Self-layering coating as well as preparation method and application thereof

By combining modified silicone resin and polyurea resin, a self-layer coating is formed, which solves the problems of poor weather resistance and mechanical properties of existing coatings, and achieves efficient layered structure and environmental protection performance, satisfying the high-performance coatings. need.

CN118879173AActive Publication Date: 2024-11-01GUANGDONG ENERGY GROUP SCIENCE & TECHNOLOGY RESEARCH INSTITUTE CO LTD

Patent Information

Application Number
CN202410956090.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing self-layer coatings have poor weather resistance and mechanical properties after application, making it difficult to form a stable layered structure, and have a pollution impact on the environment and affect practical applications.

Method used

Modified silicone resin and polyurea resin are combined, and the silicone resin is modified by an alkyl silane coupling agent to reduce its surface energy and separate it from the polyurea resin to form a self-layered coating, and the modified silicone resin is moved. Provides hydrophobic and stain-resistant to the surface, and polyurea resin migrates to the bottom surface to increase adhesion and weather resistance.

Benefits of technology

It quickly forms a good layered structure after coating, has good waterproof, anti-fouling and weather resistance, improves the coating efficiency and product life, and meets the requirements of high environmental protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879173A_ABST
    Figure CN118879173A_ABST
Patent Text Reader

Abstract

The invention provides a self-stratifying coating as well as a preparation method and application thereof. The self-stratifying coating is prepared from the following raw materials: modified organic silicon resin, polyurea resin, a curing agent, an auxiliary agent and a solvent, the preparation raw materials of the modified organic silicon resin comprise an alkyl silane coupling agent and organic silicon resin. According to the self-stratification coating provided by the invention, in the film forming process of the self-stratification coating, the modified organic silicon resin can be migrated to the surface of the formed self-stratification coating so as to provide good hydrophobic antifouling property, and the polyurea resin is migrated downwards to the bottom surface of the formed self-stratification coating, so that the adhesive force between the self-stratification coating and a base material and the overall weather resistance are improved; and a good self-layering structure is formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a self-stratifying coating and a preparation method and application thereof. Background Art

[0002] Self-stratifying coatings can form complex multi-layer or gradient coating structures in one step by simply applying the coating to the substrate, achieving the effect of integrating the bottom and the surface, and can have the excellent performance of both topcoat and primer. Existing self-stratifying coatings often achieve the self-stratification effect through the surface energy difference of the resin system in the coating. After the coating is applied to the substrate, the solvent in the coating evaporates, and the resin with low surface energy migrates to the surface layer to provide aesthetics, durability, scratch resistance and waterproof and antifouling properties, and the resin with high surface energy migrates to the substrate to provide weather resistance and improve the adhesion between the coating and the substrate.

[0003] CN105482027A discloses an acrylic modified polysiloxane resin and its application in a self-stratifying coating, wherein the self-stratifying coating comprises a component A and a component B, wherein the component A comprises the following components by weight percentage: 15%-70% acrylic modified polysiloxane resin, 5%-40% pigment and filler, 0.5%-2% auxiliary agent, and 10%-45% solvent; the component B is a curing agent, including a coupling agent or aminosilane containing an isocyanate group. The acrylic modified polysiloxane resin provided by the technical solution has two groups available for crosslinking, so that the self-stratifying coating can be cured by selecting different curing agents according to performance requirements, and the self-stratifying coating has a fast surface drying speed, low surface energy and good hydrophobic antifouling performance, but the acrylic modified polysiloxane has poor weather resistance and mechanical properties, which will lead to reduced weather resistance and poor mechanical properties of the self-stratifying coating, making it difficult to be widely used in coatings.

[0004] CN106867359A discloses a fluorine-containing block acrylate-epoxy resin weather-resistant anticorrosive self-stratifying coating and a preparation method thereof, wherein the fluorine-containing block acrylate-epoxy resin weather-resistant anticorrosive self-stratifying coating comprises component A and component B, wherein component A comprises 100 parts of epoxy resin, 10-30 parts of fluorine-containing block acrylate copolymer, 20-30 parts of pigments and fillers, 1-2 parts of dispersants, and 60-80 parts of organic solvent I, and component B comprises 30-80 parts of amide curing agents and 20-60 parts of organic solvent II. This technical solution mainly utilizes fluorine groups to make acrylates with low surface energy migrate to the surface, and epoxy resins migrate to the bottom surface to achieve self-stratification effect. The coating has a rapid stratification or gradient structure, improves coating efficiency, and saves costs. However, due to the fluorine groups, it will have a certain impact on the environment and is difficult to be applied to coatings with high environmental performance requirements today.

[0005] Most of the self-stratifying coating systems in the prior art have problems such as poor weather resistance, poor mechanical properties, environmental pollution or unstable stratified structure, which leads to a large deviation between the self-stratifying coating and the ideal stratification effect after being applied to the substrate, requiring continuous adjustment and trial, which seriously affects the practical application.

[0006] Therefore, there is an urgent need to develop a self-stratifying coating which has good stratification effect after coating and has good waterproof, antifouling and weather resistance. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide a self-stratifying coating and a preparation method and application thereof. The self-stratifying coating can quickly form a good stratified structure after coating and has good waterproof, antifouling and weather resistance.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a self-stratifying coating, wherein the raw materials for preparing the self-stratifying coating include a modified silicone resin, a polyurea resin, a curing agent, an auxiliary agent and a solvent;

[0010] The raw materials for preparing the modified silicone resin include an alkyl silane coupling agent and silicone resin.

[0011] The present invention utilizes the ingenious functional group design between the modified silicone resin, the polyurea resin and the curing agent to enable the self-stratifying coating to form a self-stratifying morphology structure and function. The silicone resin is modified by an alkyl silane coupling agent, and long alkyl chains are grafted on both ends of the silicone resin, which can reduce the surface energy of the silicone resin, increase the hydrophobic antifouling performance, and also enable it to separate from the polyurea resin faster and migrate to the surface layer. In the film-forming process of the self-stratifying coating, as the solvent evaporates and the components are cross-linked and cured, the modified silicone resin migrates to the surface of the formed self-stratifying coating to provide good hydrophobic antifouling properties, and the polyurea resin migrates downward to the bottom surface of the formed self-stratifying coating to increase its adhesion to the substrate and the overall weather resistance, forming a good self-stratifying structure.

[0012] Preferably, the alkylsilane coupling agent includes hexadecyltrimethoxysilane (HDTMS).

[0013] Preferably, the silicone resin comprises hydroxy-terminated polymethylsiloxane.

[0014] Preferably, the hydroxyl-terminated polymethylsiloxane has a structure as shown in the following formula I.

[0015]

[0016] In formula I, n=10-15, for example, 10, 11, 12, 13, 14 or 15.

[0017] Preferably, the raw materials for preparing the modified silicone resin further include water, ethanol, acid and catalyst A.

[0018] Preferably, the acid comprises glacial acetic acid.

[0019] Preferably, the catalyst A comprises dibutyltin diacetate.

[0020] Preferably, the modified silicone resin is prepared by the following method.

[0021] (1) An alkylsilane coupling agent, water and ethanol are mixed, an acid is added to adjust the pH to 3 to 4 (e.g., 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9 or 4, etc.), and hydrolyzed to obtain a hydrolyzed alkylsilane coupling agent solution.

[0022] (2) mixing the organic silicone resin, the hydrolyzed alkylsilane coupling agent solution obtained in step (1) and the catalyst A, and reacting them to obtain the modified organic silicone resin.

[0023] Preferably, the modified silicone resin is prepared by the following method.

[0024] (1) Hexadecyltrimethoxysilane, water and ethanol are mixed, acid is added to adjust the pH to 3-4, and hydrolysis is performed to obtain a hydrolyzed hexadecyltrimethoxysilane solution. The reaction formula involved is as follows.

[0025]

[0026] (2) Mixing the hydroxyl-terminated polymethylsiloxane, the hydrolyzed hexadecyltrimethoxysilane solution obtained in step (1) and the catalyst A, and reacting them to obtain a modified silicone resin. The reaction formula involved is as follows.

[0027]

[0028] Among them, n=10-15.

[0029] Preferably, the weight proportion of the alkylsilane coupling agent in step (1) is 0.2 to 0.5 parts, for example, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts or 0.5 parts.

[0030] Preferably, the weight proportion of water in step (1) is 0.6 to 1.5 parts, for example, 0.6 parts, 0.8 parts, 1.0 parts, 1.2 parts, 1.4 parts or 1.5 parts.

[0031] Preferably, the weight proportion of the ethanol in step (1) is 1.2 to 3 parts, for example, 1.4 parts, 1.6 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.4 parts, 2.6 parts or 2.8 parts, etc.

[0032] Preferably, the weight proportion of the organic silicone resin in step (2) is 2 to 10 parts (eg, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts or 9 parts, etc.).

[0033] Preferably, the weight portion of the catalyst A in step (2) is 0.1 to 0.2 parts (e.g., 0.11 parts, 0.12 parts, 0.13 parts, 0.14 parts, 0.15 parts, 0.16 parts, 0.17 parts, 0.18 parts or 0.19 parts, etc.).

[0034] Preferably, the hydrolysis temperature in step (1) is 20-30°C (e.g., 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C or 29°C, etc.), and the time is 0.25-1h (e.g., 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h or 0.9h, etc.).

[0035] Preferably, the reaction temperature in step (2) is 20-30°C (e.g., 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, etc.), and the reaction time is 0.25-1h (e.g., 0.25h, 0.3h, 0.4h, 0.5h, 0.6h, 0.7h, 0.8h, 0.9h or 1h, etc.).

[0036] Preferably, the polyurea resin comprises polyaspartic acid polyurea resin.

[0037] Preferably, the curing agent comprises a multifunctional aliphatic isocyanate.

[0038] Preferably, the auxiliary agent includes catalyst B and / or a defoaming agent.

[0039] Preferably, the catalyst B comprises dibutyltin dilaurate and / or dibutyltin diacetate, more preferably dibutyltin diacetate.

[0040] Preferably, the defoamer comprises defoamer BYK-110.

[0041] Preferably, the raw materials for preparing the self-stratifying coating include the following components in parts by weight: 5 to 16 parts (e.g., 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, etc.) of modified silicone resin, 10 to 18 parts (e.g., 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts or 17 parts, etc.) of polyurea resin, 10 to 15 parts (e.g., 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts or 17 parts, etc.) of curing agent. For example, 11 parts, 11.5 parts, 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts or 15 parts, etc.), 0.2-0.6 parts of auxiliary agent (0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts or 0.55 parts, etc.) and 10-60 parts of solvent (for example, 10 parts, 20 parts, 30 parts, 40 parts, 50 parts or 60 parts, etc.).

[0042] In the present invention, the solvent can be used to adjust the delamination rate of the modified silicone resin and the polyurea resin in the self-stratifying coating. The weight proportion of the solvent is preferably 10 to 60 parts. If the weight proportion of the solvent is too large, the curing speed of the coating slows down, affecting the actual use of the coating; if the weight proportion of the solvent is too small, the curing speed is too fast, which may easily lead to the situation that the delamination effect cannot be achieved, the delamination fails, or the delamination effect is unstable.

[0043] Preferably, the weight proportion of the solvent in the raw materials for preparing the self-stratifying coating is 15 to 50 parts, for example, 15 parts, 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts or 50 parts.

[0044] Preferably, the solvent comprises xylene, methyl isobutyl ketone and butyl acetate.

[0045] Preferably, the solvent comprises the following components in parts by weight: 1.1 to 15 parts (e.g., 3, 5, 7, 9, 11, 13 or 15 parts, etc.) of xylene, 1.1 to 15 parts (e.g., 3, 5, 7, 9, 11, 13 or 15 parts, etc.) of methyl isobutyl ketone and 3 to 5 parts (e.g., 3, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6 or 4.8 parts, etc.) of butyl acetate.

[0046] In the present invention, the xylene is a non-polar solvent, and the weight proportion of xylene is preferably 1.1 to 15 parts. If the weight proportion of xylene is too high, it may easily lead to the situation that the stratification effect cannot be achieved, the stratification effect fails, or the stratification effect is unstable.

[0047] In a second aspect, the present invention provides a method for preparing the self-stratifying coating as described in the first aspect, the preparation method comprising the following steps: mixing a modified silicone resin, a polyurea resin, a curing agent, an auxiliary agent and a solvent.

[0048] Preferably, the preparation method specifically comprises the following steps:

[0049] (I) Xylene and methyl isobutyl ketone are mixed to obtain a mixed solution.

[0050] (II) The modified silicone resin is mixed with a part of the mixed solvent prepared in step (I) to obtain a mixture A.

[0051] (III) The polyurea resin is mixed with another part of the solvent obtained in step (I) to obtain a mixture B.

[0052] (IV) performing a first mixing of the mixture A obtained in step (II) and the mixture B obtained in step (III), adding a defoamer for a second mixing, adding a mixture of a curing agent and butyl acetate and a catalyst B for a third mixing, and obtaining the self-stratifying coating.

[0053] Step (II) and step (III) can be carried out in any order or simultaneously.

[0054] In a third aspect, a self-stratifying coating is provided, wherein the self-stratifying coating is obtained by applying the self-stratifying coating described in the first aspect to a substrate surface and curing the coating.

[0055] In the present invention, the hydroxyl groups, amino groups and isocyanate groups in the self-stratifying coating are cross-linked and cured.

[0056] Preferably, the coating comprises brush coating or roller coating.

[0057] Preferably, the curing temperature is 20 to 50°C (eg, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C or 50°C), more preferably 20 to 40°C.

[0058] Preferably, the curing time is 8 to 24 hours, for example, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours.

[0059] In the present invention, the self-stratifying coating can be used for the protection of various types of ship hulls and supporting structures such as metal and composite materials. After the self-stratifying coating is applied, a stable self-stratifying effect can be formed, the hydrophobic and antifouling effect and weather resistance can be enhanced, the problems existing in the self-stratifying coating in the prior art can be compensated, the qualified rate of the coating product in one coating can be improved, and the production and processing costs can be reduced.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] In the self-stratifying coating of the present invention, during the film-forming process of the self-stratifying coating, the modified organic silicone resin can migrate to the surface of the self-stratifying coating formed to provide good hydrophobic antifouling properties, and the polyurea resin migrates downward to the bottom surface of the self-stratifying coating formed to increase the adhesion between the self-stratifying coating and the substrate and the overall weather resistance. The self-stratifying coating can form a good self-stratifying structure. The self-stratifying coating has a simple manufacturing process and is convenient to construct. After coating, a good stratified structure can be quickly formed. Two continuous coatings with different functions can be quickly and spontaneously formed in one application. The self-stratifying coating has good waterproof, antifouling and weather resistance. After being immersed in seawater for one month, the surface morphology has not changed significantly, and no discoloration, bubbling, shedding and the like are found. The adhesion of the self-stratifying coating formed by the self-stratifying coating is above 4MPa, and its surface energy is 20 to 30J·m -2 , improves coating efficiency, saves production costs, increases the service life of coatings, and can meet the demand for high-performance coatings. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 and Figure 2 SEM images of different positions of the cross section of the self-stratified coating provided in Example 1;

[0063] Figure 3 The SEM-EDS scanning image of Si element in the cross section of the self-stratified coating provided in Example 1;

[0064] Figure 4 A comparison of the surface morphologies of the self-stratifying coating provided in Example 1 before seawater immersion (left) and after seawater immersion for one month (right);

[0065] Figure 5 A surface energy comparison diagram of the self-stratifying coating provided in Example 1 and the coating provided in Comparative Example 1;

[0066] Figure 6 SEM image of the coating provided for Comparative Example 1. DETAILED DESCRIPTION

[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0068] The sources of some components in the examples and comparative examples are as follows.

[0069] Polyurea resin: polyaspartic acid polyurea resin, brand F155, manufacturer Shenzhen Feiyang Junyan New Materials Co., Ltd.;

[0070] Silicone resin: Hydroxy-terminated polymethylsiloxane, brand name JZH-203, manufactured by Jiangsu Sanmu Group Co., Ltd., with the following structure:

[0071] Where n = 11;

[0072] Curing agent: isocyanate curing agent GB605B-100, the manufacturer is Shenzhen Feiyang Junyan New Materials Co., Ltd.;

[0073] Defoaming agent: Defoaming agent BYK-100, manufactured by BYK Chemical of Germany.

[0074] Example 1

[0075] The present embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The raw materials for preparing the self-stratifying coating include the following components in parts by weight: 9.3 parts of modified silicone resin, 16 parts of polyurea resin, 10 parts of curing agent, 0.1 part of catalyst B (dibutyltin diacetate), 0.1 part of defoaming agent, 3 parts of butyl acetate, 6.65 parts of xylene and 6.65 parts of methyl isobutyl ketone.

[0076] Preparation of modified silicone resin:

[0077] (1) 0.5 parts by weight of hexadecyltrimethoxysilane, 1.5 parts by weight of deionized water, and 3 parts by weight of anhydrous ethanol were added to a beaker for dissolution and mixing, and glacial acetic acid was added to adjust the pH to 3, the weight portion of glacial acetic acid added was 0.2 parts, and magnetic stirring was performed at 25° C. for 0.5 h for hydrolysis to obtain a hydrolyzed alkylsilane coupling agent solution.

[0078] (2) 4 parts by weight of an organic silicone resin, the hydrolyzed alkylsilane coupling agent solution obtained in step (1) and 0.1 parts by weight of a catalyst A (dibutyltin diacetate) were mixed, and stirred at 25° C. and 500 r / min for 0.5 h to obtain a modified organic silicone resin.

[0079] The preparation method of the self-stratifying coating is as follows:

[0080] (I) mixing 6.65 parts by weight of xylene and 6.65 parts by weight of methyl isobutyl ketone to form a mixed solution;

[0081] (II) mixing the modified silicone resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture A;

[0082] (III) mixing 16 parts by weight of a polyurea resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture B;

[0083] (IV) Mixture A obtained in step (II) and mixture B obtained in step (III) are first mixed by stirring at 500 r / min for 30 minutes, 0.1 parts by weight of a defoamer is added and stirred at 500 r / min for 30 minutes for a second mixing, a mixture of 10 parts by weight of a curing agent and 3 parts by weight of butyl acetate is added, and 0.1 parts by weight of a catalyst B is added and stirred evenly for a third mixing to obtain the self-stratifying coating.

[0084] The preparation method of the self-stratifying coating is as follows:

[0085] The self-stratifying coating was coated on a glass substrate, dried and cured at 30° C. for 20 h to obtain the self-stratifying coating.

[0086] Example 2

[0087] The present embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The raw materials for preparing the self-stratifying coating include the following components in parts by weight: 9.25 parts of modified silicone resin, 17 parts of polyurea resin, 10 parts of curing agent, 0.5 parts of catalyst B (dibutyltin diacetate), 0.1 parts of defoaming agent, 5 parts of butyl acetate, 2.5 parts of xylene and 2.5 parts of methyl isobutyl ketone.

[0088] Preparation of modified silicone resin:

[0089] (1) 0.5 parts by weight of hexadecyltrimethoxysilane, 1.5 parts by weight of deionized water, and 3 parts by weight of anhydrous ethanol were added to a beaker for dissolution and mixing, and glacial acetic acid was added to adjust the pH to 4, the weight portion of glacial acetic acid added was 0.1 parts, and magnetic stirring was performed at 20° C. for 0.5 h for hydrolysis to obtain a hydrolyzed alkylsilane coupling agent solution.

[0090] (2) 4 parts by weight of an organic silicone resin, the hydrolyzed alkylsilane coupling agent solution obtained in step (1) and 0.15 parts by weight of a catalyst A (dibutyltin diacetate) were mixed, and stirred at 20° C. and 500 r / min for 0.5 h to obtain a modified organic silicone resin.

[0091] The preparation method of the self-stratifying coating is as follows:

[0092] (I) mixing 2.5 parts by weight of xylene and 2.5 parts by weight of methyl isobutyl ketone to form a mixed solution;

[0093] (II) mixing the modified silicone resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture A;

[0094] (III) mixing 17 parts by weight of a polyurea resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture B;

[0095] (IV) Mixture A obtained in step (II) and mixture B obtained in step (III) are first mixed by stirring at 500 r / min for 30 minutes, 0.1 parts by weight of a defoamer is added and stirred at 500 r / min for 30 minutes for a second mixing, a mixture of 10 parts by weight of a curing agent and 5 parts by weight of butyl acetate is added, and 0.5 parts by weight of a catalyst B is added and stirred evenly for a third mixing to obtain the self-stratifying coating.

[0096] The preparation method of the self-stratifying coating is as follows:

[0097] The self-stratifying coating was coated on a glass substrate, dried and cured at 40° C. for 8 hours to obtain the self-stratifying coating.

[0098] Example 3

[0099] The present embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The raw materials for preparing the self-stratifying coating include the following components in parts by weight: 9.3 parts of modified silicone resin, 18 parts of polyurea resin, 10 parts of curing agent, 0.3 parts of catalyst B (dibutyltin diacetate), 0.1 parts of defoaming agent, 3 parts of butyl acetate, 10 parts of xylene and 10 parts of methyl isobutyl ketone.

[0100] Preparation of modified silicone resin:

[0101] (1) 0.5 parts by weight of hexadecyltrimethoxysilane, 1.5 parts by weight of deionized water, and 3 parts by weight of anhydrous ethanol were added to a beaker for dissolution and mixing, and glacial acetic acid was added to adjust the pH to 4, the weight portion of glacial acetic acid added was 0.1 parts, and magnetic stirring was performed at 30° C. for 0.5 h for hydrolysis to obtain a hydrolyzed alkylsilane coupling agent solution.

[0102] (2) 4 parts by weight of an organic silicone resin, the hydrolyzed alkylsilane coupling agent solution obtained in step (1) and 0.2 parts by weight of a catalyst A (dibutyltin diacetate) were mixed, and stirred at 30° C. and 500 r / min for 0.5 h to obtain a modified organic silicone resin.

[0103] The preparation method of the self-stratifying coating is as follows:

[0104] (I) mixing 10 parts by weight of xylene and 10 parts by weight of methyl isobutyl ketone to form a mixed solution;

[0105] (II) mixing the modified silicone resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture A;

[0106] (III) mixing 18 parts by weight of a polyurea resin and 1 / 2 of the mixed solution obtained in step (I) to obtain a mixture B;

[0107] (IV) Mixture A obtained in step (II) and mixture B obtained in step (III) are first mixed by stirring at 500 r / min for 30 minutes, 0.1 parts by weight of a defoamer is added and stirred at 500 r / min for 30 minutes for a second mixing, a mixture of 10 parts by weight of a curing agent and 3 parts by weight of butyl acetate is added, and 0.3 parts by weight of a catalyst B is added and stirred evenly for a third mixing to obtain the self-stratifying coating.

[0108] The preparation method of the self-stratifying coating is as follows:

[0109] The self-stratifying coating was coated on a glass substrate, dried and cured at 20° C. for 24 hours to obtain the self-stratifying coating.

[0110] Examples 4 to 7 adopt the same preparation method as Example 1, except that the added raw materials and their contents are calculated by weight, as shown in Table 1.

[0111] Table 1

[0112]

[0113]

[0114] Example 8

[0115] This embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The only difference between this embodiment and Embodiment 1 is that hexadecyltrimethoxysilane is replaced with octyltrimethoxysilane of the same mass, and other conditions are the same as those in Embodiment 1.

[0116] Example 9

[0117] This embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The difference between this embodiment and embodiment 1 is that the catalyst B dibutyltin diacetate is replaced with dibutyltin dilaurate of the same mass, and other conditions are the same as those in embodiment 1.

[0118] Example 10

[0119] This embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The only difference between this embodiment and Embodiment 1 is that the weight fraction of xylene is adjusted to 15 parts, the weight fraction of methyl isobutyl ketone is adjusted to 15 parts, and the other conditions are the same as those in Embodiment 1.

[0120] Embodiment 11

[0121] This embodiment provides a self-stratifying coating, a preparation method thereof, and a self-stratifying coating. The difference between this embodiment and embodiment 1 is that the curing temperature is adjusted to 50° C., and other conditions are the same as those in embodiment 1.

[0122] Comparative Example 1

[0123] This comparative example provides a coating, a preparation method thereof, and a coating, which differs from Example 1 only in that 9.3 parts by weight of modified silicone resin in the raw materials for preparing the coating are replaced by 4 parts by weight of silicone resin, and other conditions are the same as those in Example 1.

[0124] Comparative Example 2

[0125] This comparative example provides a coating, a preparation method thereof, and a coating. The difference between the comparative example and Example 1 is that hexadecyltrimethoxysilane is replaced with heptadecafluorodecyltrimethoxysilane of the same mass, and other conditions are the same as those in Example 1.

[0126] The self-stratifying coatings and coatings provided in the above embodiments and comparative examples were tested, and the specific testing methods are as follows:

[0127] Delamination effect: Scanning electron microscopy and element scanning were used to determine whether the self-stratifying coatings and the cross-sections of the coatings provided in the embodiments and comparative examples had delamination phenomena. Five positions on the cross-section were taken for observation. If delamination occurred at different positions, it was recorded as delamination; if delamination occurred at some positions and not at other positions, it was recorded as unstable; if no delamination occurred at different positions, it was recorded as no delamination.

[0128] Adhesion: Tested in accordance with GB / T 5210-2006.

[0129] Contact angle: The water contact angle and diiodomethane contact angle were measured according to GB / T 30693-2014.

[0130] Surface energy: calculated using the OWRK surface energy calculation method.

[0131] Weather resistance: After the self-stratifying coatings and coatings provided in the examples and comparative examples were immersed in seawater for one month, the surface morphology was observed to show no obvious change. If no discoloration, blistering or shedding occurred, it was recorded as "qualified", otherwise it was recorded as "unqualified".

[0132] The test results are shown in Table 2 below:

[0133] Table 2

[0134]

[0135]

[0136] In Table 2, “ / ” means that the test was not conducted.

[0137] It can be seen from the contents of Table 1 that the self-stratifying coatings provided in Examples 1-11 can form self-stratifying coatings with self-stratifying structures, the adhesion of the self-stratifying coatings is above 4 MPa, and the surface energy is 23.9-27.6 MJ·m -2 , has good waterproof, anti-fouling and weather-resistant properties, and has good protective properties.

[0138] Figure 1 and Figure 2 The SEM images of the self-stratified coating cross section at different positions provided in Example 1 are as follows: Figure 3 for Figure 1 The SEM-EDS scanning diagram of Si elements corresponding to the cross section of the self-stratified coating shows the different distribution of Si elements in the surface and bottom layers of the cross section of the self-stratified coating. Figure 3 It can be seen that the Si content of the surface layer of the self-stratified coating is higher. Figure 1-3 It is clearly shown that the self-stratifying coating has a stratified structure.

[0139] Figure 4 The surface morphology comparison diagram of the self-stratifying coating provided in Example 1 before seawater immersion (left) and after seawater immersion for one month (right); Figure 4 It can be seen that the surface morphology of the self-stratifying coating provided in Example 1 did not change significantly after being immersed in seawater for one month, and no discoloration, blistering, shedding and the like were found.

[0140] Figure 5 This is a comparison chart of the surface energies of the self-stratifying coating provided in Example 1 and the coating provided in Comparative Example 1. The surface energy of the self-stratifying coating provided in Example 1 is lower.

[0141] Figure 6 This is a SEM image of the coating provided in Comparative Example 1. No self-stratified structure is found in the coating provided in Comparative Example 1.

[0142] Compared with Example 1 and Examples 4-5, it can be seen that as the mass of the silicone resin increases, the adhesion decreases, the water contact angle and the diiodomethane contact angle increase, and the surface energy decreases.

[0143] Compared with Example 1, the hexadecyltrimethoxysilane is replaced with the same mass of octyltrimethoxysilane (Example 8), and the stratification effect of the prepared self-stratifying coating is unstable, and the water contact angle, diiodomethane contact angle and surface energy are all reduced, and the weather resistance is unqualified. It can be seen that the alkyl silane coupling agent is preferably hexadecyltrimethoxysilane, and the self-stratifying coating prepared has better performance.

[0144] Compared with Example 1, if the catalyst B dibutyltin diacetate is replaced with the same mass of dibutyltin dilaurate (Example 9), the adhesion, water contact angle, diiodomethane contact angle and surface energy are slightly reduced. It can be seen that the self-stratifying coating prepared by catalyst B preferably being dibutyltin diacetate has better performance.

[0145] Compared with Example 1, if the curing temperature is too high (Example 11), the adhesion is reduced. Therefore, it can be seen that the curing temperature is preferably 20-40° C., and the self-stratification coating obtained has better performance.

[0146] Compared with Example 1, if the organosilicon resin is not modified with hexadecyltrimethoxysilane (Comparative Example 1), the prepared coating does not have a layered structure.

[0147] Compared with Example 1, if hexadecyltrimethoxysilane is replaced with heptadecafluorodecyltrimethoxysilane of the same mass (Comparative Example 2), the prepared coating does not have a layered structure.

[0148] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A self-stratifying coating, characterized in that: The raw materials for preparing the self-stratifying coating include modified silicone resin, polyurea resin, curing agent, auxiliary agent and solvent; The raw materials for preparing the modified silicone resin include an alkyl silane coupling agent and silicone resin.

2. The self-stratifying coating according to claim 1, characterized in that The alkylsilane coupling agent includes hexadecyltrimethoxysilane; Preferably, the silicone resin comprises hydroxy-terminated polymethylsiloxane; Preferably, the hydroxyl-terminated polymethylsiloxane has a structure as shown in the following formula I; In formula I, n=10 to 15; Preferably, the raw materials for preparing the modified silicone resin further include water, ethanol, acid and catalyst A; Preferably, the acid comprises glacial acetic acid; Preferably, the catalyst A comprises dibutyltin diacetate.

3. The self-stratifying coating according to claim 1 or 2, characterized in that The modified silicone resin is prepared by the following method: (1) mixing an alkyl silane coupling agent, water and ethanol, adding acid to adjust the pH to 3-4, and hydrolyzing to obtain a hydrolyzed alkyl silane coupling agent solution; (2) mixing the organic silicone resin, the hydrolyzed alkyl silane coupling agent solution obtained in step (1) and the catalyst A, and reacting them to obtain the modified organic silicone resin; Preferably, the weight portion of the alkylsilane coupling agent in step (1) is 0.2 to 0.5 parts; Preferably, the weight proportion of water in step (1) is 0.6 to 1.5 parts; Preferably, the weight proportion of ethanol in step (1) is 1.2 to 3 parts; Preferably, the weight proportion of the silicone resin in step (2) is 2 to 10 parts; Preferably, the weight portion of the catalyst A in step (2) is 0.1 to 0.2 parts; Preferably, the hydrolysis temperature in step (1) is 20 to 30° C. and the time is 0.25 to 1 h; Preferably, the reaction temperature in step (2) is 20-30° C. and the reaction time is 0.25-1 h.

4. The self-stratifying coating according to any one of claims 1 to 3, characterized in that The polyurea resin includes polyaspartic acid polyurea resin; Preferably, the curing agent comprises a multifunctional aliphatic isocyanate; Preferably, the auxiliary agent includes catalyst B and / or a defoaming agent; Preferably, the catalyst B comprises dibutyltin dilaurate and / or dibutyltin diacetate, more preferably dibutyltin diacetate.

5. The self-stratifying coating according to any one of claims 1 to 4, characterized in that The raw materials for preparing the self-stratifying coating include the following components in parts by weight: 5-16 parts of modified organic silicone resin, 10-18 parts of polyurea resin, 10-15 parts of curing agent, 0.2-0.6 parts of auxiliary agent and 10-60 parts of solvent.

6. The self-stratifying coating according to any one of claims 1 to 5, characterized in that The solvent includes xylene, methyl isobutyl ketone and butyl acetate; Preferably, the solvent comprises the following components in parts by weight: 1.1 to 15 parts of xylene, 1.1 to 15 parts of methyl isobutyl ketone and 3 to 5 parts of butyl acetate.

7. A method for preparing a self-stratifying coating according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: mixing modified organic silicon resin, polyurea resin, curing agent, auxiliary agent and solvent to obtain the self-stratifying coating.

8. The preparation method according to claim 7, characterized in that: The preparation method specifically comprises the following steps: (I) mixing xylene and methyl isobutyl ketone to obtain a mixed solution; (II) mixing the modified silicone resin and a portion of the mixed solvent prepared in step (I) to obtain a mixture A; (III) mixing the polyurea resin and another portion of the solvent obtained in step (I) to obtain a mixture B; (IV) performing a first mixing of the mixture A obtained in step (II) and the mixture B obtained in step (III), performing a second mixing by adding a defoamer, and performing a third mixing by adding a mixture of a curing agent and butyl acetate and a catalyst B to obtain the self-stratifying coating; Step (II) and step (III) can be carried out in any order or simultaneously.

9. A self-stratifying coating, characterized in that The self-stratifying coating is obtained by applying the self-stratifying coating according to any one of claims 1 to 6 on the surface of a substrate and curing it.

10. The self-stratifying coating according to claim 9, characterized in that The curing temperature is 20 to 50°C, more preferably 20 to 40°C; Preferably, the curing time is 8 to 24 hours.

Citation Information

Patent Citations

  • Preparation and using method of organic silicon-polyurea self-stratifying coating

    CN107298930A

  • Antifouling coating as well as use method and application thereof

    CN113881329A

  • Catalyst for recycling thermosetting epoxy resin and recycling method thereof

    CN115400759A

  • Bimetal oxide supported catalyst as well as preparation method and application thereof

    CN117599840A

Cited By

  • Ultraviolet-aging-resistant self-layering coating and preparation method thereof

    CN120574517A