Dry-type casing composite material based on dielectrophoresis regulation and control as well as preparation method and application of dry-type casing composite material
Through dielerophoretic regulation technology, the nanofillers are arranged in a directional manner in epoxy resin, which solves the problem of degradation of insulation performance caused by thermal stress aging of high-pressure epoxy resin sleeves, which significantly improves thermal conductivity and toughness, and extends service life.
Patent Information
- Application Number
- CN202410958066.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The electrical insulation performance of high-voltage epoxy resin casings decreases due to thermal stress aging during long-term operation, increasing the risk of failure. The performance of existing nanocomposites does not increase but decreases after doping large volume fractions.
Using dielerophoretic regulation technology, by adding modified CNC and modified h-BN to the epoxy resin, the AC electric field is used to arrange the nanofillers in an orderly manner along the direction of the electric field, and the directional state is fixed in combination with the curing process to improve the thermal conductivity of the composite material. and resilience.
It significantly improves the thermal conductivity and toughness of composite materials, extends the service life under high pressure, and achieves performance improvements under low usage, and increases the thermal conductivity by 78% under 300V/mm and 10kHz conditions.
Smart Images

Figure CN118879025A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of epoxy resin materials for high voltage, and relates to a dry-type bushing epoxy resin composite material based on dielectrophoresis regulation, and a preparation method and application thereof. Background Art
[0002] As an important component of converter transformers, epoxy resin impregnated paper bushings (also known as dry bushings) have been widely used in UHV power grids due to their large installation angles, strong earthquake resistance, and low partial discharge levels. However, according to the statistical results of the Cigre report, as the voltage level increases, the proportion of transformer failures caused by bushings increases. As the operating years increase, the bushings age due to severe thermal stress, thereby reducing the electrical insulation performance of the bushings. The above insulation problems can easily cause power equipment failures or even damage.
[0003] In order to overcome these challenges and avoid the risk of the above accidents, researchers began to explore new methods of material improvement. In this context, epoxy resin nanocomposites have become a research field that has attracted much attention. Compared with pure epoxy resin, epoxy resin composites reinforced with micron- or even nano-scale inorganic or organic fillers (such as alumina, boron nitride, and nanocellulose) have higher dielectric breakdown voltage, better thermal conductivity and mechanical properties, and have therefore become the preferred insulation material in high-voltage applications.
[0004] However, inorganic nanofillers have poor compatibility with the epoxy resin matrix. Although they can improve the electrical, mechanical and thermal conductivity of the material to a certain extent, there is still a disadvantage that the material performance decreases instead of increases after large volume fraction doping. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a dry sleeve epoxy resin composite material based on dielectrophoresis regulation and its preparation method and application. The preparation method of the present invention can orient the modified CNC and modified h-BN in the composite material into chains, reduce the dosage and significantly improve the toughness, thermal stability and thermal conductivity of the composite material.
[0006] According to one aspect of the present invention, a method for preparing a dry-type casing composite material based on dielectrophoresis regulation is provided, comprising the following steps:
[0007] (1) After heating the epoxy resin, adding the modified CNC suspension to mix, and then adding the modified h-BN to mix to obtain a mixed solution, wherein the amount of the modified CNC added is 0.1% by weight of the epoxy resin, and the amount of the modified h-BN added is 1% by weight of the epoxy resin;
[0008] (2) adding a curing agent and an accelerator to the mixed liquid, stirring evenly and extracting bubbles, placing the mixed liquid in a mold with electrodes, and pre-curing at 70-80° C. to obtain a pre-cured material;
[0009] (3) After cooling the pre-cured material to 40-45° C., an AC electric field is applied and maintained for 30-35 min. The temperature is then raised to 60-65° C. and maintained for 9-11 min. After removing the AC electric field, the temperature is raised and cured to obtain a composite material.
[0010] In the above preparation method, modified CNC (nanocellulose) and modified h-BN (hexagonal boron nitride) are used as nanofillers. The blending of the two can improve the thermal conductivity of the composite material. When an AC electric field is applied during the curing process, due to the high aspect ratio of CNC, after mixing with modified h-BN, the entanglement connection between the nanoparticles will be effectively improved, and the construction of heat conduction channels will be promoted, thereby significantly improving the thermal conductivity of the composite material at a low dosage, thereby extending the service life of the composite material under high pressure.
[0011] When an AC electric field is applied, driven by dielectrophoresis, the modified CNC and modified h-BN gradually evolve from a randomly distributed state to an orderly arrangement along the direction of the electric field. However, when the AC electric field is removed, the two particles will return from a state of directional arrangement along the electric field to a disordered state. Therefore, pre-curing is used to initially increase the viscosity of the system, and then curing is performed while applying an AC electric field, which can fix the directionally arranged particles and maintain their directional arrangement state.
[0012] Optionally, the modified CNC accounts for 5wt%-7wt% in the suspension containing modified CNC, and the pre-curing time is 10-15min.
[0013] Optionally, in step (3), the temperature for curing after removing the AC electric field is 70-90° C. and the time is 8-12 hours.
[0014] Optionally, the electric field strength of the AC electric field in step (3) is 100-300 V / mm.
[0015] Optionally, the electric field frequency of the AC electric field in step (3) is 8-10 kHz.
[0016] The electric field strength and frequency match the amount of filler added, which can promote the arrangement of the two fillers into chains and achieve a significant improvement in performance when low-content fillers are added. When the electric field strength is high and the electric field frequency is low, the filler is prone to "field-induced turbulence" in the system, which seriously hinders the interaction between particles, making it impossible for CNC and h-BN to form chains, and thus unable to achieve the improvement of the thermal conductivity of the composite material.
[0017] Optionally, the modification method of the modified h-BN is: adding h-BN to a solution of a silane coupling agent, adjusting the pH to 4-5, heating to 80-90° C. for 6-8 hours after ultrasonic treatment, cooling, rinsing, and drying to obtain the modified h-BN;
[0018] Preferably, the silane coupling agent is KH560, and the amount of the silane coupling agent used accounts for 1.5-2.0% of the total weight of h-BN.
[0019] The modified h-BN prepared by the above method can improve the dispersibility of h-BN, and the independence of each h-BN sheet is improved, which helps to improve the agglomeration of BN nanofillers.
[0020] Optionally, the particle size of the modified h-BN is 50 nm.
[0021] Optionally, the modification method of the modified CNC is: placing CNC in water to obtain a CNC suspension, the weight of CNC accounts for 1.5-2.0% of the weight of water, heating to 30-35°C, then using nitric acid to adjust the pH to 0.9-1.1 to obtain a pre-modified liquid, then adding ammonium cerium nitrate and stirring evenly, and finally adding methyl acrylate to carry out graft polymerization reaction, and separating to obtain modified CNC after the reaction is completed.
[0022] Optionally, in 1L of pre-modified liquid, the amount of cerium ammonium nitrate added is 4.9-5.1 mmol, and the weight ratio of methyl acrylate to CNC is 3-4:1, preferably 3:1.
[0023] Ammonium cerium nitrate can promote the grafting polymerization of methyl acrylate on CNC, thereby achieving lipophilic treatment of CNC. It has been verified that when CNC modified with methyl acrylate is added to epoxy resin, the toughness and thermal conductivity of epoxy resin can be improved. Within the addition range of 2%, the thermal conductivity increases with the increase of doping concentration, but when the addition amount is greater than 2%, the thermal conductivity decreases instead.
[0024] Optionally, the amount of the curing agent added is 80-90% of the weight of the epoxy resin, and the curing agent is selected from methyl hexahydrophthalic anhydride;
[0025] The amount of the accelerator added is 1-2% of the weight of the epoxy resin, and the accelerator is selected from DMP-30.
[0026] According to another aspect of the present invention, there is provided a CNC, h-BN and epoxy resin composite material prepared by any of the above-mentioned methods for preparing a dry-type bushing composite material based on dielectrophoresis control.
[0027] According to another aspect of the present invention, there is provided application of a composite material prepared by any of the preparation methods described above in a high-voltage insulation device.
[0028] The beneficial effects of the present invention include but are not limited to:
[0029] 1. The present invention is based on the preparation method of the dry-type casing composite material regulated by dielectrophoresis, adopts CNC and h-BN to dope the epoxy resin, and combines the dielectrophoresis technology to orient the above fillers, providing a new technical concept for preparing high thermal conductivity epoxy resin composite materials with low filler concentration.
[0030] 2. Compared with random filler composite materials without DEP regulation, the dry-type bushing composite material of the present invention has significantly improved thermal conductivity. The composite material obtained under the conditions of 300 V / mm and 10 kHz has the best thermal conductivity, and the thermal conductivity growth rate at 100°C can reach 78%.
[0031] 3. According to the preparation method of dry-type casing composite materials based on dielectrophoresis regulation of the present invention, the directional arrangement of nanofillers along the direction of the electric field is achieved through the alternating current electric field dielectrophoresis technology, thereby further improving the thermal conductivity of the composite material, and the study found that the greater the electric field intensity and the higher the electric field frequency, the higher the chain degree of the nanoparticles. Under different field strengths, as the chain degree of the particles increases, the conductivity and dielectric loss of the mixed system show a downward trend, and the lower the electric field frequency, the greater the dielectric loss of the mixed system.
[0032] 4. According to the preparation method of the dry sleeve composite material based on dielectrophoresis regulation of the present invention, the addition of modified CNC significantly improves the toughness and thermal conductivity of the epoxy resin, and the above-mentioned doping amount will not have a significant effect on the dielectric loss of the epoxy resin; the addition amount of modified CNC is 10% of the modified h-BN. In this case, the modified CNC can act as a bridge connecting the modified h-BN, which is beneficial to the contact and winding between the modified h-BN. While improving the interface between the modified h-BN and the epoxy resin matrix, it promotes the construction of the thermal conductive channel and improves the thermal conductivity level of the composite material.
[0033] 5. According to the preparation method of the dry-type sleeve composite material based on dielectrophoresis regulation of the present invention, the directional chain formation of modified CNC and modified h-BN is promoted by appropriate curing conditions and electric field conditions, thereby significantly improving the thermal conductivity of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0035] Figure 1 It is the Fourier transform infrared spectra of the unmodified CNC and methyl acrylate (MMA) modified CNC involved in Example 1 of the present invention.
[0036] Figure 2 This is a schematic diagram of the C element peak fitting results of the unmodified CNC and modified CNC1# involved in Example 1 of the present invention.
[0037] Figure 3 These are SEM test images of the unmodified h-BN and modified h-BN 1# involved in Example 2 of the present invention.
[0038] Figure 4 This is a diagram of the mold used in Example 3 of the present invention and the sample prepared.
[0039] Figure 5 This is a test graph of thermal conductivity of composite materials 1#-3# prepared in Example 3 of the present invention, comparative composite material D1# and pure epoxy resin.
[0040] Figure 6 This is a test graph of thermal conductivity of composite materials 4#-5#, composite material 3#, comparative composite material D1# and pure epoxy resin prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0041] The present invention is described in detail below in conjunction with embodiments, but the present invention is not limited to these embodiments.
[0042] Unless otherwise specified, the raw materials in the examples of the present invention are purchased through commercial channels. The epoxy resin is E51 epoxy resin with an epoxy value of 0.48-0.54, purchased from Nanchang Weiligute Flagship Store; the purity of methyl hexahydrophthalic anhydride is 98%, purchased from Roan Reagent; the release agent model is: 717, purchased from Walkerson New Materials Co., Ltd.; the accelerator DMP-30 is purchased from Suzhou Qicaishi Composite Materials Co., Ltd.; and the hexagonal boron nitride nanosheets are purchased from Shanghai MCC New Materials Co., Ltd.
[0043] The preparation method of unmodified CNC is as follows: first, take 200g (dry weight) of air-dried cotton fiber, add it to a pre-prepared 60% sulfuric acid solution according to a solid-liquid ratio of 1:10, and the reaction is carried out in a constant temperature and constant speed water bath, the temperature is 45°C, the stirring speed is 170r / min, and the reaction time is 3 hours; next, the CNC suspension after the reaction is transferred to a 10L beaker, and an appropriate amount of deionized water is added to dilute it to 5L; then the suspension is centrifuged using a refrigerated centrifuge to separate the solids. The separated solids are added to water again and placed in a dialysis bag for dialysis until the pH value is neutral; stirring is required during the dialysis process, and the dialysis solution is replaced every 8 hours. The concentration of the dialyzed CNC suspension is adjusted to 1%, and then ultrasonic treatment is performed (600W, 10 minutes); finally, the treated CNC powder is stored in a refrigerator for use.
[0044] Unless otherwise specified, the methods used in the embodiments of the present invention are conventional methods in the prior art.
[0045] Example 1 Preparation method of modified CNC
[0046] Modified CNC1#
[0047] The preparation method is:
[0048] S1: 15.0 g of unmodified CNC was placed in 750 ml of water to obtain a CNC suspension, which was added to a 1000 ml three-necked flask equipped with a stirring device, the three-necked flask was placed in a constant temperature water bath at 30°C, and the pH value of the CNC suspension was adjusted to 1.0 with 20% nitric acid to obtain a pre-modified solution;
[0049] S2: Then, add ammonium cerium nitrate to the pre-modified solution. In 1L of the pre-modified solution, the amount of ammonium cerium nitrate added is 5.0 mmol. Stir evenly at a stirring speed of 500 rpm, and introduce nitrogen for 30 minutes to remove oxygen in the reaction system.
[0050] S3: adding 45.0 g of methyl acrylate solution dropwise by a peristaltic pump to carry out graft polymerization. The reaction equation is shown in formula (1). The methyl acrylate is added dropwise for 60 minutes. After the addition is stopped, stirring is continued for 2 hours, and then the reaction is terminated.
[0051] S4: After the reaction is completed, use a 10,000 rpm centrifuge at 4°C for 15 minutes to separate the solid and the liquid, and then rinse the solid with deionized water until it is neutral to remove the ammonium cerium nitrate and nitric acid; the washed solid is dispersed with acetone and centrifuged again at 10,000 rpm and 4°C for 15 minutes to separate the solid and the liquid, and finally the solid is dried to obtain modified CNC1#.
[0052]
[0053] Modified CNC2#
[0054] The preparation method of modified CNC2# is different from that of modified CNC1# in that the overall reaction temperature is 35°C, and the amount of methyl acrylate added is 60.0 g, thereby obtaining modified CNC2#.
[0055] Test Example 1
[0056] 1. Infrared spectroscopy analysis: Infrared spectroscopy analysis of unmodified CNC, modified CNC1# and modified CNC2# was performed using reflection mode: wavelength range 7800cm -1 ~350cm -1 , signal-to-noise ratio 45000:1, resolution ≤0.4cm -1, and the Fourier transform infrared spectrum of the material is obtained. The results are shown in Figure 1 The spectra of modified CNC1# and modified CNC2# are the same, so Figure 1 MMA-CNC is used in all of them.
[0057] from Figure 1 It can be seen that for the pure CNC sample, at 3335.13 cm -1 (-OH group stretching vibration), 2899.00cm -1 There are obvious vibration peaks at (-CH group stretching vibration), reflecting the specific chemical bonds and functional groups in the molecular structure of CNC samples. For MMA-CNC, new vibration peaks were observed, and the most significant change occurred at 1723.7cm -1 These new vibration peaks indicate the successful esterification of MMA.
[0058] 2.XPS analysis
[0059] The electron spectrometer was used to measure the energy distribution of photoelectrons and Auger electrons emitted from the surfaces of unmodified CNC samples and modified CNC1# samples irradiated by X-ray photons for correlation analysis. First, the sample was scanned in full spectrum. The elemental composition of the sample was preliminarily determined, and the distribution of three elements C, O, and Si on its surface was obtained. The results are shown in Table 1. Analysis of the results in Table 1 shows that compared with the original CNC and modified CNC1# samples, the ratio of C and O elements in modified CNC1# has changed, indicating that the chemical structure of CNC has changed during the modification process.
[0060] Table 1
[0061]
[0062] In order to further understand the surface chemical characteristics of the sample, the peak separation of C element was performed. Figure 2 and Table 2, where (a) is a schematic diagram of the C element peak fitting results of unmodified CNC, and (b) is a schematic diagram of the C element peak fitting results of modified CNC1#. Figure 2 It can be seen that the carbon element signal of the CNC sample has been decomposed into different carbon components. Specifically, there are three types of carbon components, C1, C2 and C3, corresponding to different chemical bonds and functional groups. C1 is mainly related to the CC / CH bond, indicating the presence of CC bonds and CH bonds of CNC in the sample; C2 corresponds to the CO bond of alcohol and ether, indicating the presence of alcohol and ether functional groups in the sample; C3 is related to the acetal group OCO and C=O bond, indicating the presence of acetal group and ketone functional groups in the sample.
[0063] Table 2
[0064]
[0065] As shown in Table 2, the proportion of C1 in the modified CNC1# sample increased, while the proportions of C2 and C3 decreased accordingly, indicating that grafting modification increased the C1 component on the CNC surface and reduced the proportions of C2 and C3 components. The above results show that the chemical structure of the modified CNC samples has changed, and also reflect the degree of modification of the samples.
[0066] Example 2 Preparation method of modified h-BN
[0067] Modified h-BN1#
[0068] The preparation method is:
[0069] S1: h-BN was added to a 95% ethanol aqueous solution of KH560, and the pH was adjusted to 4-5 with diluted acetic acid. The amount of KH560 accounted for 1.5% of the total weight of h-BN;
[0070] S2: The mixture was ultrasonically stirred for 30 min, and then heated to 80 °C for 6 h;
[0071] S3: After cooling to room temperature, rinse with ethanol at least 3 times, and finally dry in an oven at 120°C for 10 h to obtain modified h-BN1#.
[0072] Modified h-BN2#
[0073] The preparation method of modified h-BN2# is different from that of modified h-BN1# in that the amount of KH560 used in step S1 accounts for 1.5% of the total weight of h-BN, and in step S2, it is heated to 90°C for 8 hours to obtain modified h-BN2#.
[0074] Test Example 2
[0075] 1. SEM analysis: The morphology of the dried h-BN powder and modified h-BN1# was observed using a scanning electron microscope (SEM) at a magnification of 10k. The results are as follows: Figure 3 As shown, (a) is the test graph of unmodified h-BN, and (b) is the test graph of modified h-BN1#. It can be seen that unmodified h-BN has a large number of agglomerates and poor dispersion, while the number of agglomerates of modified h-BN1# is significantly reduced, and the independence of each BN sheet is improved, proving that chemical grafting helps to improve the agglomeration of BN nanofillers.
[0076] Example 3
[0077] This embodiment relates to a method for preparing a dry-type casing composite material based on dielectrophoresis control, comprising the following steps:
[0078] (1) After heating the epoxy resin at 70° C. for 10 min, the epoxy resin was added to an acetone suspension containing modified CNC and mixed, and then the modified h-BN was added to obtain a mixed solution, wherein the amount of the modified CNC added was 0.1% of the weight of the epoxy resin, and the amount of the modified h-BN added was 1% of the weight of the epoxy resin;
[0079] (2) adding methyl hexahydrophthalic anhydride and DMP-30 to the mixed solution, wherein the amount of methyl hexahydrophthalic anhydride added is 80-90% of the weight of the epoxy resin, and the amount of DMP-30 added is 1-2% of the weight of the epoxy resin, stirring evenly, extracting bubbles, placing in a mold with electrodes, and pre-curing at 70-80° C. for 10-15 minutes to obtain a pre-cured material;
[0080] (3) After cooling the pre-cured material to 40-45°C, an AC electric field is applied with an electric field strength of 100-300 V / mm and an electric field frequency of 8-10 kHz for 30-35 min, and then the temperature is raised to 60-65°C and maintained for 10 min. After removing the AC electric field, the temperature is raised to 70-90°C and cured for 8-12 h to obtain a composite material.
[0081] The mold reference used in this preparation method Figure 4 , where (a) and (b) are the appearance and internal structure of the mold. Two copper plate electrodes are fixed inside the polytetrafluoroethylene mold. Metal wires are welded on the edges of the two electrodes and led out to serve as the connection between the signal source and the electrodes. (c) is the thermal conductivity test sample after curing. The sample is a square sheet with a thickness of 1 mm. The thermal conductivity test direction is the thickness direction of the sample. Before the test, graphite needs to be evenly sprayed on the sample surface to increase the reflectance of the sample.
[0082] The preparation of composite materials 1#-3# and comparative composite material D1# all include the following steps:
[0083] (1) After heating the epoxy resin at 70° C. for 10 min, an acetone suspension containing 5 wt % of modified CNC was added and mixed, and then the modified h-BN was added and mixed to obtain a mixed solution, wherein the amount of the modified CNC added was 0.1% of the weight of the epoxy resin, and the amount of the modified h-BN added was 1% of the weight of the epoxy resin;
[0084] (2) adding methyl hexahydrophthalic anhydride and DMP-30 to the mixed solution, wherein the amount of methyl hexahydrophthalic anhydride added is 90% of the weight of the epoxy resin, and the amount of DMP-30 added is 1% of the weight of the epoxy resin, stirring the mixed solution to remove air bubbles, placing the mixed solution in a mold with electrodes, and pre-curing the mixed solution at 70-80° C. for 10 minutes to obtain a pre-cured material;
[0085] (3) After the pre-cured material is cooled to 45°C, an AC electric field is applied with an electric field strength of 100-300 V / mm and an electric field frequency of 10 kHz for 30 min, and then the temperature is raised to 65°C and maintained for 10 min. After the AC electric field is removed, the temperature is raised to 85°C and cured for 10 h to obtain a composite material.
[0086] The composite material D1# is not subjected to an electric field in step (3); the electric field strength of the composite material 1# is 100 V / mm; the electric field strength of the composite material 2# is 200 V / mm; and the electric field strength of the composite material 3# is 300 V / mm.
[0087] Test Example 3
[0088] The thermal conductivity of the composite materials 1#-3# obtained in Example 3 and the comparative composite material D1# was tested by a laser thermal conductivity analyzer (LFA447), and pure epoxy resin EP was used for comparison. The results are shown in Figure 5 The specific test method is:
[0089] The sample is made into a square sheet with a side length of 10mm and a thickness of 1-2mm. The surface of the prepared sample is polished and cleaned, and the sample surface is sprayed with graphite spray to form a uniform and dense film on the surface after drying. A constant temperature point T is set at the control end. After the furnace reaches the target temperature, the laser source or flash xenon lamp will emit a beam of light pulses, which are evenly irradiated on the lower surface of the sample. After the surface absorbs the light energy, the temperature rises instantly. At this time, the lower surface acts as a heating end and conducts energy to the upper surface in a one-dimensional heat transfer manner. The infrared detector continuously measures the temperature rise process of the center of the upper surface of the sample and obtains the temperature rise curve. Ideally, the width of the light pulse is close to infinitesimal, so the conduction of heat flow inside the sample can be regarded as one-dimensional heat transfer, and there is no lateral heat flow loss. The thermal diffusion coefficient of the sample at temperature T can be further calculated by measuring the half-heating time. When the specific heat Cp and density are known, the thermal conductivity can be calculated by the following formula:
[0090] λ(T)=α(T)·Cp(T)·ρ(T).
[0091] Figure 5(a) is the curve of the change of thermal conductivity of the five materials with temperature. Among them, the thermal conductivity of pure epoxy resin EP is the lowest, and the overall level of thermal conductivity is distributed between 0.2 and 0.26W / (m*K). After adding h-BN and CNC, the thermal conductivity of composite materials 1#-3# and comparative composite material D1# are improved. For temperature points below 100℃, except for the thermal conductivity of composite material 3# prepared with an electric field strength of 300V / mm, which is significantly improved, the thermal conductivity of other composite materials is relatively small, and the improvement of thermal conductivity compared with pure epoxy resin is limited. When the temperature point is 100℃ and above, the higher the electric field strength, the higher the thermal conductivity of the composite material, and the difference in thermal conductivity of each material becomes gradually obvious, showing a phenomenon of hierarchical distribution with the size of the electric field, and no cross distribution occurs.
[0092] Extract the thermal conductivity of each material at 100°C and compare it with pure epoxy resin, calculate the growth rate of thermal conductivity and draw a bar chart as shown below: Figure 5 (b) It was observed that the thermal conductivity of the composite material D1# increased by 18% compared with that of pure epoxy resin. After applying an AC electric field, the growth rate of the thermal conductivity of the composite material increased with the increase of the electric field strength. When the electric field strength was 300V / mm, the growth rate of the thermal conductivity of the composite material 3# could reach 78%.
[0093] Therefore, it can be seen that when the temperature is below 100°C, only the thermal conductivity of the composite material 3# prepared by an electric field of 300V / mm is significantly better than that of the comparative composite material D1#. At this time, the low electric field intensity greatly limits the orientation level of the two fillers in the epoxy resin, thereby affecting the improvement of the thermal conductivity of the material.
[0094] The thermal conductivity of composite materials 1#-3# above 100°C is significantly improved compared with pure epoxy resin and comparative composite material D1#, indicating that the oriented chaining of nanofillers promotes the formation of thermal conductive paths. The higher the electric field intensity, the higher the chaining degree and the greater the thermal conductivity coefficient. Therefore, the AC electric field orientation of dielectrophoresis is more conducive to the improvement of thermal conductivity at temperature points above 100°C. The reason is that when the temperature rises, the thermal expansion effect of epoxy resin intensifies, thereby generating greater thermal stress and causing the stacking of h-BN to be tighter, which will inhibit the interfacial thermal resistance between h-BN and increase the thermal conductivity. The chaining of nanofillers in the thermal conductive direction will further enhance the occurrence of the above situation, so it can explain the thermal conductivity enhancement phenomenon of the oriented composite material induced by the electric field at high temperature points in the present invention.
[0095] Example 4
[0096] In this embodiment, based on the composite material 3# of embodiment 3, composite materials 4# and 5# are prepared by changing the electric field frequency, wherein the electric field frequency of composite material 4# is 8 kHz, the electric field frequency of composite material 5# is 9 kHz, and the rest are the same as composite material 3#.
[0097] Test Example 4
[0098] The thermal conductivity of composite materials 4#-5# prepared in Example 4 was tested by the same method as in Test Example 3, and composite material 3#, pure epoxy resin EP and comparative composite material D1# were used for comparison. The results are shown in Figure 6 .
[0099] Figure 6 (a) is the curve of the thermal conductivity of the composite material obtained under different electric field frequencies with temperature. It can be seen that the thermal conductivity performance of the composite materials obtained under different electric field frequencies is quite different. Except for the partial crossover between the comparative composite material D1# and the composite materials 3#-5#, the other composite materials 3#-5# are quite distinct. With the increase of frequency, the thermal conductivity of the prepared composite materials is improved as a whole. When the temperature reaches 100℃ and above, the thermal conductivity of the composite materials 3#-5# exceeds that of the pure epoxy resin EP and the comparative composite material D1#.
[0100] Figure 6 (b) is the growth rate of thermal conductivity of each material at 100°C. The results show that the higher the electric field frequency, the higher the growth rate of thermal conductivity of the composite material, and it reaches the maximum when the electric field frequency is 10kHz. Therefore, it can be seen that
[0101] The higher the frequency of the electric field, the better the chain formation effect of the nanofiller, thereby promoting the construction of thermal conductive channels and improving the thermal conductivity of the composite material.
[0102] According to the results of test examples 3 and 4, the greater the electric field strength and the higher the frequency, the less time the nanoparticles take to rotate and translate. The greater the electric field strength and the higher the electric field frequency, the higher the degree of chain formation of the nanoparticles. Under different field strengths, as the degree of chain formation of the particles increases, the conductivity and dielectric loss of the mixed system show a downward trend. The lower the electric field frequency, the greater the dielectric loss of the mixed system. Appropriate curing temperature and curing time are conducive to the directional chain formation of nanoparticles after applying an electric field. The combination of an electric field strength of 100-300V / mm and an electric field frequency of 8-10kHz can obtain the best filler-oriented composite material. Among them, the composite material with the best thermal conductivity under the conditions of 300V / mm and 10kHz can achieve a thermal conductivity growth rate of 78% at a temperature point of 100°C.
[0103] The above description is only an embodiment of the present invention. The protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent substitution, improvement, etc. made within the technical ideas and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a dry-type casing composite material based on dielectrophoresis control, characterized in that: The steps include: (1) After heating the epoxy resin, adding the modified CNC suspension to mix, and then adding the modified h-BN to mix to obtain a mixed solution, wherein the amount of the modified CNC added is 0.1% by weight of the epoxy resin, and the amount of the modified h-BN added is 1% by weight of the epoxy resin; (2) adding a curing agent and an accelerator to the mixed liquid, stirring evenly and extracting bubbles, placing the mixed liquid in a mold with electrodes, and pre-curing at 70-80° C. to obtain a pre-cured material; (3) After cooling the pre-cured material to 40-45° C., an AC electric field is applied and maintained for 30-35 min. The temperature is then raised to 60-65° C. and maintained for 9-11 min. After removing the AC electric field, the pre-cured material is heated and cured to obtain a composite material.
2. The preparation method according to claim 1, characterized in that: In step (3), the temperature for curing after removing the AC electric field is 70-90° C. and the time is 8-12 hours.
3. The preparation method according to claim 1, characterized in that: The electric field strength of the AC electric field in step (3) is 100-300 V / mm.
4. The preparation method according to claim 1, characterized in that: The electric field frequency of the AC electric field in step (3) is 8-10kHz.
5. The preparation method according to claim 1, characterized in that: The modified h-BN modification method comprises: adding h-BN to a solution of a silane coupling agent, adjusting the pH to 4-5, heating to 80-90° C. for 6-8 hours after ultrasonic treatment, cooling, rinsing and drying to obtain the modified h-BN; The amount of the silane coupling agent used accounts for 1.5-2.0% of the total weight of h-BN.
6. The preparation method according to claim 1, characterized in that: The modified CNC modification method comprises: placing CNC in water to obtain a CNC suspension, wherein the weight of CNC accounts for 1.5-2.0% of the weight of water, heating to 30-35° C., then adjusting the pH to 0.9-1.1 with nitric acid to obtain a pre-modified liquid, then adding ammonium cerium nitrate and stirring evenly, and finally adding methyl acrylate to carry out a graft polymerization reaction, and separating to obtain the modified CNC after the reaction is completed.
7. The preparation method according to claim 6, characterized in that: In 1L of pre-modified liquid, the amount of cerium ammonium nitrate added is 4.9-5.1mmol; the weight ratio of methyl acrylate to CNC is 3-4:
1.
8. The preparation method according to claim 1, characterized in that: The added amount of the curing agent accounts for 80-90% of the weight of the epoxy resin; the added amount of the accelerator accounts for 1-2% of the weight of the epoxy resin.
9. The dry-type casing composite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the dry bushing composite material prepared by the preparation method according to any one of claims 1 to 8 in high voltage insulation devices.