Water-peelable temporary bonding adhesive, and preparation method and application thereof

By combining deionized water with hydrophilic solvent compounding and hydrophilic modified thermoplastic resin, temporary bonding glue can be prepared by peeling off water, solving the problems of pollution and difficulty in cleaning of traditional temporary bonding glue, and achieving environmental protection and high quality Fluidity and stable bonding effect, suitable for ultra-thin device processing.

CN118879249APending Publication Date: 2024-11-01ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113889.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing temporary bonding glue has serious pollution and difficulty in cleaning, especially the pollution caused by organic solvent-based temporary bonding glue during the debonding process and the difficulty in cleaning caused by high-temperature debonding. The ultraviolet laser debonding material equipment is high and the stability is poor. , difficult to popularize.

Method used

Deionized water and hydrophilic solvent are combined with hydrophilic modified thermoplastic resin, alkynol wetting agent and polymeric defoaming agent. The water peelable temporary preparation is made by modified thermoplastic resin and efficient stirring and dispersion technology. Bonding glue realizes nanodispersion and stability of the colloid, reduces spin coating inhomogeneity, and achieves room temperature peeling in water.

Benefits of technology

It realizes environmentally friendly, easy-to-clean water peelable temporary bonding glue, with high flowability and high temperature resistance, avoids the problems of uneven spin coating and difficulty in cleaning after bonding, and is suitable for ultra-thin device processing and has good applications. Prospects and industrial promotion potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879249A_ABST
    Figure CN118879249A_ABST
Patent Text Reader

Abstract

The invention provides a water-peelable temporary bonding adhesive, and a preparation method and application thereof. The water-peelable temporary bonding adhesive comprises the following components by weight: 40-60 parts of deionized water; 5-20 parts of a hydrophilic solvent; 0.5 to 5 parts of a coalescing agent; 20 to 40 parts of hydrophilic modified thermoplastic resin; 0.1-1 part of an antistatic agent; 0.1 to 1 part of a defoaming agent; and 0.5-2 parts of a wetting agent. The invention also discloses a preparation method of the water-peelable temporary bonding adhesive and application of the water-peelable temporary bonding adhesive in the field of ultrathin device processing. The water-peelable temporary bonding adhesive has the advantages of high flowability, high temperature resistance and easiness in water stripping, and compared with the traditional organic solvent type temporary bonding adhesive, the water-peelable temporary bonding adhesive also has the advantages of good environmental protection property, direct normal-temperature stripping in water after cleaning after bonding, easiness in cleaning and no pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to bonding adhesive technology, and in particular to a water-peelable temporary bonding adhesive, a preparation method and application thereof. Background Art

[0002] With the rapid replacement of consumer electronic products, high-end chips such as 5G communication CPU / GPU are also developing in the direction of high frequency, high speed, multi-function, high performance, small size and high reliability. In order to meet the requirements of miniaturization, multi-function and intelligence of integrated circuit chips, the development of Moore's Law is also challenged by physical limits. With the reduction of chip size, chip wafers are getting thinner and thinner, which is prone to curling or even breaking. Therefore, in the chip manufacturing process, in order to hold ultra-thin wafers, temporary bonding technology must be used to temporarily bond them to thick carriers. The "additive manufacturing" of ultra-thin devices also requires temporary bonding technology to support the semiconductor process of ultra-thin device layers. III-V compound semiconductor materials are brittle. In order to prevent breakage during processing, temporary bonding technology is also indispensable. Temporary bonding / debonding is the core technology for thinning and holding ultra-thin wafers. By fixing the device wafer on the carrier wafer, it can provide sufficient mechanical support for the ultra-thin device wafer, ensuring that the device wafer can smoothly and safely complete subsequent processes such as lithography, etching, passivation, sputtering, electroplating and reflow soldering. Temporary bonding adhesive used in ultra-thin device processing is a key material.

[0003] At present, hot-slip debonding and ultraviolet laser debonding are the two most widely used temporary bonding material system solutions. The early hot-slip debonding material WaferBond HT-10.10 and the latest ultraviolet laser debonding materials WaferBond 305 and WaferBond 701 developed by Brewer Science in the United States occupy the main domestic market, but its hot-slip debonding material WaferBond HT-10.10 is mainly composed of organic solvents, thermoplastic resins, etc., which are seriously polluted, and the debonding temperature is high and difficult to clean. The laser debonding material WaferBond 305 has high equipment costs, is difficult to popularize on a large scale, has poor product stability, is greatly affected by light, has serious local thermal damage, requires a carrier with good light transmittance, and has limited application scenarios. Therefore, it is urgent to develop an environmentally friendly, low-pollution, easy-to-clean water-peelable temporary bonding adhesive to replace the traditional solvent-based temporary bonding adhesive. Summary of the invention

[0004] The purpose of the present invention is to propose a water-peelable temporary bonding adhesive, in view of the problems of serious pollution and difficulty in cleaning to varying degrees in the current organic solvent-based temporary bonding adhesive. The temporary bonding adhesive has the advantages of high fluidity, high temperature resistance, and easy water peeling. Compared with traditional organic solvent-based temporary bonding adhesives, it also has the advantages of good environmental protection, direct peeling in water at room temperature after bonding, easy cleaning and no pollution.

[0005] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a water-peelable temporary bonding adhesive, comprising the following components in weight proportions:

[0007]

[0008] Furthermore, the deionized water is 40-50 parts.

[0009] Furthermore, the hydrophilic solvent is a polyol.

[0010] Furthermore, the hydrophilic solvent is one or more of propylene glycol, ethylene glycol, glycerol, isohexylene glycol, triethylene glycol, diethylene glycol, neopentyl glycol and dipropylene glycol.

[0011] Furthermore, the hydrophilic solvent is preferably triethylene glycol.

[0012] Furthermore, the hydrophilic solvent is 10-20 parts.

[0013] The present invention uses deionized water as the main solvent and mixes it with a hydrophilic solvent. It is safe, environmentally friendly, low-cost, and beneficial to industrial safety. At the same time, it can effectively avoid the problem of uneven spin coating caused by excessive evaporation of water during spin coating of the temporary bonding glue.

[0014] Furthermore, the film-forming aid is one or more of dipropylene glycol butyl ether, tripropylene glycol butyl ether, propylene glycol butyl ether and dipropylene glycol methyl ether.

[0015] Furthermore, the film-forming aid is preferably dipropylene glycol butyl ether.

[0016] Furthermore, the film-forming aid is 0.5-2 parts.

[0017] Furthermore, the antistatic agent is a water-soluble antistatic agent containing multiple charges.

[0018] Furthermore, the antistatic agent is one or more of octadecyl dimethyl hydroxyethyl quaternary ammonium salt, polyquaternium-30 and polyquaternium-10.

[0019] Furthermore, the antistatic agent is preferably octadecyl dimethyl hydroxyethyl quaternary ammonium salt.

[0020] Furthermore, the antistatic agent is 0.1-0.5 parts.

[0021] Furthermore, the defoamer is a polymeric defoamer.

[0022] Furthermore, the defoaming agent is one or more of polyoxyethylene ether siloxane, polydimethylsiloxane and polyoxypropylene siloxane.

[0023] Furthermore, the defoaming agent is preferably polyoxyethylene ether siloxane.

[0024] Furthermore, the defoaming agent is 0.5-1 part.

[0025] Furthermore, the wetting agent is an acetylene alcohol wetting agent.

[0026] Furthermore, the wetting agent is one or more of polyoxyethylene dodecylene glycol ether, polyoxyethylene tetradecylene glycol ether, polyoxyethylene decylene glycol ether and polyoxyethylene butynediol ether.

[0027] Furthermore, the wetting agent is preferably polyoxyethylene dodecyl alcohol ether.

[0028] Furthermore, the wetting agent is 0.5-1 part.

[0029] Furthermore, the mass ratio of the wetting agent to the defoaming agent is 1-5:1.

[0030] Furthermore, the preferred mass ratio of the wetting agent to the defoaming agent is 1-3:1.

[0031] Furthermore, the hydrophilic modified thermoplastic resin is a hydrophilic modified thermoplastic resin with a softening point of 100-160°C.

[0032] Furthermore, the hydrophilically modified thermoplastic resin is one or more of hydrophilically modified polyacrylic acid (molecular weight 3000-50,000), hydrophilically modified polyurethane (molecular weight 5000-20,000), hydrophilically modified polyvinyl acetate (molecular weight 10,000-50,000) and hydrophilically modified polyethylene terephthalate (molecular weight 10,000-100,000).

[0033] Furthermore, the modified thermoplastic resin is preferably a hydrophilic modified polyurethane (molecular weight 5000-10,000).

[0034] Furthermore, the modified thermoplastic resin is 20-30 parts.

[0035] Furthermore, the preparation method of the hydrophilic modified thermoplastic resin is as follows:

[0036] Step 1: Under nitrogen protection, add dimethyl sulfoxide and N-methylpyrrolidone to the thermoplastic resin and completely dissolve them at 40-60°C;

[0037] Step 2: Add azobisisobutyronitrile, sorbitol and poly(glycidyl methacrylate) to the material obtained in step 1, and stir to dissolve;

[0038] Step 3: Under nitrogen protection, the material obtained in step 2 is heated to 90-100° C., reacted for 18-24 hours, and then distilled under reduced pressure at 180-200° C. to remove the residual solvent, and then cooled to room temperature to prepare a hydrophilic modified thermoplastic resin.

[0039] Furthermore, the thermoplastic resin is one or more of polyacrylic acid (molecular weight 3000-50,000), polyurethane (molecular weight 5000-20,000), polyvinyl acetate (molecular weight 10,000-50,000) and polyethylene terephthalate (molecular weight 10,000-100,000).

[0040] Furthermore, the thermoplastic resin is preferably polyurethane (molecular weight 5000-10,000).

[0041] Furthermore, in step 1, the mass ratio of the thermoplastic resin, dimethyl sulfoxide and N-methylpyrrolidone is 80-120:200-300:80-150.

[0042] Furthermore, the mass ratio of the thermoplastic resin, dimethyl sulfoxide and N-methylpyrrolidone in step 1 is preferably 100:250:100.

[0043] Furthermore, in step 2, the mass ratio of the material obtained in step 1, azobisisobutyronitrile, sorbitol and poly(glycidyl methacrylate) is 400-500:0.1-1:5-20:5-20.

[0044] Furthermore, in step 2, the mass ratio of the material obtained in step 1, azobisisobutyronitrile, sorbitol and poly(glycidyl methacrylate) is preferably 450:0.5:10:10.

[0045] Another object of the present invention is to disclose a method for preparing the water-peelable temporary bonding adhesive, comprising the following steps:

[0046] Step (1): mixing deionized water, a hydrophilic solvent, a film-forming aid, a wetting agent and an antistatic agent uniformly;

[0047] Step (2): heating the solution obtained in step (1) to 60-90° C. under continuous stirring, adding a hydrophilic modified thermoplastic resin, and heating the resin to allow it to swell and dissolve rapidly until a clear and transparent liquid is formed, and cooling the mixture to room temperature;

[0048] Step (3): under high-speed dispersing and stirring conditions, add a defoaming agent, disperse the defoaming agent into the nanoparticles through high-speed shearing, form uniform nano-dispersed particles in the system, keep them stable and not aggregated, stir until the mixture is uniform, and prepare a water-peelable temporary bonding adhesive.

[0049] Furthermore, the stirring time in step (1) is 1-10 min.

[0050] Furthermore, step (2) is heated to 70-90°C.

[0051] Furthermore, the stirring condition of step (2) is 50-100 r / min.

[0052] Furthermore, the stirring condition of step (3) is 1000-2000r / min.

[0053] Furthermore, the stirring time in step (3) is 30-60 min.

[0054] Furthermore, the stirring time in step (3) is preferably 30-40 min.

[0055] Another object of the present invention is to disclose the use of the water-strippable temporary bonding adhesive in the field of ultra-thin device processing.

[0056] Furthermore, the ultra-thin device refers to a hard and brittle material wafer with a thickness of 50-200 μm, including but not limited to a gallium arsenide chip wafer, an indium phosphide chip wafer or a single crystal silicon wafer.

[0057] Furthermore, in the method for cleaning the water-strippable temporary bonding adhesive, the wafer coated with the water-strippable temporary bonding adhesive after pyrolysis bonding is placed in an aqueous solution, immersed and cleaned at 20-30° C. for 5-15 minutes, and then taken out and blown dry with nitrogen.

[0058] The water-peelable temporary bonding adhesive, preparation method and use thereof of the present invention have the following advantages compared with the prior art:

[0059] 1) The present invention can increase the hydrophilicity of the thermoplastic resin by modifying the thermoplastic resin, so that the thermoplastic resin has a hydrophilic-hydrophobic structure, prompting it to form a nano-dispersed colloid in the water system, and cooperate with the antistatic agent to avoid the adsorption and agglomeration of the dispersed colloid particles, ensuring that the hydrophilic modified thermoplastic resin is evenly distributed and stable in the temporary bonding glue, thereby ensuring that the temporary bonding glue forms a uniform thickness of the glue layer after spin coating. In the subsequent cleaning process, only room temperature water immersion treatment is required, and the hydrophilic end resin absorbs more hydrophilic charges and separates from the device surface due to the principle of like-compatibility, so that the hydrophilic modified thermoplastic resin is completely peeled off from the device surface and cleaned, thereby avoiding the temporary bonding glue from being not cleaned cleanly after bonding and the appearance of residues.

[0060] 2) The present invention uses an acetylene alcohol wetting agent and a polymeric defoamer to ensure that the temporary bonding glue can be quickly spread and leveled on the surface of the wafer device, reducing the TTV of the adhesive layer after bonding. At the same time, the polymeric defoamer has good compatibility, avoids precipitation, and reduces the protrusion of particles in the adhesive layer after bonding. The polymeric defoamer has a rapid degassing and defoaming function, so that the bubbles of the high-viscosity temporary bonding glue disappear quickly, avoiding defects in bonding, and ensuring that the temporary bonding glue has a high flatness when spin-coated.

[0061] 3) The present invention uses deionized water as the main solvent and mixes it with a hydrophilic solvent, which is safe, environmentally friendly, low-cost, and beneficial to industrial safety. At the same time, it can effectively avoid the problem of uneven spin coating caused by excessive evaporation of water during spin coating of the temporary bonding glue.

[0062] In summary, the water-peelable temporary bonding glue of the present invention is environmentally friendly, has good fluidity, is evenly spin-coated, has stable bonding, is easy to clean after peeling in water after bonding, and is environmentally friendly. It has very good application prospects and large-scale industrial promotion potential in the field of ultra-thin device processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 This is a photo of a 4-inch silicon wafer after spin coating and drying in Example 1;

[0064] Figure 2 This is a photo of the 4-inch silicon wafer after spin coating and drying in Comparative Example 4;

[0065] Figure 3 This is a photo of a 4-inch silicon wafer evenly bonded to a sapphire carrier after spin coating in Example 1;

[0066] Figure 4 This is a photo of Comparative Example 5, in which a 4-inch silicon wafer is evenly bonded to a sapphire carrier after spin coating;

[0067] Figure 5 This is a photo of the temporary bonding adhesive peeling after immersion at 25°C in Example 1;

[0068] Figure 6This is a photo of the temporary bonding adhesive peeling off after immersion in 25°C in Comparative Example 1. DETAILED DESCRIPTION

[0069] The present invention is further described below with reference to the examples. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0070] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0071] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0072] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.

[0073] In this specification, the word "may" includes both performing a certain process and not performing a certain process.

[0074] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0075] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.

[0076] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0077] Examples 1-6

[0078] Examples 1-6 disclose a variety of water-peelable temporary bonding adhesives, the components and weight ratios of which are shown in Table 1, and the preparation methods thereof are as follows:

[0079] Step (1): add deionized water, hydrophilic solvent, film-forming aid, wetting agent and antistatic agent into a stirred tank, and stir for 10 minutes to mix evenly;

[0080] Step (2): The solution of step (1) is heated to 90° C. under continuous stirring at 100 r / min, and a hydrophilic modified thermoplastic resin (hereinafter referred to as resin 1-4) is added, and the resin is rapidly swelled and dissolved by heating until a clear and transparent liquid is formed, and then cooled to room temperature;

[0081] Step (3): The reactor is started to disperse and stir at a high speed of 2000 r / min, a defoaming agent is added, and the mixture is stirred for 60 minutes until the mixture is evenly mixed, thereby completing the preparation of the water-peelable temporary bonding adhesive.

[0082] Table 1 Components and weight ratios of water-peelable temporary bonding adhesives in Examples 1-6

[0083]

[0084] Comparative Examples 1-5

[0085] Comparative Examples 1-5 disclose a variety of temporary bonding adhesives, the components and weight ratios of which are shown in Table 2, and the preparation methods thereof are the same as those of Example 1.

[0086] Table 2 Components and weight ratios of temporary bonding adhesives in comparative examples 1-5

[0087]

[0088] The preparation method of the hydrophilic modified thermoplastic resin 1-4 included in Examples 1-6 and 1-5 is as follows:

[0089] The preparation method of the hydrophilic modified thermoplastic resin 1 is as follows:

[0090] Step 1: Add 100 g of polyurethane (molecular weight 10,000) into a 500 mL reactor, protect with nitrogen, add 250 g of DMSO solvent and 100 g of NMP, and completely dissolve at 40°C.

[0091] Step 2: Add 0.5 g of azobisisobutyronitrile, 10 g of sorbitol and 10 g of poly(glycidyl methacrylate) and stir to dissolve.

[0092] Step 3: Under nitrogen protection, heat to 100°C and react for 24 hours. After the reaction is completed, perform reduced pressure distillation at 200°C to remove residual solvent, and then cool to room temperature to complete the thermoplastic resin modification.

[0093] The preparation method of the hydrophilic modified thermoplastic resin 2 is as follows:

[0094] Step 1: Add 100 g of polyacrylic acid (molecular weight 10,000) into a 500 mL reactor, protect with nitrogen, add 250 g of DMSO solvent and 100 g of NMP, and completely dissolve at 40°C.

[0095] Step 2: Add 0.5 g of azobisisobutyronitrile, 10 g of sorbitol and 10 g of poly(glycidyl methacrylate) and stir to dissolve.

[0096] Step 3: Under nitrogen protection, heat to 100°C and react for 24 hours. After the reaction is completed, perform reduced pressure distillation at 200°C to remove residual solvent, and then cool to room temperature to complete the thermoplastic resin modification.

[0097] The preparation method of the hydrophilic modified thermoplastic resin 3 is as follows:

[0098] Step 1: Add 100 g of polyvinyl acetate (molecular weight 10,000) into a 500 mL reactor, protect with nitrogen, add 250 g of DMSO solvent and 100 g of NMP, and completely dissolve at 40°C.

[0099] Step 2: Add 0.5 g of azobisisobutyronitrile, 10 g of sorbitol and 10 g of poly(glycidyl methacrylate) and stir to dissolve.

[0100] Step 3: Under nitrogen protection, heat to 100°C and react for 24 hours. After the reaction is completed, perform reduced pressure distillation at 200°C to remove residual solvent, and then cool to room temperature to complete the thermoplastic resin modification.

[0101] The preparation method of the hydrophilic modified thermoplastic resin 4 is as follows:

[0102] Step 1: Add 100 g of polyethylene terephthalate (molecular weight 10,000) to a 500 mL reactor, protect with nitrogen, add 250 g of DMSO solvent and 100 g of NMP, and completely dissolve at 40°C.

[0103] Step 2: Add 0.5 g of azobisisobutyronitrile, 10 g of sorbitol and 10 g of poly(glycidyl methacrylate) and stir to dissolve.

[0104] Step 3: Under nitrogen protection, heat to 100°C and react for 24 hours. After the reaction is completed, perform reduced pressure distillation at 200°C to remove residual solvent, and then cool to room temperature to complete the thermoplastic resin modification.

[0105] The various properties of the above embodiments or comparative examples are tested below. The test results are shown in Table 3.

[0106] Table 3 Test data

[0107]

[0108]

[0109] As shown in Table 3, the TTV after coating with the water-peelable temporary bonding adhesive of Examples 1-6 is smaller, indicating that the film formation is more uniform, and it is easy to peel and clean after use, and the bonding stability is better.

[0110] Figure 1 This is a photo of a 4-inch silicon wafer after spin coating and drying in Example 1. The bonding adhesive is spread evenly on the surface of the silicon wafer without defects. Figure 2 This is a photo of a 4-inch silicon wafer after spin coating and drying in comparative example 4. The bonding adhesive is cracked and uneven. Figure 3 This is a photo of a 4-inch silicon wafer evenly bonded to a sapphire carrier after spin coating in Example 1. The bonding is complete without defects such as voids and snowflakes. Figure 4 This is a photo of a 4-inch silicon wafer evenly bonded to a sapphire carrier after spin coating for comparative example 5; Figure 5 This is a photo of the temporary bonding adhesive peeling after immersion at 25°C in Example 1; Figure 6 This is a photo of the temporary bonding adhesive peeling after immersion in 25°C in Comparative Example 1. Figure 1 It can be seen that the surface of the 4-inch silicon wafer spin-coated in Example 1 is smooth and flawless after drying, and has high flatness. Figure 2 It can be seen that after the 4-inch silicon wafer spin-coated in Comparative Example 4 was dried, cracks appeared on the surface and the surface glue coating was uneven. Figure 3 It can be seen that the 4-inch silicon wafer of Example 1 is evenly bonded to the sapphire carrier after spin coating, and the bonding is intact and has no defects. Figure 4 It can be seen that the 4-inch silicon wafer of comparative example 5 is evenly bonded to the sapphire carrier after being spin-coated with glue, and the bonding has bubble snowflake defects, and the bonding is abnormal. Figure 5 It can be seen that after soaking at 25°C, the temporary bonding adhesive of Example 1 is peeled off, and the adhesive layer is peeled off as a whole, which is easy to clean without any residue. Figure 6 It can be seen that the temporary bonding adhesive of Comparative Example 1 cannot be peeled off after being immersed at 25° C., and the residue is serious.

[0111] in:

[0112] Performance 1 TTV test method after glue coating is:

[0113] Taking a 4-inch silicon wafer as an example, a temporary bonding glue was used for spin coating verification. The 4-inch silicon wafer was placed in the inner cavity of the spin coater, the speed was set to 1000r / min, the spin coating time was 20s, and 4.5ml of glue was dripped. The spin-coated silicon wafer was placed in a 140℃ oven for 120s to evaporate the solvent, the dried silicon wafer was taken out, and the TTV of the silicon wafer after the glue coating was measured.

[0114] Performance 2 cleaning residue test method:

[0115] Taking a 4-inch silicon wafer as an example, a bonding adhesive is used for spin coating verification. The spin-coated silicon wafer is placed in a 140°C oven for 120 seconds to evaporate the solvent. The dried silicon wafer is taken out and placed in an aqueous solution, soaked and cleaned at 25°C for 10 minutes to check whether the bonding adhesive of the silicon wafer is peeled off. After peeling, take it out and blow it dry with nitrogen to observe the cleanliness of the silicon wafer surface.

[0116] Performance 3 Bonding stability test method:

[0117] The bonding adhesive was used to perform the die bonding experiment. The silicon wafer was spin-coated with the bonding adhesive and baked to evaporate the solvent. The adhesive layer was adhered to the surface of a sapphire carrier at 160°C and heated at 90g / cm 2 The pressure is pressed for 60 seconds, then cooled to room temperature, and then chemical mechanical polishing verification is performed to observe whether the silicon wafer is scratched or damaged after polishing and bonding. If there is scratching or damage, it means that the bonding is not firm and unstable.

[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-peelable temporary bonding adhesive, characterized in that: The composition includes the following components in weight ratio:

2. The water-peelable temporary bonding adhesive according to claim 1, characterized in that: The hydrophilic solvent is a polyol; And / or, the film-forming aid is one or more of dipropylene glycol butyl ether, tripropylene glycol butyl ether, propylene glycol butyl ether and dipropylene glycol methyl ether; And / or, the antistatic agent is a water-soluble antistatic agent containing multiple charges; and / or, the defoamer is a polymeric defoamer; And / or, the wetting agent is an acetylene alcohol wetting agent.

3. The water-peelable temporary bonding adhesive according to claim 1, characterized in that: The hydrophilic modified thermoplastic resin is a hydrophilic modified thermoplastic resin with a softening point of 100-160°C.

4. The water-peelable temporary bonding adhesive according to claim 1, characterized in that: The hydrophilically modified thermoplastic resin is one or more of hydrophilically modified polyacrylic acid, hydrophilically modified polyurethane, hydrophilically modified polyvinyl acetate and hydrophilically modified polyethylene terephthalate.

5. The water-peelable temporary bonding adhesive according to claim 1, 3 or 4, characterized in that: The preparation method of the hydrophilic modified thermoplastic resin is as follows: Step 1: Under nitrogen protection, add dimethyl sulfoxide and N-methylpyrrolidone to the thermoplastic resin and completely dissolve them at 40-60°C; Step 2: Add azobisisobutyronitrile, sorbitol and poly(glycidyl methacrylate) to the material obtained in step 1, and stir to dissolve; Step 3: Under nitrogen protection, the material obtained in step 2 is heated to 90-100° C., reacted for 18-24 hours, and then distilled under reduced pressure at 180-200° C. to remove the residual solvent, and then cooled to room temperature to prepare a hydrophilic modified thermoplastic resin.

6. The water-peelable temporary bonding adhesive according to claim 5, characterized in that: The thermoplastic resin is one or more of polyacrylic acid, polyurethane, polyvinyl acetate and polyethylene terephthalate.

7. The water-peelable temporary bonding adhesive according to claim 5, characterized in that: The mass ratio of the thermoplastic resin, dimethyl sulfoxide and N-methylpyrrolidone in step 1 is 80-120:200-300:80-150.

8. The water-peelable temporary bonding adhesive according to claim 5, characterized in that: In step 2, the mass ratio of the material obtained in step 1, azobisisobutyronitrile, sorbitol and poly(glycidyl methacrylate) is 400-500:0.1-1:5-20:5-20.

9. A method for preparing the water-peelable temporary bonding adhesive according to any one of claims 1 to 8, comprising the following steps: Step (1): mixing deionized water, a hydrophilic solvent, a film-forming aid, a wetting agent and an antistatic agent uniformly; Step (2): heating the solution obtained in step (1) to 60-90° C. under continuous stirring, adding a hydrophilic modified thermoplastic resin until a clear and transparent liquid is formed, and cooling to room temperature; Step (3): under high-speed dispersing and stirring conditions, add a defoaming agent and stir until the mixture is uniformly mixed to prepare a water-peelable temporary bonding adhesive.

10. Use of the water-peelable temporary bonding adhesive according to any one of claims 1 to 8 in the field of ultra-thin device processing.