Alum-based hydrogel and preparation process thereof
Through the preparation process of alum-based hydrogel, the quaternary ammonium structure and hydroxyl group of modified chitosan are used to solve the problem of insufficient antibacterial performance of hydrogels, and efficient resistance to a variety of bacteria is achieved. It is suitable for medicine and food field.
Patent Information
- Application Number
- CN202411388254.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hydrogels are prone to breed bacteria and have high requirements for antibacterial effects in the fields of medicine, food, etc. It is difficult for the existing technology to effectively improve the antibacterial properties of hydrogels.
Using the preparation process of alum-based hydrogel, modified chitosan, sodium polyacrylate, polyvinylpyrrolidone, calcium chloride, ethylene glycol bis(2-aminoethyl ether) tetraacetic acid, additives and tartaric acid, etc. The raw materials are mixed in a specific proportion, and modified chitosan is prepared through specific process steps, using its quaternary ammonium salt structure and hydroxyl groups to form hydrogen bonds, achieving efficient antibacterial effects.
It significantly improves the antibacterial properties of the hydrogel and can effectively resist a variety of bacteria, including Gram-positive bacteria, Gram-negative bacteria, molds and yeasts, providing efficient and safe antibacterial protection.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogel preparation, and in particular relates to an alum-based hydrogel and a preparation process thereof. Background Art
[0002] Alum, also known as white alum, potassium alum, potassium alum, potassium aluminum alum, is a complex salt of potassium sulfate and aluminum sulfate containing crystal water, with a chemical formula of KAl(SO 4 ) 2 12H 2 O, directly extracted from alum stone, has abundant reserves in my country and is soluble in water. Alum can be added into hydrogel as a cross-linking agent.
[0003] Hydrogel is a structural gel with a three-dimensional network structure. It is highly hydrophilic and water-absorbent. It can swell quickly in water and wrap a large amount of water. It can be divided into natural hydrogels and synthetic hydrogels, such as chitosan hydrogel, sodium alginate hydrogel, polyacrylic acid hydrogel, sodium polyacrylate hydrogel, polyacrylamide hydrogel, etc., which can be obtained by chemical crosslinking or physical crosslinking. The high water absorption and water retention properties of hydrogel make it have important applications in cosmetic facial masks, fever-reducing patches, and preservatives in food.
[0004] Hydrogels are prone to breeding bacteria, thus causing infection, and in the fields of medicine and food, there are often high requirements for the antibacterial effect of hydrogels. Therefore, it is urgent to design an alum-based hydrogel to improve the antibacterial effect of hydrogels to meet market demand. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an alum-based hydrogel and a preparation process thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions: An alum-based hydrogel comprises the following raw materials in parts by weight: 5-8 parts of sodium polyacrylate, 3-5 parts of polyvinyl pyrrolidone, 2-4 parts of modified chitosan, 0.2-0.5 parts of alum, 0.1-0.2 parts of calcium chloride, 0.1-0.2 parts of ethylene glycol bis(2-aminoethyl ether) tetraacetic acid, 0.1-0.3 parts of an auxiliary agent, 0.2-0.3 parts of tartaric acid, and 80-90 parts of deionized water.
[0007] Furthermore, the modified chitosan is prepared by the following steps: S1. Add 1,3-dihydroxymethyl-5,5-dimethylhydantoin, aluminum chloride and DMF (N,N-dimethylformamide) into a dry three-necked flask under nitrogen protection, stir until mixed, then slowly add epichlorohydrin, then heat to 40°C and stir to react for 4 hours. After the reaction is completed, cool to room temperature, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and ether is selected as the eluent, and the volume ratio of benzene and ether is 6:4), and distill under reduced pressure to obtain intermediate 1; the dosage ratio of 1,3-dihydroxymethyl-5,5-dimethylhydantoin, epichlorohydrin, aluminum chloride and DMF is 16.3g:6.3mL:2.1g:120mL; Under heating and acid catalysis conditions, the molar ratio of 1,3-dihydroxymethyl-5,5-dimethylhydantoin and epichlorohydrin is controlled to be 1.05-1.1:1, and a -OH group of 1,3-dihydroxymethyl-5,5-dimethylhydantoin and the epoxy group of epichlorohydrin undergo a nucleophilic substitution reaction. The reaction process is as follows: ; S2, nitrogen was blown into a dry three-necked flask for 30 minutes to drive away the air in the flask, and then intermediate 1, triethylamine and DMF were added in sequence, stirred and dissolved, and then meglumine was slowly added, the temperature was raised to 80°C and stirred for reaction for 3 hours, and after the reaction was completed, the reaction was cooled to room temperature and distilled under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, meglumine, triethylamine and DMF was 18.4g:11.7g:13.5mL:180mL; Under the action of triethylamine, the molar ratio of meglumine to intermediate 1 is controlled to be 1:1.05-1.1, and -NH- of meglumine and -Cl of intermediate 1 undergo nucleophilic substitution reaction. The reaction process is as follows: ; S3. Add 1,3-dichloropropane, triethylamine and DMF into a dry three-necked flask under nitrogen protection, stir to dissolve, then slowly add intermediate 2. After the addition is complete, heat to 80°C and stir to react for 4 hours. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain intermediate 3. The usage ratio of intermediate 2, 1,3-dichloropropane, triethylamine and DMF is 17.6 g:4.5 mL:8.5 mL:140 mL. Under the action of triethylamine, the molar ratio of intermediate 2 to 1,3-dichloropropane is controlled to be 1:1.1-1.2, and the tertiary amine group of intermediate 2 undergoes a nucleophilic substitution reaction with a -Cl of 1,3-dichloropropane. The reaction process is as follows: ; S4, under nitrogen protection, add intermediate 3, triethylamine and DMF into a three-necked flask, stir and dissolve, then slowly add the mixed solution of chitosan and DMF, heat to 90°C and stir to react for 5h, cool to room temperature after the reaction, and distill under reduced pressure to obtain modified chitosan. The ratio of chitosan to intermediate 3 is 10g:2.8g; Under heating conditions, the -NH 2 A nucleophilic substitution reaction occurs with the -Cl of intermediate 3. The reaction process is as follows: ; The chitosan in the modified chitosan is a deacetylated product of the natural polysaccharide chitin. It has abundant amino groups on its surface and has broad-spectrum antibacterial properties. Chitosan mainly interacts with the cell wall of bacteria, causing the destruction of the cell membrane, thereby killing bacteria. The quaternary ammonium salt structure in the modified chitosan dissociates into a positively charged quaternary ammonium salt cation—N + Ions can be adsorbed onto the cell walls of negatively charged bacteria, thereby destroying bacterial cell membranes and denaturing their proteins, hindering DNA replication and reproduction, etc., thereby achieving antibacterial effects; 1,3-dihydroxymethyl-5,5-dimethylhydantoin is grafted into the modified chitosan, which is a broad-spectrum, highly effective antibacterial preservative that can effectively resist Gram-positive bacteria, Gram-negative bacteria, molds, yeasts, etc. The three antibacterial components work synergistically to give alum-based hydrogels excellent antibacterial effects.
[0008] The quaternary ammonium salt structure improves the compatibility of modified chitosan with other raw materials. In addition, there are abundant hydroxyl groups in the modified chitosan. The lone pair electrons of oxygen in the hydroxyl group interact with the hydrogen in the water molecule to form hydrogen bonds, so that the modified chitosan can be further dispersed in the hydrogel, and the modified chitosan can stably exist in the hydrogel, exerting an efficient and safe antibacterial effect.
[0009] Furthermore, the auxiliary agent is one or both of methyl diisopropyl propionamide and menthol.
[0010] A preparation process of an alum-based hydrogel comprises the following steps: (1) After weighing each raw material by weight, sodium polyacrylate, alum, calcium chloride, ethylene glycol bis(2-aminoethyl ether) tetraacetic acid and the auxiliary agent are added into a magnetic stirrer in sequence, and stirred at 50°C for 5 min; (2) Add polyvinyl pyrrolidone and stir at 20°C for 5 min. Then add deionized water, tartaric acid and modified chitosan in sequence and stir at 30°C for 5 min to obtain an alum-based hydrogel.
[0011] Furthermore, the stirring temperature in step (1) is 45-65°C.
[0012] The invention has the beneficial effects that the modified chitosan contains chitosan, quaternary ammonium salt and 1,3-dihydroxymethyl-5,5-dimethylhydantoin, the quaternary ammonium salt structure improves the compatibility of the modified chitosan with other raw materials, and the modified chitosan is rich in hydroxyl groups, which further improves the dispersion uniformity of the modified chitosan. Therefore, the modified chitosan of the invention can stably exist in the hydrogel, and the three antibacterial components therein act synergistically to endow the alum-based hydrogel with efficient and safe antibacterial effect. DETAILED DESCRIPTION
[0013] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0014] Example 1
[0015] The preparation of modified chitosan, the specific steps are as follows: S1. Under nitrogen protection, 16.3 g of 1,3-dihydroxymethyl-5,5-dimethylhydantoin, 2.1 g of aluminum chloride, and 120 mL of DMF were added to a dry 250 mL three-necked flask, stirred until uniformly mixed, and then 6.3 mL of epichlorohydrin was slowly added, and then the temperature was raised to 40 ° C. and stirred for 4 h. After the reaction was completed, it was cooled to room temperature, distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of benzene and diethyl ether, and the volume ratio of benzene and diethyl ether was 6:4), and distilled under reduced pressure to obtain intermediate 1; S2, blow nitrogen gas into a dry 500mL three-necked flask for 30 minutes to drive away the air in the flask, then add 18.4g of intermediate 1, 13.5mL of triethylamine and 180mL of DMF in sequence, stir to dissolve, then slowly add 11.7g of meglumine, heat to 80°C and stir to react for 3h, cool to room temperature after the reaction is completed, and distill under reduced pressure to obtain intermediate 2; S3, under nitrogen protection, add 4.5 mL of 1,3-dichloropropane, 8.5 mL of triethylamine and 140 mL of DMF into a dry 250 mL three-necked flask, stir to dissolve, then slowly add 17.6 g of intermediate 2, after the addition is complete, heat to 80 ° C and stir to react for 4 h, cool to room temperature after the reaction is completed, and distill under reduced pressure to obtain intermediate 3; S4. Under nitrogen protection, add 2.8 g of intermediate 3, 1 mL of triethylamine and 20 mL of DMF into a 250 mL three-necked flask, stir to dissolve, then slowly add a mixed solution of 10 g of chitosan and 100 mL of DMF. After the addition is complete, heat to 90 °C and stir to react for 5 h. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain modified chitosan.
[0016] Example 2
[0017] The alum-based hydrogel was prepared by the following steps: After weighing each raw material by weight, 5 parts of sodium polyacrylate, 0.2 parts of alum, 0.1 parts of calcium chloride, 0.1 parts of ethylene glycol bis(2-aminoethyl ether) tetraacetic acid and 0.1 parts of methyl diisopropyl propionamide were sequentially added into a magnetic stirrer and stirred at 45°C for 5 min; then 3 parts of polyvinyl pyrrolidone were added and stirred at 20°C for 5 min, and then 80 parts of deionized water, 0.2 parts of tartaric acid and 2 parts of the modified chitosan prepared in Example 1 were sequentially added and stirred at 30°C for 5 min to obtain an alum-based hydrogel.
[0018] Example 3
[0019] The alum-based hydrogel was prepared by the following steps: After weighing the raw materials by weight, 6 parts of sodium polyacrylate, 0.4 parts of alum, 0.15 parts of calcium chloride, 0.15 parts of ethylene glycol bis(2-aminoethyl ether) tetraacetic acid and 0.2 parts of menthol were added to a magnetic stirrer in sequence and stirred at 65° C. for 5 min; then 4 parts of polyvinyl pyrrolidone were added and stirred at 20° C. for 5 min, and then 88 parts of deionized water, 0.26 parts of tartaric acid and 3.5 parts of the modified chitosan prepared in Example 1 were added in sequence and stirred at 30° C. for 5 min to obtain an alum-based hydrogel.
[0020] Example 4
[0021] The alum-based hydrogel was prepared by the following steps: After weighing the raw materials by weight, 8 parts of sodium polyacrylate, 0.5 parts of alum, 0.2 parts of calcium chloride, 0.2 parts of ethylene glycol bis(2-aminoethyl ether) tetraacetic acid, 0.2 parts of methyl diisopropyl propionamide and 0.1 parts of menthol were sequentially added into a magnetic stirrer and stirred at 50° C. for 5 min; then 5 parts of polyvinyl pyrrolidone were added and stirred at 20° C. for 5 min, and then 90 parts of deionized water, 0.3 parts of tartaric acid and 4 parts of the modified chitosan prepared in Example 1 were sequentially added and stirred at 30° C. for 5 min to obtain an alum-based hydrogel.
[0022] Comparative Example 1 The alum-based hydrogel was prepared by the following steps: The remaining steps remained unchanged, except that the modified chitosan in Example 4 was replaced by chitosan without any treatment to obtain an alum-based hydrogel.
[0023] Comparative Example 2 The alum-based hydrogel was prepared by the following steps: The remaining steps remained unchanged, except that the modified chitosan in Example 4 was replaced by triclosan to obtain an alum-based hydrogel.
[0024] Comparative Example 3 The alum-based hydrogel was prepared by the following steps: The remaining steps remain unchanged, only the modified chitosan in Example 4 is removed to obtain the alum-based hydrogel.
[0025] Performance Testing Antibacterial test: The alum-based hydrogels prepared in Examples 2-4 and Comparative Examples 1-3 were made into corresponding samples according to the standard, and the antibacterial properties before and after 60 days were tested with reference to the standard GB / T 21866-2008. The test results are shown in the following table: ; “-” means no antibacterial property.
[0026] From the test results in the above table, it can be seen that the alum-based hydrogels prepared in Examples 2-4 of the present invention have efficient and safe antibacterial effects and can be used in the fields of medicine, cosmetics, etc. From the test results of Comparative Examples 1 and 2, it can be seen that when the modified chitosan is replaced with untreated chitosan or triclosan, the antibacterial stability of the hydrogel is greatly reduced.
[0027] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0028] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. An alum-based hydrogel, characterized in that The invention comprises the following raw materials in parts by weight: 5-8 parts of sodium polyacrylate, 3-5 parts of polyvinyl pyrrolidone, 2-4 parts of modified chitosan, 0.2-0.5 parts of alum, 0.1-0.2 parts of calcium chloride, 0.1-0.2 parts of ethylene glycol bis(2-aminoethyl ether) tetraacetic acid, 0.1-0.3 parts of auxiliary agent, 0.2-0.3 parts of tartaric acid, and 80-90 parts of deionized water; Wherein, the auxiliary agent is one or both of methyl diisopropyl propionamide and menthol; The modified chitosan is prepared by the following steps: S1. Under nitrogen protection, 1,3-dihydroxymethyl-5,5-dimethylhydantoin, aluminum chloride and DMF were added to a flask, and epichlorohydrin was added after stirring. The mixture was reacted at 40° C. for 4 h, cooled to room temperature, and distilled under reduced pressure. The mixture was purified by column chromatography and distilled under reduced pressure to obtain intermediate 1. S2, after nitrogen blowing into the flask, add intermediate 1, triethylamine and DMF, stir and add meglumine, react at 80°C for 3h, cool, and distill under reduced pressure to obtain intermediate 2; S3, under nitrogen protection, 1,3-dichloropropane, triethylamine and DMF were added into a flask, and after stirring, intermediate 2 was added, and the mixture was reacted at 80°C for 4h, cooled, and distilled under reduced pressure to obtain intermediate 3; S4. Under nitrogen protection, add intermediate 3, triethylamine and DMF into a flask, stir and add chitosan and DMF, react at 90° C. for 5 h, cool, and distill under reduced pressure to obtain modified chitosan.
2. An alum-based hydrogel according to claim 1, characterized in that: The usage ratio of 1,3-dihydroxymethyl-5,5-dimethylhydantoin, epichlorohydrin, aluminum chloride and DMF in step S1 is 16.3 g:6.3 mL:2.1 g:120 mL.
3. An alum-based hydrogel according to claim 1, characterized in that: The usage ratio of intermediate 1, meglumine, triethylamine and DMF in step S2 is 18.4 g:11.7 g:13.5 mL:180 mL.
4. An alum-based hydrogel according to claim 1, characterized in that: The usage ratio of intermediate 2, 1,3-dichloropropane, triethylamine and DMF in step S3 is 17.6 g:4.5 mL:8.5 mL:140 mL.
5. An alum-based hydrogel according to claim 1, characterized in that: The usage ratio of chitosan in step S4 and intermediate 3 is 10 g:2.8 g.
6. The process for preparing an alum-based hydrogel according to claim 1, characterized in that: The steps include: (1) After weighing each raw material by weight, sodium polyacrylate, alum, calcium chloride, ethylene glycol bis(2-aminoethyl ether) tetraacetic acid and the auxiliary agent are added into a magnetic stirrer in sequence, and stirred at 50°C for 5 min; (2) Add polyvinyl pyrrolidone and stir at 20°C for 5 min. Then add deionized water, tartaric acid and modified chitosan in sequence and stir at 30°C for 5 min to obtain an alum-based hydrogel.
Citation Information
Patent Citations
Antibacterial material of nano-silver covalently grafted halogenated hydantoin-based chitosan and preparation method thereof
CN111334053A
Ultrafiltration polyethylene porous membrane for water treatment and preparation process thereof
CN112755789A
High-strength high-antibacterial-property composite adhesive film and preparation method thereof
CN115260718A
Dry-state high-temperature-resistant hydrogel and preparation method thereof
CN115850732A
Nano-antibacterial condensation gel and preparation method thereof
CN116355241A
Cited By
Photoresponsive drug gel carrier and preparation method thereof
CN120585728A
A light-responsive drug gel carrier and a preparation method thereof
CN120585728B