Graphene peelable coating for vehicle paint protection
Through the optimization of the formula of graphene peelable coating, the existing automotive protective film has been solved, the problems of complex construction technology, high cost and difficult to peel, and the coating with moderate adhesion, easy peeling and environmentally friendly has been achieved, and it has good scratch resistance and resistance. The wear waterproof performance and UV aging resistance, and the material cost is low and the construction process is simple.
Patent Information
- Application Number
- CN202411127900.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing automotive protective film has complex construction technology, high cost, is not easy to peel, is prone to residues, and is poor in environmental protection.
Using graphene peelable coatings, optimized by formula, including polymer polymers, graphene, diluents, dispersants, release aids, defoamers, thickeners, hydrophobic agents and wetting agents, through dispersers and After processing, the sand mill is stirred at high speed and defoamed in vacuum to form a paint that is easy to peel and environmentally friendly.
It achieves moderate adhesion, easy peeling, and no residue left. It has good scratch resistance, wear and water resistance, long-lasting and beautiful paint surface, excellent UV aging resistance, low material cost, simple construction technology, and environmentally friendly.
Smart Images

Figure CN118879183A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of protective films, and is mainly applied to automobile protective films, and in particular to a graphene strippable coating for protecting automobile paint. Background Art
[0002] Existing car protective films (car covers) are usually made of PVC (polyvinyl chloride) and TPU (thermoplastic polyurethane elastomer rubber). Although PVC has a high hardness, it will gradually decompose and turn yellow and crack with long-term exposure to the sun, and it will also emit odor, which is very harmful to the environment. In addition, when replacing, the glue is easy to remain on the surface of the car, and the residual glue is not easy to remove. The PVC film is not easy to tear. TPU is relatively expensive, the production process is complicated, it is not resistant to yellowing, and it is easy to absorb dust in the air. In addition, both PVC and TPU have the characteristics of complex construction process and greater difficulty in film application. Summary of the invention
[0003] In order to solve the problems of complex construction process, high cost, difficulty in peeling, easy to leave residues and poor environmental protection of existing automobile protective films, the present invention provides a graphene strippable coating for car paint protection. Through the optimization of the formula, the graphene strippable coating is environmentally friendly, has moderate adhesion, is easy to peel off, does not leave residues, etc.
[0004] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0005] A graphene strippable coating for protecting vehicle paint. The graphene strippable coating comprises the following components in parts by weight: 80-90 parts of a high molecular polymer, 0.1-0.5 parts of graphene, 1-10 parts of a diluent, 0.5-3 parts of a dispersant, 0.5-2 parts of a stripping aid, 0.1-0.3 parts of a defoaming agent, 0.5-2 parts of a thickener, 0.5-2 parts of a hydrophobic agent, and 0.2-2 parts of a wetting agent.
[0006] Furthermore, the high molecular polymer is one or more of polyurethane emulsion or acrylic modified polyurethane emulsion, such as waterborne polyurethane emulsion JT-3070 (Guangzhou Jintu Technology Co., Ltd.).
[0007] Furthermore, the graphene is 0.1 to 0.5 parts, and the graphene is 1 to 3 layers of thin-layer graphene.
[0008] Furthermore, the diluent is 1 to 10 parts, and the diluent is one or more of deionized water, anhydrous ethanol, isopropanol and propylene glycol.
[0009] Furthermore, the dispersant is one or more of Digo 760W and polyvinyl pyrrolidone PVP K30.
[0010] Furthermore, the stripping aid is one or more of a stripping aid wax and an aqueous silicone oil, such as Silok 9666.
[0011] Furthermore, the defoaming agent is a silicone polymer, such as AFCONA-2508.
[0012] Furthermore, the thickener is one or more of a polyurethane thickener, an acrylic thickener and a cellulose thickener, such as a polyurethane thickener Z-D189 (Anqing Youtou Import and Export Co., Ltd.).
[0013] Furthermore, the hydrophobic agent is one or more of an organosilicon hydrophobic agent and a hydrophobic wax, such as PTFE-1008B wax emulsion produced by Nanjing Tianshi New Material Technology Co., Ltd.
[0014] Furthermore, the wetting agent is Digo 270.
[0015] The graphene strippable coating for automobile protective film of the present invention comprises the following steps:
[0016] Step 1: stir the graphene, water and dispersant with a disperser at 2000 r / min for 10 minutes until they are evenly dispersed, and then grind them with a sand mill to a fineness of less than 10 microns to obtain graphene slurry A;
[0017] Step 2: After the polyurethane emulsion, graphene slurry A, deionized water, stripping agent, defoaming agent, hydrophobic agent, wetting agent and thickener are mixed according to a proportion, high-speed stirring is performed until the dispersion is uniform (speed 800r / min, time 10-20min), and vacuum degassing is performed to obtain the graphene strippable coating.
[0018] Compared with the existing technology, the graphene strippable coating of the present invention has the following beneficial effects:
[0019] 1. Moderate adhesion, easy to peel off, and no residue left.
[0020] 2. It has good scratch resistance, wear resistance and waterproof performance, and can keep the paint surface beautiful for a long time.
[0021] 3. Excellent UV aging resistance.
[0022] 4. Stable performance, does not contain substances harmful to the human body, and is green and environmentally friendly.
[0023] 5. The material cost is low, the spraying method is adopted, and the construction process is simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart of the process for preparing the graphene strippable coating for vehicle paint protection. DETAILED DESCRIPTION
[0025] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, a detailed description is given below in conjunction with specific implementation methods. The following content is only an example and explanation of the concept of the present invention. The technicians in the relevant technical field can make various modifications or supplements to the specific implementation cases described or replace them with similar methods. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0026] Example 1
[0027] like Figure 1 As shown, the present embodiment prepares the graphene strippable coating according to the following steps:
[0028] Step 1: 94.5 parts of water, 5 parts of graphene, and 0.5 parts of dispersant were stirred at 2000 r / min by a disperser for 10 minutes until they were evenly dispersed, and then ground by a sand mill to a fineness of less than 10 microns to obtain graphene slurry A for standby use;
[0029] Step 2: 85 parts of polyurethane resin, 1 part of graphene slurry A, 10.8 parts of deionized water, 0.6 parts of stripping aids, 0.2 parts of defoaming agents, 0.8 parts of thickeners, 0.8 parts of hydrophobic agents, and 0.8 parts of wetting agents are stirred at high speed until they are evenly dispersed (speed 800r / min, time 10 to 20min), and vacuum degassing is performed to obtain a graphene strippable coating.
[0030] Example 2
[0031] In this embodiment, the graphene strippable coating is prepared according to the following steps:
[0032] Step 1: 94.5 parts of water, 5 parts of graphene, and 0.5 parts of dispersant were stirred at 2000 r / min by a disperser for 10 minutes until they were evenly dispersed, and then ground by a sand mill to a fineness of less than 10 microns to obtain graphene slurry A for standby use;
[0033] Step 2: 85 parts of polyurethane resin, 3 parts of graphene slurry A, 8.8 parts of deionized water, 0.6 parts of stripping aids, 0.2 parts of defoaming agents, 0.8 parts of wetting agents, 0.8 parts of thickeners, and 0.8 parts of hydrophobic agents are stirred at high speed until they are evenly dispersed (speed 800r / min, time 10-20min), and vacuum degassing is performed to obtain a graphene strippable coating.
[0034] Example 3
[0035] In this embodiment, the graphene strippable coating is prepared according to the following steps:
[0036] Step 1: 94.5 parts of water, 5 parts of graphene, and 0.5 parts of dispersant were stirred at 2000 r / min by a disperser for 10 minutes until they were evenly dispersed, and then ground by a sand mill to a fineness of less than 10 microns to obtain graphene slurry A for standby use;
[0037] Step 2: Stir 85 parts of polyurethane resin, 5 parts of graphene slurry A, 6.8 parts of deionized water, 0.6 parts of stripping aid, 0.2 parts of defoaming agent, 0.8 parts of thickener, 0.8 parts of hydrophobic agent, and 0.8 parts of wetting agent at high speed until uniformly dispersed (speed 800r / min, time 10-20min), and vacuum degassing to obtain the graphene strippable coating.
[0038] Comparative Example 1
[0039] An imported TPU car protective film.
[0040] Comparative Example 2
[0041] Imported PVC car protective film.
[0042] According to the above embodiment formula, after the configuration is completed, the coating is evenly sprayed on a substrate of the same material as the automobile shell by spraying with a spray gun, and cured for 7 days in an environment of 25±2°C and less than 50% humidity. At the same time, the film thickness of the comparative example and the embodiment is controlled to be the same. According to the test standard of Table 1, the test data of the embodiment and the comparative example are shown in Table 2.
[0043] Table 1 Test standards for various indicators
[0044] project Detection Methods Test Equipment Fineness(μm) GB / T1724-79 Scraper fineness meter (QXD-100 type) Dry film thickness GBT13452.2-2008 Coating Thickness Tester Impact strength kg.cm GB / T1732-93 QCJ paint film impact tester Hardness(H) GB / T6739-2006 Pencil Hardness Tester Peel force N GB / T2792-2014 Universal tensile testing machine Elongation at break GB / T1040-2006 Universal tensile testing machine Tensile Strength GB / T1040-2006 Universal tensile testing machine Water resistance GB / T1763-79 Soak in 50℃ warm water for 7 days Surface resistance Q / HTY017-2018 Surface resistance tester UV resistance test GB / T16422-2014 UV Accelerated Tester
[0045] Table 2 Comparison of protective film performance data of various embodiments and comparative examples
[0046]
[0047] From the data in Table 2, it can be concluded that the graphene strippable coatings prepared in Examples 1 to 3 of the present invention have the following advantages compared with the comparative example:
[0048] 1. Moderate adhesion, easy to peel off, and no residue left.
[0049] 2. It has good scratch resistance, wear resistance and waterproof performance, and can keep the paint surface beautiful for a long time.
[0050] 3. Excellent UV aging resistance.
[0051] 4. Stable performance, does not contain substances harmful to the human body, and is green and environmentally friendly.
[0052] 5. The material cost is low, the spraying method is adopted, and the construction process is simple.
[0053] The above description is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make corresponding adjustments and improvements without departing from the principles of the present invention. These adjustments and improvements should also be regarded as the scope of protection of the present invention.
Claims
1. A graphene strippable coating for car paint protection, the graphene strippable coating of the present invention comprises the following components in parts by weight: 80-90 parts of a high molecular polymer, 0.1-0.5 parts of graphene, 1-10 parts of a diluent, 0.5-3 parts of a dispersant, 0.5-2 parts of a stripping aid, 0.1-0.3 parts of a defoaming agent, 0.5-2 parts of a thickener, 0.5-2 parts of a hydrophobic agent, and 0.2-2 parts of a wetting agent.
2. The graphene strippable coating according to claim 1, characterized in that: The high molecular polymer is one or more of polyurethane emulsion or acrylic acid modified polyurethane emulsion.
3. The graphene strippable coating according to claim 1, characterized in that: The graphene is 1 to 3 layers of thin-layer graphene.
4. The graphene strippable coating according to claim 1, characterized in that: The diluent is one or more of deionized water, anhydrous ethanol, isopropanol and propylene glycol.
5. The graphene strippable coating according to claim 1, characterized in that: The dispersant is one or more of Digo 760W and polyvinyl pyrrolidone PVP K30.
6. The graphene strippable coating according to claim 1, characterized in that: The strippable auxiliary agent is one or more of a stripping auxiliary wax and an aqueous silicone oil.
7. The graphene strippable coating according to claim 1, characterized in that: The defoaming agent is an organosilicon polymer.
8. The graphene strippable coating according to claim 1, characterized in that: The thickener is one or more of a polyurethane thickener, an acrylic thickener and a cellulose thickener.
9. The graphene strippable coating according to claim 1, characterized in that: The hydrophobic agent is one or more of an organic silicon hydrophobic agent and a hydrophobic wax.
10. The graphene strippable coating according to claim 1, characterized in that: The wetting agent is Digo 270.
11. A graphene strippable coating according to any one of claims 1 to 10, characterized in that: The method comprises the following preparation steps: Step 1, stirring graphene, deionized water and dispersant with a disperser at 2000 r / min for 10 minutes until they are evenly dispersed, and then grinding with a sand mill to a fineness of less than 10 microns to obtain graphene slurry A; Step 2: After the polyurethane emulsion, graphene slurry A, deionized water, stripping agent, defoaming agent, hydrophobic agent, wetting agent and thickener are mixed according to a proportion, the mixture is evenly dispersed by stirring at a low speed (speed 800 r / min, time 10 to 20 min), and vacuum degassing is performed to obtain a graphene strippable coating.