Preparation method of fiber-reinforced metal-based PMI (polymethacrylimide) composite foam
Through the preparation method of fiber-reinforced metal-based PMI composite foam, combined with PMI particles, metal-based substrates, fiber-reinforced materials and other components, the high density of metal materials, easy corrosion and low surface hardness of polymethacryimide foam is solved. The problem of this material has achieved the improvement of lightweight, flexibility and antioxidant properties, and is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202411129121.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, polymethacryimide foam with high density, easy corrosion and low hardness have poor wear resistance, which limits its application field and flexibility, and cannot effectively overcome the high density, easy corrosion and The problem of low hardness of polypolymer materials.
By adopting the preparation method of fiber-reinforced metal-based PMI composite foam, PMI particles, metal-based materials, fiber-reinforced materials, fillers, adhesives, dispersants, plastic adjustment components and antioxidant performance adjustment components in a specific proportion Mix and synthesize through process flow to prepare composite materials with comprehensive performance improvement.
It has achieved the improvement of the lightweight, flexibility and oxidation resistance of the material, overcome the problems of high density of metal materials, easy corrosion and low surface hardness of polymethacryimide foam, and is suitable for AI robot materials, solar photovoltaic panels and other fields. , improves transportation convenience and flexibility.
Smart Images

Figure CN118879015A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, in particular to a method for preparing a fiber-reinforced metal-based PMI composite foam. Background Art
[0002] Polymethacrylimide (hereinafter referred to as "PMI") foam is a lightweight, high-strength, corrosion-resistant foam with a relatively low density, usually between 20 and 110 kg / m 3 In many cases, it is used as sandwich materials, sheet films, fishing floats, etc. Because the surface hardness is not high, it is difficult to resist the force of hard objects pressing into its surface alone, and the wear resistance is poor, so it is rarely used alone.
[0003] Metal materials refer to metal elements or materials with metal properties that are mainly composed of metal elements, including pure metals, alloys, intermetallic compounds and special metal materials. Metal is a traditional material with outstanding mechanical properties, surface hardness, stability, temperature resistance and other properties. The density of this type of material is very high, usually between 2000 and 16000 kg / m 3 Metal materials have the characteristics of high density, high specific gravity, and low buoyancy, which makes transportation difficult, energy consumption high, and application areas limited.
[0004] For some products, such as AI robot materials, the use of metal materials alone is usually heavy, which limits its flexibility. At the same time, metal materials are not corrosion-resistant and are prone to corrosion and material damage during long-term outdoor use. The use of polymer materials alone also has problems such as low hardness and poor wear resistance.
[0005] Therefore, we need a composite material that can overcome these two defects to solve the above problems. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing a fiber-reinforced metal-based PMI composite foam to solve the problems raised in the above background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A fiber-reinforced metal-based PMI composite foam, comprising PMI particles, a metal substrate, a fiber-reinforced material component, a filler, an adhesive, a dispersant component, a plasticity regulating component, an anti-oxidation performance regulating component and other performance regulating components;
[0009] The PMI particles include, by weight, methacrylic acid (1 to 80 parts), methacrylonitrile or acrylonitrile (1 to 70 parts), an initiator (0.01 to 10 parts), a foaming agent (0.01 to 15 parts), a crosslinking agent (0.01 to 15 parts), and a nucleating agent (0.01 to 15 parts);
[0010] The metal substrate includes one or more combinations of foamed metal materials, small granular metal powders or flaky metal particles;
[0011] The adhesive is added with a flexibility-adjusting component, in which a flexible, long-chain component is grafted onto an adhesive molecular chain to form a flexible adhesive, a dispersion performance regulator, an antioxidant, an anti-aging agent and other components are added, mixed evenly, an initiator, a catalyst, a molecular sieve and an auxiliary agent are added and synthesized according to a process flow to obtain an adhesive component used in a composite material;
[0012] The antioxidant performance adjusting component includes an antioxidant, a coating agent or a sustained-release agent, and the antioxidant needs to be coated or sustained-released;
[0013] The filler is selected from one or more combinations of hollow microspheres, fumed silica, graphite powder, mica powder, silicate powder, marble powder, PMI foam powder, and calcium carbonate powder. The filler needs to be surface treated, including but not limited to organic solvent immersion, surface grafting, and dispersion treatment.
[0014] As a further solution of the present invention: the adhesive comprises one or more combinations of unsaturated resin, phenolic resin, polyurethane, EVA hot melt adhesive, acrylate adhesive, epoxy resin, ethyl cyanoacrylate adhesive, cyanoacrylate adhesive, and methacrylic resin adhesive. The adhesive is added with a flexible component, a dispersibility regulator, an antioxidant, and an anti-aging agent according to the process.
[0015] The fiber reinforcement material component and the filler are soaked in an organic solvent and surface treated, and the method includes but is not limited to one or more combinations of organic solvent soaking, surface grafting chemical groups and dispersion treatment methods.
[0016] As a further solution of the present invention: the fiber reinforcement material component includes one or more combinations of carbon fiber, basalt fiber, glass fiber, graphene fiber, silicate fiber, metal fiber, polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber, viscose fiber, acetate fiber, and cuprammonia fiber.
[0017] As a further solution of the present invention: the surface of the fiber-reinforced material component is degreased, cut into a certain length, processed into a specific shape, roughened, grafted with coupling groups, and added with a surfactant to obtain the fiber used for the composite material, wherein the length of the fiber-reinforced material component ranges from 0.01 to 10 mm.
[0018] As a further solution of the present invention: the dispersant component includes one or more of silicone oil, butyl acetate, n-amyl acetate, isoamyl acetate, cyclohexane, carbon tetrachloride, tetrachloroethane, petroleum ether, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, fatty acid polyethylene glycol esters, 3020, 3007, 9010S, and the added mass proportion of the dispersant component is 0.01-30 parts.
[0019] As a further embodiment of the present invention: the plasticity adjusting component includes one or more combinations of benzoates, parabens, trimellitates, zinc oxalate, magnesium oxalate, succinate, maleate, maleic anhydride, fumarate, adipate, azelaic acid ester, sebacate, polymethylsiloxane, and terminal hydroxyl polysiloxane, and the added amount of the plasticity adjusting component is 0.01 to 30 parts.
[0020] As a further solution of the present invention: the antioxidant is coated or sustained-released, and the treatment methods include but are not limited to one or more combinations of surface coating, film coating, microencapsulation, microspherization, microgranulation, nano-microgel spherization, dispersed gelation and macromolecular pore skeleton sustained release.
[0021] As a further embodiment of the present invention: the antioxidant includes one or more combinations of pentaerythritol, octadecyl propionate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, 2,6-di-tert-butyl-p-cresol, bisphenol A, bisphenol C, phenyl-p-phenylenediamine, and diphenyl-p-phenylenediamine, and the antioxidant is added in an amount of 0.01 to 15 parts.
[0022] Another object of the present invention is to provide a method for preparing a fiber-reinforced metal-based PMI composite foam, which specifically comprises the following steps:
[0023] Step 1: Preparation of PMI particles: Methacrylic acid, methacrylonitrile or acrylonitrile, initiator, foaming agent, crosslinking agent, and nucleating agent are mixed and dissolved uniformly to obtain a mixed solution, and the uniformly mixed solution is placed in a polymerization mold for polymerization at a polymerization temperature of 28 to 60° C. After the polymerization is completed, pre- and post-treatment, crushing, and screening are performed to obtain expandable polymethacrylimide resin particles, i.e., PMI particles;
[0024] Step 2: Selecting foam metal material, small granular metal powder or flaky metal particles to prepare the metal substrate;
[0025] Step 3: Add the adhesive to adjust the flexibility component, and process it according to the process. Add the plasticity and flexibility components to the adhesive, add the initiator, catalyst, and other additives, and process it according to the process to graft the flexibility group into the adhesive molecular chain. At the same time, add the dispersion performance regulator, antioxidant performance component, anti-aging agent and other components in a certain way and process, mix them evenly, and prepare them according to the process flow to obtain the adhesive component dedicated to the composite material;
[0026] Step 4: Preparation of fiber-reinforced material components: cutting the fibers in the selected fiber-reinforced material components into a certain length, usually between 0.01 and 10 mm, and then soaking them in an organic solvent, grafting a coupling agent, adding a surfactant, and obtaining the fibers used for the composite material.
[0027] Step 5: Soak the filler in an organic solvent, graft coupling groups on the surface, add surfactants, and enhance compatibility with other materials;
[0028] Step 6: PMI particles, metal-based materials, fiber-reinforced material components, fillers, adhesives, dispersants, plasticity regulators and other performance regulators are weighed in proportion, preheated, and mixed evenly to obtain a foamable mixed prepolymer;
[0029] Step 7: Weigh a certain weight of the foamable mixed prepolymer, put it into the mold, heat it according to the program, foam it, cool it, demould it, cut it, and process it into shape to obtain a lightweight composite foam material.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention provides a method for preparing a fiber-reinforced metal-based PMI composite material with better comprehensive performance. The composite material has the advantages of both metal materials and polymethacrylimide foam; it can overcome the defects of low surface hardness and easy wear of polymethacrylimide foam, as well as the shortcomings of high density, easy corrosion, and limited application scenarios of metal materials, and improve the ability of the material in lightweight and flexible application scenarios, and improve the convenience and speed of transportation. This type of composite material can be used in AI robot materials, solar photovoltaic panel materials, pontoons, floating bridges, gun stocks, baseballs, baseball bats, ice hockey, weapon chassis, submersibles and other fields;
[0032] 2. The present invention adjusts the comprehensive performance of the material in a variety of ways. Different from general composite foams, the adhesive used in the composite material has a component for adjusting flexibility added thereto. In the adhesive, the molecular chain of the flexible component is grafted onto the molecular chain of the adhesive. The prepared composite foam will not become brittle or powdery, but has better flexibility and better tensile properties.
[0033] 3. The present invention adds a fiber reinforcement component, which can better connect the metal base and the polymethacrylimide foam into an organic whole, prevent corner collapse and edge loss, and improve the overall mechanical properties;
[0034] 4. The present invention adds a plasticity regulating component to increase the flexibility and ductility of the composite material, improve the plasticity of material processing, and have better processing performance;
[0035] 5. The present invention adds an antioxidant performance regulating component to increase the antioxidant performance of the composite material, which will not change color or decay over a long period of time, and has improved stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the actual rendering of fiber-reinforced metal-based PMI composite foam.
[0037] Figure 2 The actual rendering of the structural component "blade" made of fiber-reinforced metal-based PMI composite foam. DETAILED DESCRIPTION
[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] A fiber-reinforced metal-based PMI composite foam comprises PMI particles, a metal substrate, a fiber-reinforced material component, a filler, an adhesive, a dispersant, a plasticizer, an antioxidant performance regulating component and other regulating components. The specific preparation process is as follows:
[0041] Step 1: Preparation of polymethacrylimide (PMI) resin particles
[0042] The raw materials include: methacrylic acid (1-80 parts), methacrylonitrile or acrylonitrile (1-70 parts), initiator (0.01-10 parts), foaming agent (0.01-15 parts), crosslinking agent (0.01-15 parts), nucleating agent (0.01-15 parts). These components are mixed and dissolved evenly to obtain a mixed solution. The mixed solution is placed in a polymerization mold for polymerization at a polymerization temperature of 28-60°C. After the polymerization is completed, pre- and post-treatment, crushing, and screening are performed to obtain expandable polymethacrylimide resin particles.
[0043] Step 2: Preparation of metal-based materials
[0044] The metal substrate generally uses metal foam materials, small granular metal powder, flaky metal particles and other metal materials. When selecting metal substrates, it is advisable to use small-sized, granular materials, which are easier to process. Small granular and powdered metal-based materials that can be machined and cut can be selected, such as foamed aluminum chips, stainless steel powder, iron chips, aluminum powder and other materials. The metal can be selected from one or more of the above materials. These metal-based materials are degreased, crushed, dried and sieved to obtain metal-based materials. The metal-based materials can be selected from small aluminum metal particles such as metal aluminum, aluminum alloy, foamed aluminum powder, foamed aluminum chips, etc.
[0045] The metal-based material may be small iron metal particles such as metallic iron, iron alloy, foamed iron, iron powder, and stainless steel powder.
[0046] The metal-based material may be small metal particle powders such as metallic zinc, zinc alloy, and zinc metal powder.
[0047] The metal-based material may be small metal particle powders such as magnesium metal, magnesium alloy, and magnesium metal powder.
[0048] Step 3: Preparation of adhesive components
[0049] The types of adhesives include: one or more of unsaturated resins, phenolic resins, polyurethanes, EVA hot melt adhesives, acrylate adhesives, epoxy resins, ethyl cyanoacrylate adhesives, cyanoacrylate adhesives, and methacrylate resin adhesives.
[0050] The adhesive component needs to be synthesized and processed by special process to prepare a component with certain properties such as flexibility, dispersibility, fluidity, anti-oxidation, compatibility, etc. This includes, but is not limited to, adding plasticity and flexibility adjustment components, grafting the flexibility components to the adhesive molecular chain according to the process treatment to become a flexible adhesive; adding dispersion performance regulators, antioxidants, anti-aging agents and other components according to a certain method and process, mixing them evenly, adding initiators, catalysts, molecular sieves and other additives, and preparing them according to a certain process flow to become a component with good flexibility, good anti-oxidation effect, good dispersibility and good compatibility, and obtaining an adhesive component dedicated to composite materials.
[0051] The dispersant is selected from one or more of silicone oil, butyl acetate, n-amyl acetate, isoamyl acetate, cyclohexane, carbon tetrachloride, tetrachloroethane, petroleum ether, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, fatty acid polyethylene glycol esters, 3020, 3007, 9010S and the like as a dispersibility adjustment and comprehensive performance adjustment component, and the added mass portion is 0.01-30 parts.
[0052] The plasticity regulating component is selected from one or more substances selected from benzoate, benzoate, trimellitate, zinc oxalate, magnesium oxalate, succinate, maleate, maleic anhydride, fumarate, adipate, azelaic acid ester, sebacate, polymethylsiloxane, and terminal hydroxyl polysiloxane, and the added amount is 0.01 to 30 parts.
[0053] The antioxidant performance regulating component is selected from one or more substances selected from antioxidant 1010 (pentaerythritol ester), antioxidant 1076 (octadecyl propionate), antioxidant-3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid), antioxidant-168 (tris(2,4-di-tert-butylphenyl) phosphite), antioxidant-626 (bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite), antioxidant 264 (2,6-di-tert-butyl-p-cresol), bisphenol A, bisphenol C, antioxidant DNP (phenyl-p-phenylenediamine), and antioxidant E (diphenyl-p-phenylenediamine) as the antioxidant performance regulating component, and the added amount is 0.01 to 15 parts.
[0054] Antioxidants need to be surface coated and slow-released, including but not limited to surface coating, coating film, microencapsulation, microspherization, microgranulation, nano-microgel spherization, dispersion gelation, macromolecular channel skeleton slow-release, etc., to achieve the effect of regular, slow and continuous release of antioxidants, to prevent the adverse effects of antioxidants on the reaction in the early stage, and to consume residual oxygen in the composite material, chelate metal ions, absorb free radicals, interrupt peroxides, and prevent the oxidation process of the composite material in the later stage. The effect of coating or slow-release treatment is preferably that the reaction is not affected in the early stage, and there is no discoloration, deterioration, brittleness, powdering, etc. in the later stage.
[0055] Step 4: Preparation of fiber-reinforced material components
[0056] Fiber-reinforced material components need to be processed by special processes, cut into a certain length, processed into a specific shape, and surface-grafted with chemical groups to ensure compatibility between organic matter and metals, including but not limited to organic solvent immersion, surface grafting, and dispersion treatment.
[0057] Fiber-reinforced materials can include carbon fiber, basalt fiber, glass fiber, graphene fiber, silicate fiber, metal fiber, polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber, viscose fiber, acetate fiber, cuprammonia fiber, etc.
[0058] The fibers need to be cut into a certain length, usually between 0.01 and 10 mm.
[0059] The fiber needs to be soaked in an organic solvent, grafted with a coupling agent, and treated by adding a surfactant to improve its compatibility with components such as the metal base, polymethacrylimide resin, and adhesive.
[0060] Step 5: Filler treatment
[0061] The filler needs to be surface treated, including but not limited to organic solvent soaking, surface grafting, and dispersion treatment. The filler with good surface treatment has better compatibility with PMI particles, metal substrates, fiber reinforcement components and other components.
[0062] The filler is selected from one or more of hollow microspheres, fumed silica, graphite powder, mica powder, silicate powder, marble powder, PMI foam powder, and calcium carbonate powder as an antioxidant performance adjustment component, and the addition amount is 0.01 to 30 parts. The filler needs to be soaked in a solvent, a coupling agent is grafted on the surface, and a dispersant is added to enhance the compatibility with other materials.
[0063] Step 6: Preparation of foamable prepolymer
[0064] The foamable polymethacrylimide resin particles, metal-based materials, fiber-reinforced material components, fillers, adhesives, dispersants, plasticity regulators, antioxidant performance regulating components and other additives are weighed in proportion, preheated and mixed evenly to obtain a foamable mixed prepolymer.
[0065] Step 7: Foaming of composite materials
[0066] A certain weight of the foamable mixed prepolymer is weighed and put into a mold, and the temperature is increased according to a program, foamed, cooled, demoulded, cut, and processed to obtain a lightweight composite foam material.
[0067] In step seven, the foaming method can be conventional electric heating method.
[0068] In step seven, the foaming method can be a heating method using gas to provide thermal energy.
[0069] In step seven, the foaming method can be microwave rapid heating method foaming.
[0070] The specific material ratios in Example 1 are shown in Table 1:
[0071] Table 1:
[0072] 1 PMI resin pellets 80 servings 2 Surface treated aluminum foam particles 60 servings 3 Toughened adhesive 30 servings 4 Surface treated basalt fiber 8 servings 5 Surface treated fumed silica 16 servings 6 Parabens 6 servings 7 Encapsulated Antioxidant 1076 5 servings 8 Silicone oil 3 servings
[0073] After foaming, the density is 296kg / m 3 The closed porosity is more than 93%, the compression strength is 5.9MPa, the compression modulus is 328MPa; the tensile strength is 2.3MPa, the tensile modulus is 316MPa, and the compression energy absorption rate is 4.2J / cm 3 The surface has the properties of foam aluminum, and its hardness is close to that of foam aluminum. It can be cut, drilled, and bonded, and is not easy to discolor or age.
[0074] Unlike ordinary composite foams, the adhesive used in this composite material has components for adjusting flexibility added to it. Through process processing, the flexible molecular chains are grafted into the molecular chains of the adhesive. The prepared composite foam will not become brittle or powdery, but will have better flexibility and tensile properties.
[0075] Different from general composite foams, this composite material has fiber-reinforced components added to better connect the metal matrix and polymethacrylimide foam into an organic whole, preventing corner chipping and edge falling, and improving overall mechanical properties.
[0076] Different from common composite foams, this composite material has antioxidant performance regulating components added to increase the antioxidant performance of the composite material. It will not change color or decay over a long period of time, and its stability is improved.
[0077] At the same time, the composite material prepared by this method overcomes the defects of low surface hardness and easy wear of polymethacrylimide foam, and can also overcome the shortcomings of high density, easy corrosion and limited application scenarios of metal materials. This type of composite material can be used in pontoon bridges, floating bridges, gun stocks, baseballs, baseball bats, ice hockey, weapon chassis, submersibles and other fields.
[0078] The fiber-reinforced metal-based PMI composite material has an adhesive grafted with flexible molecular chains, which makes it more flexible. Fiber-reinforced components, plasticity-adjusting components, and antioxidant components are added to the composite material, which makes it more stable, improves processing performance, and significantly enhances its overall comprehensive performance.
[0079] Summary: This method provides a method for preparing fiber-reinforced metal-based PMI composites with better comprehensive performance through adjustments in a variety of ways, reduces the density of the composite material, enhances the corrosion resistance of the material, improves the ability of the material in lightweight and flexible applications, and improves the convenience and speed of transportation.
[0080] Example 2
[0081] The material ratio of the embodiment was adjusted, and the ratio of the metal-based material was appropriately increased, as shown in Table 2, to prepare a fiber-reinforced metal-based PMI composite foam.
[0082] Table 2:
[0083]
[0084]
[0085] After foaming, the density is 428kg / m 3 The closed porosity is more than 92%, the compression strength is 6.32MPa, the compression modulus is 353MPa; the tensile strength is 2.35MPa, the tensile modulus is 336MPa, and the compression energy absorption rate is 4.5J / cm 3 The surface has the properties of aluminum alloy, but the density is much lower than that of aluminum alloy, and the hardness is close to that of aluminum alloy. It can be cut, drilled, and bonded, and is not easy to change color or age.
[0086] The composite material can be used to prepare the robot's extension and bending arms. It has the texture of metal materials and the characteristics of light weight, flexible bending, good buffering performance, fatigue resistance and long service life.
[0087] Example 3
[0088] The material ratio of the embodiment was adjusted, and the ratio of PMI resin and hollow microsphere filler was appropriately increased, as shown in Table 3, to prepare a fiber-reinforced metal-based PMI composite foam.
[0089] Table 3:
[0090] 1 PMI resin pellets 85 copies 2 Surface treated aluminum foam particles 30 servings 3 Toughened adhesive 38 servings 4 Surface treated carbon fiber 12 servings 5 Surface-coupling treated hollow microspheres 45 servings 6 Sebacate 7 servings 7 Film coated antioxidant 3114 6 servings 8 Isoamyl acetate 3.5 servings
[0091] After foaming, the density is 268kg / m 3 The closed porosity is more than 95%, the compression strength is 3.6MPa, the compression modulus is 216MPa; the tensile strength is 1.9MPa, the tensile modulus is 215MPa, and the compression energy absorption rate is 3.6J / cm 3 , can be cut, drilled and bonded.
[0092] This composite material can be used for the preparation of temporary pontoon bridges and floating bridges. This composite material has a small specific gravity, low density, large buoyancy, large load capacity, and is easy to erect. This composite material can also be used as the material of ship "blades". It has the characteristics of low density, good fatigue resistance, and long service life. The specific physical effects are as follows Figure 2 shown.
[0093] It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Although this specification is described in accordance with the implementation modes, not every implementation mode includes only one technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A fiber-reinforced metal-based PMI composite foam, characterized in that: Including PMI particles, metal substrates, fiber reinforcement components, fillers, adhesives, dispersion performance adjustment components, plasticity adjustment components, antioxidant performance adjustment components and other performance adjustment components; The PMI particles include, by weight, methacrylic acid (1 to 80 parts), methacrylonitrile or acrylonitrile (1 to 70 parts), an initiator (0.01 to 10 parts), a foaming agent (0.01 to 15 parts), a crosslinking agent (0.01 to 15 parts), and a nucleating agent (0.01 to 15 parts); The metal substrate includes one or more combinations of foamed metal materials, small granular metal powders or flaky metal particles; The adhesive is added with a flexibility-adjusting component, in which a flexible, long-chain component is grafted into the adhesive molecular chain to form a flexible adhesive, a dispersion performance regulator, an antioxidant, an anti-aging agent and other components are added, mixed evenly, an initiator, a catalyst, a molecular sieve and an auxiliary agent are added and synthesized according to the process flow to obtain an adhesive component used in the composite material; The antioxidant performance adjusting component includes an antioxidant, a coating agent or a sustained-release agent, and the antioxidant needs to be coated or sustained-released; The filler is selected from one or more combinations of hollow microspheres, fumed silica, graphite powder, mica powder, silicate powder, marble powder, PMI foam powder, and calcium carbonate powder. The filler needs to be surface treated, including but not limited to organic solvent immersion, surface grafting, and dispersion treatment; The fiber reinforcement material component and the filler are soaked in an organic solvent and surface treated, and the method includes but is not limited to one or more combinations of organic solvent soaking, surface grafting chemical groups and dispersion treatment methods.
2. The fiber-reinforced metal-based PMI composite foam according to claim 1, characterized in that: The adhesive comprises one or more combinations of unsaturated resin, phenolic resin, polyurethane, EVA hot melt adhesive, acrylate adhesive, epoxy resin, ethyl cyanoacrylate adhesive, cyanoacrylate adhesive, and methacrylic resin adhesive. The adhesive is added with a flexible component, a dispersing performance regulator, an antioxidant, and an anti-aging agent according to the process.
3. The fiber-reinforced metal-based PMI composite foam according to claim 1, characterized in that: The fiber reinforcement material component includes one or more combinations of carbon fiber, basalt fiber, glass fiber, graphene fiber, silicate fiber, metal fiber, polyester fiber, polyamide fiber, polyvinyl alcohol fiber, polyacrylonitrile fiber, polypropylene fiber, polyvinyl chloride fiber, viscose fiber, acetate fiber, and cuprammonia fiber.
4. The fiber-reinforced metal-based PMI composite foam according to claim 1, characterized in that: The fiber reinforcement material component is degreased on the surface, cut into a certain length, processed into a specific shape, roughened on the surface, grafted with coupling groups, and added with a surfactant to obtain the fiber used for the composite material. The fiber reinforcement material component has a length range of 0.01 to 10 mm.
5. The fiber-reinforced metal-based PMI composite foam according to claim 1, characterized in that: The dispersant component includes one or more of silicone oil, butyl acetate, n-amyl acetate, isoamyl acetate, cyclohexane, carbon tetrachloride, tetrachloroethane, petroleum ether, triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, cellulose derivatives, polyacrylamide, guar gum, fatty acid polyethylene glycol ester, 3020, 3007, 9010S, and the added mass portion of the dispersant component is 0.01-30 parts.
6. According to the fiber-reinforced metal-based PMI composite foam according to claim 1, the plasticity regulating component includes one or more combinations of benzoates, phthalates, trimellitates, zinc oxalate, magnesium oxalate, succinate, maleate, maleic anhydride, fumarate, adipate, azelaic acid ester, sebacate, polymethylsiloxane, and terminal hydroxyl polysiloxane, and the amount of the plasticity regulating component added is 0.01 to 30 parts.
7. According to claim 1, the fiber-reinforced metal-based PMI composite foam, the antioxidant is coated or sustained-released, and the treatment methods include but are not limited to one or more combinations of surface coating, coating film, microencapsulation, microspheroidization, microgranulation, nano-microgel spheroidization, dispersed gelation and macromolecular pore skeleton sustained release methods.
8. A fiber-reinforced metal-based PMI composite foam according to claim 7, wherein the antioxidant comprises one or more combinations of pentaerythritol ester, octadecyl propionate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, tris(2,4-di-tert-butylphenyl) phosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, 2,6-di-tert-butyl-p-cresol, bisphenol A, bisphenol C, phenyl-p-phenylenediamine, and diphenyl-p-phenylenediamine, and the antioxidant is added in an amount of 0.01 to 15 parts.
9. A method for preparing a fiber-reinforced metal-based PMI composite foam, according to any one of claims 1 to 8, characterized in that: The specific steps include: Step 1: Preparation of PMI particles: Methacrylic acid, methacrylonitrile or acrylonitrile, initiator, foaming agent, crosslinking agent, and nucleating agent are mixed and dissolved uniformly to obtain a mixed solution, and the uniformly mixed solution is placed in a polymerization mold for polymerization at a polymerization temperature of 28 to 60° C. After the polymerization is completed, pre- and post-treatment, crushing, and screening are performed to obtain expandable polymethacrylimide resin particles, i.e., PMI particles; Step 2: Selecting foam metal material, small granular metal powder or flaky metal particles to prepare the metal substrate; Step 3: Add flexibility-adjusting components to the adhesive. Add flexibility-adjusting, long-chain components to the adhesive, add initiators, catalysts and other additives, synthesize according to the process, and graft the flexible groups into the adhesive molecular chains. At the same time, a dispersing property regulator, an antioxidant property component, an anti-aging agent and other components are added, mixed evenly, and synthesized in a certain manner and process to obtain an adhesive component dedicated to the composite material; Step 4: Preparation of fiber-reinforced material components, cutting the fibers in the selected fiber-reinforced material components into a certain length, usually between 0.01 and 10 mm, and then soaking them in an organic solvent, grafting a coupling agent, adding a surfactant, and obtaining a fiber component used for the composite material; Step 5: Soak the filler in an organic solvent, graft coupling groups on the surface, add surfactants to enhance compatibility with other materials, and coat or slow-release the antioxidant performance regulating component; Step 6: PMI particles, metal-based materials, fiber-reinforced material components, fillers, adhesives, additives, dispersants, plasticity regulators, antioxidant performance regulating components and other additives are weighed in proportion, preheated, and mixed evenly to obtain a foamable mixed prepolymer; Step 7: Weigh a certain weight of the foamable mixed prepolymer, put it into the mold, heat it according to the program, foam it, cool it, demould it, cut it, and process it into shape to obtain a lightweight composite foam material.