase ceramics and dense phase ceramics;
[0033] The porous ceramic and dense ceramic mentioned in step one have different crystal structure types. The difference between the sintering densification temperature of the porous ceramic and the dense ceramic is greater than 100℃. The dense ceramic is a high refractive index phase with n1>1.85, while the porous ceramic is a low refractive index phase with n2<1.8 and n1-n2>0.2. Both the porous ceramic and the dense ceramic have a thermal conductivity of less than 2W / (m·K).
[0034] II. Preparation of slurry and casting:
[0035] ① First, mix the porous ceramic powder, solvent, dispersant and binder, and ball mill for a period of time. Then add the plasticizer and continue ball milling for a period of time. Finally, add n-butanol and continue ball milling for a period of time to obtain the porous ceramic slurry.
[0036] The volume fraction of the porous phase ceramic slurry mentioned in step 2① is 50% to 65%;
[0037] The mass ratio of the porous ceramic powder, dispersant, plasticizer, and binder mentioned in step 2① is 1:0.01:0.01:(0.05~0.1);
[0038] ② Mix the dense phase ceramic powder, solvent, dispersant and binder, ball mill for a period of time, then add plasticizer and continue ball milling for a period of time to obtain dense phase ceramic slurry;
[0039] The volume fraction of the dense phase ceramic slurry mentioned in step 2② is 50% to 65%;
[0040] The mass ratio of the dense phase ceramic powder, dispersant, plasticizer, and binder mentioned in step 2② is 1:0.01:0.01:(0.05~0.1);
[0041] ③ Adjust the height of the casting blade to cast the porous phase ceramic slurry into a porous phase ceramic film; dry the porous phase ceramic film to obtain a porous layer ceramic substrate.
[0042] ④ Adjust the height of the casting knife to cast the dense phase ceramic slurry into a dense phase ceramic film; dry the dense phase ceramic film to obtain a dense phase ceramic film substrate.
[0043] III. High-temperature sintering:
[0044] ① A dense phase ceramic cast film substrate and a porous layer ceramic substrate are sequentially cross-laminated, and then held at 50-100℃ and 10MPa uniaxial pressure for 30-90 minutes to obtain a laminated ceramic preform.
[0045] The absolute value of the difference between the refractive index of the porous phase ceramic and the refractive index of the dense phase ceramic, as described in step 3①, is |n2-n1|, and the product of the number of layers is greater than 8.
[0046] ② The laminated ceramic preform is kept at 500-600℃ for 4-12 hours for debinding treatment to obtain the laminated ceramic preform after debinding treatment;
[0047] ③ The laminated ceramic preform after debinding is heated to the sintering temperature and sintered at the sintering temperature to obtain a multiphase porous laminated heat shield ceramic with a total thickness of ≥500μm.
[0048] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the dense phase ceramic described in step one is a rare earth tannate or rare earth niobate with a monoclinic phase structure; the rare earth tannate is ReTaO4; the rare earth niobate is ReNbO4; and Re is a rare earth element. Other steps are the same as in Specific Implementation Method One.
[0049] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One or Two in that the porous phase ceramic mentioned in step one is ReSiO5, Re2Si2O7, Re3NbO7, or Re3TaO7; and Re is a rare earth element. Other steps are the same as in Specific Implementation Method One or Two.
[0050] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that: the particle size of the porous ceramic powder in step two① is 3μm to 5μm; in step two①, the porous ceramic powder, solvent, dispersant, and binder are first mixed and ball-milled for 8 to 16 hours, then a plasticizer is added, and ball milling continues for 4 to 6 hours, and finally n-butanol is added, and ball milling continues for 0.5 to 1 hour to obtain a porous ceramic slurry; the mass fraction of n-butanol in the porous ceramic slurry in step two① is 0.1%. Other steps are the same as in Specific Implementation Methods One to Three.
[0051] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods One to Four in that: the particle size of the dense phase ceramic powder mentioned in step two ② is 0.5 μm to 5 μm; the solvent mentioned in steps two ① and two ② is one or a mixture of two of deionized water, anhydrous ethanol, and toluene; and the dispersant mentioned in steps two ① and two ② is fish oil. The other steps are the same as in Specific Implementation Methods One to Four.
[0052] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in that: the adhesive mentioned in Step Two ① and Step Two ② is polyvinyl alcohol, cellulose, or polyacrylic acid; the plasticizer mentioned in Step Two ① and Step Two ② is glycerol or polyethylene glycol; and the material ratio for ball milling in Step Two ① and Step Two ② is (3-5):1. Other steps are the same as in Specific Implementation Methods One to Five.
[0053] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that: In step two ②, the dense phase ceramic powder, solvent, dispersant, and binder are first mixed and ball-milled for 8 to 16 hours. Then, a plasticizer is added, and ball milling continues for 4 to 6 hours. Finally, n-butanol is added, and ball milling continues for 0.5 to 1 hour to obtain a dense phase ceramic slurry. The mass fraction of n-butanol in the dense phase ceramic slurry described in step two ② is 0.1%. Other steps are the same as in Specific Implementation Methods One to Six.
[0054] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Methods One to Seven in the following ways: In step two to three, the height of the casting knife is 1.1 to 3 times the thickness of the porous ceramic casting film, and the casting speed is 0.5 m / min to 2 m / min; the drying temperature of the porous ceramic casting film is 25°C to 50°C, and the drying time is 8 to 24 hours; the pore size of the porous ceramic substrate in step two to three is 0.3 μm to 5 μm, and the porosity is 10% to 70%; the thickness of the porous ceramic substrate in step two to three is 5 μm to 50 μm. Other steps are the same as in Specific Implementation Methods One to Seven.
[0055] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Methods One to Eight in that: the thickness of the dense phase ceramic cast film substrate mentioned in step two, fourth step is 1–50 μm; the ratio h1 / h2 of the thickness h1 of the dense phase ceramic cast film substrate to h2 of the porous layer ceramic substrate mentioned in step two, fourth step is 0.5–2 times the ratio n2 / n1 of the refractive index n2 of the porous phase ceramic to the refractive index n1 of the dense phase ceramic. The other steps are the same as in Specific Implementation Methods One to Eight.
[0056] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Methods One through Nine in the following ways: The sintering described in step three ③ is pressureless air sintering, the sintering temperature is 1500℃~1650℃, and the sintering time is 4h~12h; the heating rate described in step three ③ is 0.5℃ / min~5℃ / min; the thermal conductivity of the multiphase porous stacked structure heat shielding ceramic described in step three ③ is less than 0.8W / (m·K) at 25℃~1300℃, the spectral transmittance in the 0.3~10μm band is less than 10%, and the equivalent thermal conductivity of the sum of thermal conduction and thermal radiation in the 25~1300℃ range is less than 1W / (m·K); the fracture toughness of the multiphase porous stacked structure heat shielding ceramic described in step three ③ is greater than 1.5MPa·m. 1 / 2 The transverse shrinkage rate of the ceramic sintering is less than 30%. Other steps are the same as those in specific implementation methods one through nine.
[0057] The beneficial effects of the present invention are verified using the following embodiments:
[0058] Example 1: A method for preparing a multiphase porous stacked structure heat-shielding ceramic, specifically completed according to the following steps:
[0059] I. Y3NbO7 powder was selected as the porous phase ceramic, and GdTaO4 powder was selected as the dense phase ceramic;
[0060] The particle size of the Y3NbO7 powder mentioned in step one is 3 μm, and the particle size of the GdTaO4 powder is 2 μm;
[0061] II. Preparation of slurry and casting:
[0062] ① First, mix the porous ceramic powder, solvent, dispersant and binder, and ball mill for 12 hours. Then add plasticizer and continue ball milling for 5 hours. Finally, add n-butanol and continue ball milling for 0.5 hours to obtain porous ceramic slurry.
[0063] The volume fraction of the porous phase ceramic slurry mentioned in step 2① is 60%;
[0064] The mass ratio of the porous ceramic powder, dispersant, plasticizer, and binder mentioned in step 2① is 1:0.01:0.01:0.1;
[0065] ② Mix the dense phase ceramic powder, solvent, dispersant and binder, ball mill for 12 hours, then add plasticizer and continue ball milling for 5 hours, finally add n-butanol and continue ball milling for 0.5 hours to obtain dense phase ceramic slurry;
[0066] The volume fraction of the dense phase ceramic slurry mentioned in step 2② is 60%;
[0067] The mass ratio of the dense phase ceramic powder, dispersant, plasticizer, and binder mentioned in step 2② is 1:0.01:0.01:0.1;
[0068] The solvent mentioned in Step 2① and Step 2② is anhydrous ethanol;
[0069] The dispersant mentioned in steps 2① and 2② is fish oil;
[0070] The adhesive mentioned in steps 2① and 2② is polyvinyl alcohol;
[0071] The plasticizer mentioned in Step 2① and Step 2② is glycerol;
[0072] The material ratio for ball milling described in steps 2① and 2② is 4:1, and the grinding balls are zirconia balls;
[0073] The mass fraction of n-butanol in the dense phase ceramic slurry described in steps 2① and 2② is 0.1%.
[0074] ③ Adjust the height of the casting knife to cast the porous phase ceramic slurry into a porous phase ceramic film; dry the porous phase ceramic film to obtain a Y3NbO7 porous layer ceramic substrate.
[0075] In step 2③, the casting speed is 0.5 m / min; the drying temperature of the porous ceramic cast film is 35℃, and the drying time is 12 h.
[0076] The porous ceramic substrate mentioned in step 2③ has a pore size of 1μm and a porosity of 30%.
[0077] ④ Adjust the height of the casting knife to cast the dense phase ceramic slurry into a dense phase ceramic film; dry the dense phase ceramic film to obtain a GdTaO4 dense phase ceramic film substrate.
[0078] In step 2③, the height of the casting knife is determined based on the refractive indices of the porous and dense ceramic phases: Y3NbO7 has a refractive index of 1.7, and GdTaO4 has a refractive index of 2.1. Therefore, the thickness of the Y3NbO7 porous ceramic substrate is selected as 40 μm, and the thickness of the GdTaO4 dense ceramic casting film substrate is selected as 35 μm. Further, based on the layer thickness, the height of the Y3NbO7 casting knife is selected as 60 μm, and the height of the GdTaO4 casting knife is selected as 50 μm.
[0079] In step 2, the casting speed is 0.5 m / min; the drying temperature of the porous ceramic cast film is 35℃, and the drying time is 12 h.
[0080] III. High-temperature sintering:
[0081] ① A dense phase ceramic cast film substrate and a porous layer ceramic substrate are sequentially cross-laminated, and then held at 80℃ and 10MPa uniaxial pressure for 60 minutes to obtain a laminated ceramic preform.
[0082] In step 3①, the total number of stacked layers is determined based on the refractive indices of the porous and dense ceramic phases: the refractive index of Y3NbO7 is 1.7, the refractive index of GdTaO4 is 2.1, and the absolute value of the difference between their refractive indices is 0.4. Therefore, according to claim 1, the number of stacked layers is greater than 20, so 31 layers are selected (15 layers of GdTaO4, 16 layers of Y3NbO7, where Y3NbO7 is the outermost layer on both sides).
[0083] ② Heat the laminated ceramic preform to 550℃ and keep it at 550℃ for 10 hours to remove the adhesive, thus obtaining the laminated ceramic preform after adhesive removal.
[0084] The heating rate described in step 3② is 0.5℃ / min;
[0085] ③ The laminated ceramic preform after debinding treatment is heated to the sintering temperature and sintered at the sintering temperature to obtain Y3NbO7-GdTaO4 multiphase porous laminated thermal shielding ceramic.
[0086] The sintering described in step 3③ is air pressureless sintering, the sintering temperature is 1600℃, and the sintering time is 6h;
[0087] The heating rate described in step 3③ is 3℃ / min;
[0088] The thickness of the Y3NbO7-GdTaO4 multiphase porous stacked structure heat shielding ceramic mentioned in step 3③ is 1103μm; in the Y3NbO7-GdTaO4 multiphase porous stacked structure heat shielding ceramic mentioned in step 3③, the Y3NbO7 porous layer ceramic substrate is a porous layer with a thickness of 38μm, an average pore size of 1.5μm, and a porosity of 20%; the GdTaO4 dense phase ceramic cast film substrate is a dense layer with a thickness of 33μm.
[0089] The Y3NbO7-GdTaO4 multiphase porous stacked thermal shielding ceramic described in step 3③ has a thermal conductivity of 0.53 W / (m·K) at 25–1300℃, an infrared thermal radiation transmittance of <3.5% in the 0.3–10 μm band, an equivalent thermal conductivity of 0.63 W / (m·K), and a fracture toughness of 3.5 MPa·m. 1 / 2 .
[0090] Figure 2 XRD patterns of Y3NbO7 dense phase ceramics and GdTaO4 porous phase ceramics;
[0091] from Figure 2 It can be seen that the Y3NbO7 dense phase ceramic component selected in step one of Example 1 has a fluorite structure, while the GdTaO4 porous phase ceramic component has a monoclinic structure. The two have different crystal structure types and significant differences in sintering densification temperature, which provides a basis for forming a multiphase dense-porous stacked structure.
[0092] Figure 3 Cross-sectional scan of the Y3NbO7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in Example 1;
[0093] from Figure 3 As can be seen, there is a distinct Y3NbO7 and GdTaO4 layered structure interface after high-temperature sintering. This proves that Y3NbO7 and GdTaO4 can exist in a multiphase structure and will not form a single phase through solid solution. This provides conditions for optical scattering at the heterogeneous interface and improves the reflectivity of the coating.
[0094] In this embodiment, a Fourier transform spectrometer was used to test the spectral response characteristics of the Y3NbO7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in step 3③ of this embodiment. The measurement results show that the transmittance of the Y3NbO7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in step 3③ of this embodiment is 0.035 in the 0.3-10μm band.
[0095] In this embodiment, the thermal conductivity of the Y3NbO7-GdTaO4 multiphase porous stacked structure heat-shielding ceramic prepared in step 3③ was measured using an LFA457 laser thermal conductivity meter. The results show that the thermal conductivity of the Y3NbO7-GdTaO4 multiphase porous stacked structure heat-shielding ceramic prepared in step 3③ is 0.55 W / (m·K) at 1000℃.
[0096] The Y3NbO7-GdTaO4 multiphase porous laminated thermal shielding ceramic prepared in step 3③ of Example 1 exhibits a very small sintering lateral shrinkage rate of 7%. Simultaneously, the ceramic demonstrates a high fracture toughness of 3.5 MPa·m. 1 / 2 This demonstrates that the Y3NbO7-GdTaO4 multiphase porous stacked ceramic prepared in step 3③ of this embodiment has excellent thermal shielding performance.
[0097] Example 2: A method for preparing a multiphase porous stacked structure heat-shielding ceramic, specifically completed according to the following steps:
[0098] I. Yb2Si2O7 powder was selected as the porous phase ceramic, and GdTaO4 powder was selected as the dense phase ceramic;
[0099] The particle size of the Yb2Si2O7 powder mentioned in step one is 2μm, and the particle size of the GdTaO4 powder is 2μm;
[0100] II. Preparation of slurry and casting:
[0101] ① First, mix the porous ceramic powder, solvent, dispersant and binder, and ball mill for 8 hours. Then add the plasticizer and continue ball milling for 10 hours. Finally, add n-butanol and continue ball milling for 0.5 hours to obtain the porous ceramic slurry.
[0102] The volume fraction of the porous phase ceramic slurry mentioned in step 2① is 60%;
[0103] The mass ratio of the porous ceramic powder, dispersant, plasticizer, and binder mentioned in step 2① is 1:0.01:0.01:0.1;
[0104] The mass fraction of n-butanol in the porous phase ceramic slurry mentioned in step 2① is 0.1%;
[0105] ② Mix the dense phase ceramic powder, solvent, dispersant, and binder, and ball mill for 12 hours. Then add the plasticizer and continue ball milling for 5 hours. Finally, add n-butanol and continue ball milling for 0.5 hours to obtain a dense phase ceramic slurry.
[0106] The volume fraction of the dense phase ceramic slurry mentioned in step 2② is 60%;
[0107] The mass ratio of the dense phase ceramic powder, dispersant, plasticizer, and binder mentioned in step 2② is 1:0.01:0.01:0.1;
[0108] The solvent mentioned in Step 2① and Step 2② is anhydrous ethanol;
[0109] The dispersant mentioned in steps 2① and 2② is fish oil;
[0110] The adhesive mentioned in steps 2① and 2② is polyvinyl alcohol;
[0111] The plasticizer mentioned in Step 2① and Step 2② is glycerol;
[0112] The material ratio for ball milling described in steps 2① and 2② is 4:1, and the grinding balls are zirconia balls;
[0113] The mass fraction of n-butanol in the dense phase ceramic slurry described in steps 2① and 2② is 0.1%.
[0114] ③ Adjust the height of the casting knife to cast the porous phase ceramic slurry into a porous phase ceramic film; dry the porous phase ceramic film to obtain a Yb2Si2O7 porous layer ceramic substrate.
[0115] In step 2③, the casting speed is 0.5 m / min; the drying temperature of the porous ceramic cast film is 35℃, and the drying time is 12 h.
[0116] The porous ceramic substrate described in step 2③ has a pore size of 2μm and a porosity of 22%.
[0117] ④ Adjust the height of the casting knife to cast the dense phase ceramic slurry into a dense phase ceramic film; dry the dense phase ceramic film to obtain a GdTaO4 dense phase ceramic film substrate.
[0118] In step 2③, the height of the casting knife is determined based on the refractive indices of the porous and dense ceramic phases: Yb2Si2O7 has a refractive index of 1.6, and GdTaO4 has a refractive index of 2.1. Therefore, the thickness of the Yb2Si2O7 porous ceramic substrate is selected as 35 μm, and the thickness of the GdTaO4 dense ceramic casting film substrate is selected as 30 μm. Further, based on the layer thickness, the height of the Yb2Si2O7 casting knife is selected as 45 μm, and the height of the GdTaO4 casting knife is selected as 40 μm.
[0119] In step 2, the casting speed is 0.5 m / min; the drying temperature of the porous ceramic cast film is 35℃, and the drying time is 12 h.
[0120] III. High-temperature sintering:
[0121] ① A dense phase ceramic cast film substrate and a porous layer ceramic substrate are sequentially cross-laminated, and then held at 80℃ and 10MPa uniaxial pressure for 40 minutes to obtain a laminated ceramic preform.
[0122] In step 3①, the total number of stacked layers is determined based on the refractive indices of the porous and dense ceramic phases: the refractive index of Yb2Si2O7 is 1.6, and the refractive index of GdTaO4 is 2.1. The absolute value of the difference between the two refractive indices is 0.5. Therefore, the optimized stacked layer number is greater than 16 layers, so 20 layers are selected (10 layers of Yb2Si2O7 and 10 layers of GdTaO4).
[0123] ② The laminated ceramic preform is heated to 1650℃ and kept at 1650℃ for 10 hours for debinding treatment to obtain the laminated ceramic preform after debinding treatment.
[0124] The heating rate described in step 3② is 0.5℃ / min;
[0125] ③ The laminated ceramic preform after debinding treatment is heated to the sintering temperature and sintered at the sintering temperature to obtain Yb2Si2O7-GdTaO4 multiphase porous laminated thermal shielding ceramic.
[0126] The sintering described in step 3③ is air pressureless sintering, the sintering temperature is 1600℃, and the sintering time is 6h;
[0127] The heating rate described in step 3③ is 3℃ / min;
[0128] The thickness of the Yb2Si2O7-GdTaO4 multiphase porous stacked structure heat shielding ceramic mentioned in step 3③ is 590μm; in the Yb2Si2O7-GdTaO4 multiphase porous stacked structure heat shielding ceramic mentioned in step 5, Yb2Si2O7 is a porous layer with a thickness of 31μm, an average pore size of 1.5μm, and a porosity of 18%; GdTaO4 is a dense layer with a thickness of 28μm.
[0129] The Yb₂Si₂O₇-GdTaO₄ multiphase porous stacked thermal shielding ceramic described in step 3③ has a thermal conductivity of 0.57 W / (m·K) at 25–1300℃, an infrared thermal radiation transmittance of <3.0% in the 0.3–10 μm band, an equivalent thermal conductivity of 0.60 W / (m·K), and a fracture toughness of 3.0 MPa·m. 1 / 2 .
[0130] In this embodiment, a Fourier transform spectrometer was used to test the spectral response characteristics of the Yb2Si2O7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in step 3③ of this embodiment. The measurement results show that the transmittance of the Yb2Si2O7-GdTaO4 multiphase porous stacked thermal shielding ceramic prepared in step 3③ of this embodiment is 0.030 in the 0.3-10μm band.
[0131] In this embodiment, the thermal conductivity of the Yb₂Si₂O₇-GdTaO₄ multiphase porous stacked structure heat-shielding ceramic prepared in step 3③ was measured using an LFA457 laser thermal conductivity meter. The results show that the thermal conductivity of the Yb₂Si₂O₇-GdTaO₄ multiphase porous stacked structure heat-shielding ceramic prepared in step 3③ is 0.57 W / (m·K) at 1000℃.
[0132] The Yb₂Si₂O₇-GdTaO₄ multiphase porous stacked thermal shielding ceramic prepared in step 3.③ of Example 2 exhibits a very small sintering lateral shrinkage rate of 5%. Simultaneously, the ceramic demonstrates a fracture toughness as high as 3.0 MPa·m. 1 / 2 This demonstrates that the Y3NbO7-YbTaO4 multiphase porous stacked ceramic prepared in step 3③ of Example 2 has excellent thermal shielding performance.
Claims
1. A method for preparing a multiphase porous stacked thermal shielding ceramic, characterized in that... This method is specifically completed in the following steps: I. Select suitable porous phase ceramics and dense phase ceramics; The porous ceramic and dense ceramic mentioned in step one have different crystal structure types. The difference between the sintering densification temperature of the porous ceramic and the dense ceramic is greater than 100℃. The dense ceramic is a high refractive index phase with n1>1.85, while the porous ceramic is a low refractive index phase with n2<1.8 and n1-n2>0.
2. Both the porous ceramic and the dense ceramic have a thermal conductivity of less than 2W / (m·K). The dense phase ceramic mentioned in step one is a rare earth tannate or rare earth niobate with a monoclinic phase structure; the rare earth tannate is ReTaO4; the rare earth niobate is ReNbO4; and Re is a rare earth element. The porous phase ceramic mentioned in step one is ReSiO5, Re2Si2O7, Re3NbO7 or Re3TaO7; where Re is a rare earth element. II. Preparation of slurry and casting: ① First, mix the porous ceramic powder, solvent, dispersant and binder, and ball mill for a period of time. Then add the plasticizer and continue ball milling for a period of time. Finally, add n-butanol and continue ball milling for a period of time to obtain the porous ceramic slurry. The particle size of the porous ceramic powder mentioned in step 2① is 3μm~5μm; The volume fraction of the porous phase ceramic slurry mentioned in step 2① is 50%~65%; The mass ratio of the porous ceramic powder, dispersant, plasticizer, and binder mentioned in step 2① is 1:0.01:0.01:(0.05~0.1); ② Mix the dense phase ceramic powder, solvent, dispersant and binder, ball mill for a period of time, then add plasticizer and continue ball milling for a period of time to obtain dense phase ceramic slurry; The particle size of the dense phase ceramic powder mentioned in step 2② is 0.5μm~5μm; The volume fraction of the dense phase ceramic slurry mentioned in step 2② is 50%~65%; The mass ratio of the dense phase ceramic powder, dispersant, plasticizer, and binder mentioned in step 2② is 1:0.01:0.01:(0.05~0.1); ③ Adjust the height of the casting blade to cast the porous phase ceramic slurry into a porous phase ceramic film; dry the porous phase ceramic film to obtain a porous layer ceramic substrate. The porous ceramic substrate described in step 2③ has a pore size of 0.3μm~5μm and a porosity of 10%~70%. The thickness of the porous ceramic substrate mentioned in step 2③ is 5μm~50μm; ④ Adjust the height of the casting knife to cast the dense phase ceramic slurry into a dense phase ceramic film; dry the dense phase ceramic film to obtain a dense phase ceramic film substrate. The thickness of the dense phase ceramic cast film substrate mentioned in step 2④ is 1~50μm; III. High-temperature sintering: ① A dense phase ceramic cast film substrate and a porous layer ceramic substrate are sequentially cross-laminated, and then held at 50~100℃ and 10MPa uniaxial pressure for 30min~90min to obtain a laminated ceramic preform; The absolute value of the difference between the refractive index of the porous phase ceramic and the refractive index of the dense phase ceramic mentioned in step 3①, |n2-n1|, is greater than 8 when multiplied by the total number of layers in the stack. ② The laminated ceramic preform is kept at 500~600℃ for 4h~12h for debinding treatment to obtain the laminated ceramic preform after debinding treatment; ③ The laminated ceramic preform after debinding is heated to the sintering temperature and sintered at the sintering temperature to obtain a multiphase porous laminated heat shield ceramic with a total thickness of ≥500μm.
2. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... In step 2①, the porous phase ceramic powder, solvent, dispersant and binder are first mixed and ball-milled for 8h~16h. Then, a plasticizer is added and ball-milling continues for 4h~6h. Finally, n-butanol is added and ball-milling continues for 0.5h~1h to obtain a porous phase ceramic slurry. The mass fraction of n-butanol in the porous phase ceramic slurry in step 2① is 0.1%.
3. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... The solvent mentioned in Step 2① and Step 2② is one or a mixture of two of deionized water, anhydrous ethanol and toluene; the dispersant mentioned in Step 2① and Step 2② is fish oil.
4. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... The adhesive mentioned in Step 2① and Step 2② is polyvinyl alcohol, cellulose or polyacrylic acid; the plasticizer mentioned in Step 2① and Step 2② is glycerol or polyethylene glycol; the material ratio of ball milling mentioned in Step 2① and Step 2② is (3~5):
1.
5. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... In step 2②, the dense phase ceramic powder, solvent, dispersant and binder are first mixed and ball-milled for 8h~16h. Then, a plasticizer is added and ball-milling continues for 4h~6h. Finally, n-butanol is added and ball-milling continues for 0.5h~1h to obtain a dense phase ceramic slurry. The mass fraction of n-butanol in the dense phase ceramic slurry in step 2② is 0.1%.
6. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... In step 2③, the height of the casting knife is 1.1 to 3 times the thickness of the porous ceramic casting film, and the casting speed is 0.5 m / min to 2 m / min; the drying temperature of the porous ceramic casting film is 25℃ to 50℃, and the drying time is 8h to 24h.
7. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... In step 2④, the ratio h1 / h2 of the thickness h1 of the dense phase ceramic cast film substrate to h2 of the porous layer ceramic substrate is 0.5 to 2 times the ratio n2 / n1 of the refractive index n2 of the porous phase ceramic to the refractive index n1 of the dense phase ceramic.
8. The method for preparing a multiphase porous stacked thermal shielding ceramic according to claim 1, characterized in that... The sintering described in step 3.③ is air-pressureless sintering, with a sintering temperature of 1500℃~1650℃ and a sintering time of 4h~12h; the heating rate described in step 3.③ is 0.5℃ / min~5℃ / min; the thermal conductivity of the multiphase porous stacked structure heat shielding ceramic described in step 3.③ is less than 0.8W / (m·K) at 25℃~1300℃, the spectral transmittance in the 0.3~10μm band is less than 10%, and the equivalent thermal conductivity of the sum of thermal conduction and thermal radiation in the 25~1300℃ range is less than 1W / (m·K); the fracture toughness of the multiphase porous stacked structure heat shielding ceramic described in step 3.③ is greater than 1.5MPa·m. 1 / 2 The transverse shrinkage rate of ceramic sintering is less than 30%.
Citation Information
Patent Citations
Multi-layer ceramic composite
CN1758953A
Seramics material having multi layered pore sutrcture
KR1020160064804A