BNNTs (at) MXene / ANF heat conduction composite material and preparation method thereof

By growing boron nitride nanotubes on the MXene surface and forming a thermal conductivity network, the problem of interface thermal resistance in polymer-based composites is solved, and the thermal conductivity of composites is improved.

CN118879069AActive Publication Date: 2024-11-01ANHUI UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411121533.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-01
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

In existing polymer-based composite materials, there is an interface thermal resistance between the polymer and the filler, which makes its thermal conductivity unable to be improved to an ideal level.

Method used

By growing boron nitride nanotubes (BNNTs) on the surface of MXene and connecting them through carbon-nitrogen bonds, a thermal conductivity network is formed, the interface thermal resistance between the fillers is reduced, and a thermal conductivity path is formed through vacuum-assisted suction filtration to improve the thermal conductivity of the composite material.

Benefits of technology

It effectively reduces the interface thermal resistance between the fillers, enhances the thermal conductivity of the composite material, forms a thermal conductivity network, and improves thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879069A_ABST
    Figure CN118879069A_ABST
Patent Text Reader

Abstract

The invention discloses a BNNTs (at) MXene / ANF heat conduction composite material and a preparation method thereof.The preparation method comprises the steps that firstly, single-layer MXene is treated in a mixed solution of a nitrogen source and a boron source, so that the surface of MXene is nitrided, and nitrogen ions and boron ions are loaded; then, carrying out high-temperature pyrolysis on the treated MXene to enable boron nitride nanotubes to grow on the surface of the MXene in situ, so as to obtain a BNNTs (at) MXene filler; and finally, compounding the BNNTs (at) MXene filler with the aramid fiber ANF by adopting a vacuum-assisted suction filtration mode, so as to obtain the BNNTs (at) MXene / ANF composite material. The method provided by the invention can effectively reduce the contact thermal resistance between the fillers and construct a heat-conducting passage on a horizontal plane, so that the heat-conducting property of the composite material is obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of MXene and ANF composite materials, and in particular to a BNNTs@MXene / ANF thermal conductive composite material and a preparation method thereof. Background Art

[0002] As electronic devices develop rapidly towards miniaturization and high frequency, the high integration of electronic devices causes electronic components to generate a lot of heat during operation, resulting in continuous heat accumulation in electronic devices and serious heating. Therefore, it is necessary to use materials with thermal conductivity to dissipate heat. Existing materials with thermal conductivity are mainly polymer-based composite materials. Pure polymer-based materials are difficult to use directly due to their low thermal conductivity. Therefore, they need to be doped with some inorganic fillers such as high thermal conductivity metals, carbon-based materials or ceramics to improve thermal conductivity. However, in existing polymer-based composite materials, the polymer and the filler are simply compounded. For example, the document "Enhanced Electromagnetic Shielding and Thermal Management Properties in MXene / Aramid Nanofiber Films Fabricated by Intermittent Filtration" discloses a layered MXene / aramid nanofiber (ANF) composite film obtained by filtration, which is a simple compound of the filler and the substrate (Liu, Chenxu, et al. "Enhanced Electromagnetic Shielding and Thermal Management Properties in MXene / Aramid Nanofiber Films Fabricated by Intermittent Filtration." ACS Applied Materials & Interfaces 15.3 (2023): 4516-4526.). However, the polymer-based composite material obtained by simple compounding does not construct an effective filler heat conduction path, there is an interface thermal resistance between the substrate and the filler, and there is also an interface thermal resistance between the fillers, so the thermal conductivity of the material cannot be increased to an ideal level. Summary of the invention

[0003] Based on the above problems existing in the prior art, the present invention provides a BNNTs@MXene / ANF thermally conductive composite material and a preparation method thereof, aiming to connect the MXene sheets through BNNTs grown on the MXene surface, thereby reducing the contact thermal resistance between fillers and improving the thermal conductivity of the composite material.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A preparation method of a BNNTs@MXene / ANF thermal conductive composite material, characterized in that: first, a single layer of MXene is treated in a mixture of a nitrogen source and a boron source to nitride the MXene surface and load nitrogen ions and boron ions; then the treated MXene is pyrolyzed at high temperature to in-situ grow boron nitride nanotubes (BNNTs) on the MXene surface, and the MXene and the boron nitride nanotubes are connected by carbon-nitrogen bonds to obtain BNNTs@MXene filler; finally, the BNNTs@MXene filler is compounded with aramid fiber ANF by vacuum-assisted filtration to obtain a BNNTs@MXene / ANF composite material. Specifically, the steps are as follows:

[0006] Step 1: Preparation of nitrided MXene

[0007] 40-60 mg of MXene and 30-40 mL of deionized water were ultrasonically mixed in an ice bath to obtain a MXene suspension;

[0008] Dissolve 30-50 g CH4N2O in 100 mL deionized water, add 0.8-1.5 g H3BO3 and stir at room temperature for 10-14 h to obtain a precursor solution;

[0009] The MXene suspension is added to the precursor solution, and stirred at room temperature for 4 to 6 hours to nitride the surface of the MXene and load nitrogen ions and boron ions, and the precipitate is taken by centrifugation and vacuum dried to obtain the nitrided MXene;

[0010] Step 2: Preparation of BNNTs@MXene filler

[0011] The nitrided MXene is subjected to high temperature pyrolysis treatment at 800 to 1000° C. in a nitrogen atmosphere for 8 to 10 hours to obtain a BNNTs@MXene filler;

[0012] Step 3: Preparation of BNNTs@MXene / ANF composites

[0013] Add 0.75-1.0 g of chopped aramid fiber ANF and 1-1.5 g of KOH into 60-80 mL of DMSO and stir evenly to obtain an ANF dispersion;

[0014] BNNTs@MXene filler was added to the ANF dispersion, stirred evenly, then washed with water to remove DMSO, and then dispersed in 250 mL of deionized water by shearing to obtain a mixed dispersion. The BNNTs@MXene / ANF composite material was obtained by vacuum-assisted filtration and hot pressing.

[0015] As a further preferred technical solution of the present invention, in step 2, the heating rate during the high-temperature pyrolysis treatment is 2°C / min.

[0016] As a further preferred technical solution of the present invention, in step 3, the filter paper for vacuum-assisted filtration is polytetrafluoroethylene hydrophobic filter paper with a pore size of 0.22 μm.

[0017] As a further preferred technical solution of the present invention, in step 3, the pressure of the hot pressing treatment is 5-10 MPa, the temperature is 100-140° C., and the treatment time is 5-10 min.

[0018] As a further preferred technical solution of the present invention, in step 3, the amount of BNNTs@MXene filler added accounts for 10% to 40% of the total mass of the BNNTs@MXene / ANF composite material.

[0019] As a further preferred technical solution of the present invention, in step 3, the shearing rotation speed is 10000-14000 rpm.

[0020] As a further preferred technical solution of the present invention, the monolayer MXene is prepared by in-situ generation of HF by HCl and LiF to etch the MAX phase and then ultrasonically exfoliate the MAX phase. The specific steps are as follows:

[0021] 1-2 g LiF and 15-25 mL 9 M HCl solution were mixed and stirred in an ice bath, and then 1 g MAX phase powder was added and reacted at 30-40 °C for 22-26 h. The resulting slurry was repeatedly washed with deionized water and centrifuged until pH ≥ 6 to obtain Ti3C2T x precipitate; the obtained precipitate was redispersed in deionized water, ultrasonicated in an ice bath for 1 to 3 hours under oxygen isolation conditions, the supernatant was collected by centrifugation, and freeze-dried to obtain a single-layer MXene.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0023] The present invention uses MXene with in-situ growth of BNNT on the surface as filler, and BNNT as a one-dimensional material connecting two MXene two-dimensional sheet materials to construct a thermal conductive network, which can effectively reduce the interfacial thermal resistance between fillers and fillers, and further construct a thermal conductive path on the horizontal plane through the oriented structure formed by vacuum-assisted filtration, further enhancing the thermal conductivity of the composite material. At the same time, MXene and BNNT are connected by carbon-nitrogen bonds, and the interaction between them is strong. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0025] Figure 1 This is a SEM image of the single-layer MXene obtained in Example 1 of the present invention;

[0026] Figure 2 This is a SEM image of BNNTs@MXene obtained in Example 1 of the present invention;

[0027] Figure 3 TEM image of BNNTs@MXene obtained in Example 1 of the present invention;

[0028] Figure 4 This is a FI-IR comparison chart of the single-layer MXene and BNNTs@MXene obtained in Example 1 of the present invention;

[0029] Figure 5 This is the XRD pattern of BNNTs@MXene obtained in Example 1 of the present invention;

[0030] Figure 6 This is the XPS total spectrum of the single-layer MXene and BNNTs@MXene obtained in Example 1 of the present invention;

[0031] Figure 7 The thermal conductivity of the samples obtained in Examples 1, 2, 3, 4 and Comparative Example 1 of the present invention is compared. DETAILED DESCRIPTION

[0032] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0033] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0034] Example 1

[0035] In this example, the BNNTs@MXene / ANF composite material was prepared according to the following steps.

[0036] Step 1: Preparation of single-layer MXene

[0037] 1.5 g LiF was added to a polytetrafluoroethylene bottle containing 20 mL 9 M HCl solution and stirred for 15 min in an ice bath to obtain an etchant. Then 1 g MAX phase powder (Ti3AlC2) was slowly added to the etchant in batches and reacted at 35 °C for 24 h. The resulting slurry was repeatedly washed and centrifuged with deionized water at 3500 rpm until pH ≥ 6 to obtain Ti3C2T xprecipitate; the obtained precipitate was redispersed in deionized water, the dispersed liquid was poured into a gas collecting bottle, argon was passed for 5 minutes to isolate oxygen, and then ice bath ultrasonic was performed for 2 hours, and the supernatant was collected by centrifugation at 8000 rpm for 10 minutes, and freeze-dried for 24 hours to obtain a single-layer MXene powder.

[0038] Step 2: Preparation of Nitrided MXene

[0039] Add 50 mg of MXene and 35 mL of deionized water to a 100 mL beaker, place the beaker in an ultrasonic machine, and ultrasonicate for 30 min in an ice bath to obtain a MXene suspension. Dissolve 40 g of CH4N2O in 100 mL of deionized water using magnetic stirring, add 1 g of H3BO3 after complete dissolution, and stir for 12 h to obtain a precursor solution.

[0040] The prepared MXene suspension was added to the precursor solution, stirred for 5 hours, and then centrifuged at 10,000 rpm for 10 minutes. The supernatant was removed, and the lower layer of sediment was taken out and dried at 70°C in a vacuum drying oven for 24 hours to obtain nitrided MXene.

[0041] Step 3: Preparation of BNNTs@MXene filler

[0042] The nitrided MXene was ground into powder in a mortar and pyrolyzed at 900 °C in a nitrogen atmosphere for 8 h to obtain BNNTs@MXene filler.

[0043] Step 4: Preparation of BNNTs@MXene / ANF composites

[0044] Cut Kevlar 49 (0.75 g) and KOH (1.125 g) were added to 75 mL of DMSO and stirred at 800 rpm for 4 days to prepare a uniform dark red ANF dispersion (concentration of 10 mg / mL).

[0045] 5.5 mg of BNNTs@MXene filler was added to 5 mL of ANF dispersion, stirred evenly, then washed with water to remove DMSO, and then dispersed in 250 mL of deionized water by shearing (vigorous stirring at 12000 rpm for 1 min) to obtain a uniform mixed dispersion. A composite material with a filler content of 10 wt% was obtained by vacuum assisted filtration (filter paper selected polytetrafluoroethylene hydrophobic filter paper with a pore size of 0.22 μm) and hot pressing (hot pressing pressure of 5 MPa, temperature of 120 ° C, and processing time of 5 min), which was recorded as BNNTs@MXene-10 / ANF.

[0046] Example 2

[0047] In this example, a BNNTs@MXene / ANF composite material was prepared in the same manner as in Example 1, except that the amount of BNNTs@MXene filler added in step 4 was 12.5 mg, and a composite material having a filler content of 20 wt% was obtained, which was recorded as BNNTs@MXene-20 / ANF.

[0048] Example 3

[0049] In this example, a BNNTs@MXene / ANF composite material was prepared in the same manner as in Example 1, except that the amount of BNNTs@MXene filler added in step 4 was 21.43 mg, and a composite material having a filler content of 30 wt% was obtained, which was recorded as BNNTs@MXene-30 / ANF.

[0050] Example 4

[0051] In this example, a BNNTs@MXene / ANF composite material was prepared in the same manner as in Example 1, with the only difference being that in step 4, the amount of BNNTs@MXene filler added was 33.33 mg, and a composite material having a filler content of 40 wt% was obtained, which was recorded as BNNTs@MXene-40 / ANF.

[0052] Comparative Example 1

[0053] 5 mL of the 10 mg / mL ANF dispersion prepared in Example 1 was weighed into a beaker, washed with water to remove DMSO, and then dispersed in 250 mL of deionized water by shearing (vigorously stirred at a speed of 12000 rpm for 1 min) to obtain a uniform dispersion. A pure ANF membrane was obtained by vacuum assisted filtration (filter paper selected polytetrafluoroethylene hydrophobic filter paper with a pore size of 0.22 μm) and hot pressing (hot pressing pressure of 5 MPa, temperature of 120°C, and processing time of 5 min).

[0054] Figure 1 This is the SEM image of the single-layer MXene prepared in Example 1. Figure 2 This is the SEM image of the BNNTs@MXene filler obtained in Example 1. It can be seen that the BNNTs are successfully grown in situ on the MXene surface through high-temperature heat treatment. The MXene layers are connected by BNNTs to form a heat conduction path, which can effectively reduce the contact thermal resistance between fillers and improve the thermal conductivity of the composite material.

[0055] Figure 3 This is the TEM image of the BNNTs@MXene filler obtained in Example 1. An obvious cavity structure can be seen in the image, indicating that BNNTs have successfully grown on the surface of the MXene sheet.

[0056] Figure 4This is the FI-IR comparison diagram of the single-layer MXene obtained in Example 1 and BNNTs@MXene. Compared with pure MXene, BNNTs@MXene has a -1 Bending vibration of the BN bond appears at 1377 cm -1 The stretching vibration of the BN bond appears at , indicating the formation of BNNT.

[0057] Figure 5 This is the XRD pattern of BNNTs@MXene obtained in Example 1. By comparing with pure MXene and pure BNNT, it can be seen that there is an obvious peak shift, indicating that BNNTs have successfully grown on the MXene surface.

[0058] Figure 6 This is the overall XPS spectrum of the single-layer MXene and BNNTs@MXene obtained in Example 1. Compared with MXene, the atomic ratio of B and N in BNNTs@MXene is larger, indicating the successful introduction of BNNT.

[0059] Figure 7 is the thermal conductivity of the samples obtained in Examples 1, 2, 3, 4 and Comparative Example 1. Compared with the pure ANF film in Comparative Example 1, the thermal conductivity of the samples obtained in Examples 1 to 4 increases first and then decreases with the increase of filler content. This is mainly because the in-situ growth of BNNT on the MXene surface can effectively reduce the contact thermal resistance between MXene sheets, thereby improving the thermal conductivity. However, when the filler concentration is too high, agglomeration will occur, affecting the thermal conductivity of the composite film.

[0060] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a BNNTs@MXene / ANF thermally conductive composite material, Features: Firstly, a single layer of MXene is treated in a mixture of nitrogen source and boron source to nitridate the surface of MXene and load nitrogen ions and boron ions. Then, the treated MXene is pyrolyzed at high temperature to in situ grow boron nitride nanotubes on the surface of MXene, and the MXene and the boron nitride nanotubes are connected by carbon-nitrogen bonds to obtain BNNTs@MXene filler. Finally, the BNNTs@MXene filler is compounded with aramid fiber ANF by vacuum-assisted filtration to obtain BNNTs@MXene / ANF composite material.

2. The preparation method according to claim 1, It is characterized in that The steps include: Step 1: Preparation of nitrided MXene 40-60 mg of MXene and 30-40 mL of deionized water were ultrasonically mixed in an ice bath to obtain a MXene suspension; 30-50 g CH 4 N 2 O was dissolved in 100 mL of deionized water, and 0.8-1.5 g H 3 BO 3 and stirring at room temperature for 10 to 14 hours to obtain a precursor solution; The MXene suspension is added to the precursor solution, and stirred at room temperature for 4 to 6 hours to nitride the surface of the MXene and load nitrogen ions and boron ions, and the precipitate is taken by centrifugation and vacuum dried to obtain the nitrided MXene; Step 2: Preparation of BNNTs@MXene filler The nitrided MXene is subjected to high temperature pyrolysis treatment at 800 to 1000° C. in a nitrogen atmosphere for 8 to 10 hours to obtain a BNNTs@MXene filler; Step 3: Preparation of BNNTs@MXene / ANF composites Add 0.75-1.0 g of chopped aramid fiber ANF and 1-1.5 g of KOH into 60-80 mL of DMSO and stir evenly to obtain an ANF dispersion; BNNTs@MXene filler was added to the ANF dispersion, stirred evenly, then washed with water to remove DMSO, and then dispersed in 250 mL of deionized water by shearing to obtain a mixed dispersion. The BNNTs@MXene / ANF composite material was obtained by vacuum-assisted filtration and hot pressing.

3. The preparation method according to claim 2, Features: In step 3, the filter paper for vacuum-assisted filtration is polytetrafluoroethylene hydrophobic filter paper with a pore size of 0.22 μm.

4. The preparation method according to claim 2, Features: In step 3, the pressure of the hot pressing treatment is 5-10 MPa, the temperature is 100-140° C., and the treatment time is 5-10 min.

5. The preparation method according to claim 2, Features: In step 3, the amount of BNNTs@MXene filler added accounts for 10% to 40% of the total mass of the BNNTs@MXene / ANF composite material.

6. The preparation method according to claim 1 or 2, Features: The single-layer MXene is prepared by in-situ generation of HF by HCl and LiF to etch the MAX phase and then ultrasonically exfoliate it.

7. The preparation method according to claim 6, It is characterized in that The single-layer MXene is prepared according to the following steps: 1-2 g LiF and 15-25 mL 9 M HCl solution were mixed and stirred in an ice bath, and then 1 g MAX phase powder was added and reacted at 30-40 ° C for 22-26 h. The resulting slurry was repeatedly washed with deionized water and centrifuged until the pH was ≥ 6 to obtain Ti 3 C 2 T x precipitate; the obtained precipitate was redispersed in deionized water, ultrasonicated in an ice bath for 1 to 3 hours under oxygen isolation conditions, the supernatant was collected by centrifugation, and freeze-dried to obtain a single-layer MXene.

8. A BNNTs@MXene / ANF thermally conductive composite material prepared by the preparation method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Functionalized boron nitride nanosheet / MXene / polybenzimidazole high-thermal-conductivity composite film and preparation method thereof

    CN112552681A

  • Flexible aramid nanofiber / MXene high-thermal-conductivity flame-retardant composite film as well as preparation method and application of flexible aramid nanofiber / MXene high-thermal-conductivity flame-retardant composite film

    CN115584038A

  • In-situ growth carbon nanotube composite heteroatom doped porous MXene material and preparation method thereof

    CN115939343A

  • Preparation method and application of Ti3C2Tx-Mxene poly-dopamine-nano-silver composite material

    CN117304575A

  • Multifunctional layered composite film of MXene (at) h-BN as well as preparation method and application of multifunctional layered composite film

    CN117797880A