Thermochromic iodobismuthate hybrid, hybrid-containing film / ink and preparation method thereof
By developing thermochromic iodine bismuthate hybrid [(C2H8N)3][BiI6], the problems of low response sensitivity and long discoloration time in the prior art are solved, and obvious color changes in low temperatures and short time are achieved. Good complex color performance, suitable for a wide range of temperature indicator applications.
Patent Information
- Application Number
- CN202411212111.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
AI Technical Summary
The existing thermochromic iodine bismuthate organic-inorganic hybrid materials have low response sensitivity, long discoloration response time and long fading time, which limits their commercial applications.
A thermochromic iodine bismuthate hybrid [(C2H8N)3][BiI6] was developed to prepare crystals with excellent color distortion properties by reacting cyanopyridine, hydroiodic acid, and bismuth iodide in specific solvents. The material can complete color changes within 5 seconds under an environment of ≥80°C, and achieve significant color changes at a lower temperature, and has good repeatability.
It realizes color change at lower temperatures and short time, has excellent color change response and complex color performance, is suitable for temperature indicator materials, the temperature indicator range can reach 77K (-196℃)-503K (230℃), and the repeatability can be More than 500 times.
Smart Images

Figure CN118879304A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal functional materials, and in particular relates to a thermochromic iodine bismuthate hybrid and a film / ink containing the hybrid and a preparation method thereof. Background Art
[0002] The research on thermochromic crystalline materials is one of the key research projects in the field of chemistry and materials chemistry, and thermochromic materials have great application prospects in national defense science and technology, medical care and daily life. With the proposition of organic-inorganic hybrid compounds, a new field of research on thermochromic materials has been opened. Organic-inorganic hybrid materials refer to metal organic framework crystal materials with periodic structures formed by self-assembly of metal ions and small molecule ligands. They have the dual characteristics of thermal stability and high strength of inorganic compounds and easy adjustment or processing of organic compounds. They can even produce some new properties through synergistic effects and become an effective means of developing thermochromic materials. Among them, the development of iodine bismuth salt system thermochromic materials is relatively cutting-edge.
[0003] Chinese patent CN108949142A reports a metal organic hybrid material crystal with thermochromic properties and its application. The molecular formula of the material is (C 12 H 14 N2)2[Bi2Cl 10 I], which is prepared by the following method: mixing hydroiodic acid and methanol for reaction, then adding bipyridine, bismuth chloride, and hydrochloric acid, after reaction and drying, the above crystals are obtained. This material can be used for the preparation of heat-changing color windows, temperature alarms, etc. Its solution is applied to various heating machine parts such as computer mainframes and agricultural machinery engines. When the temperature is around 200°C, the material will turn red in about 30 minutes to serve as a warning. Although this thermochromic material shows obvious chromaticity difference, it has the problem of low response sensitivity (color change response time is about 30 minutes, and fading time is 1 day at room temperature), which greatly restricts its commercial application.
[0004] Therefore, in view of the defects of the existing technology, it is necessary to conduct further research on iodine bismuth salt organic-inorganic hybrid materials and apply new crystalline materials to ink or thin film thermochromic materials. This has important practical guiding significance for the application of thermochromic materials. Designing thermochromic crystalline materials with excellent color-changing properties and preparing them into thin films or ink materials (with obvious chromaticity difference, color change response and fading time <30s) is particularly important for basic research and its anti-counterfeiting applications. Summary of the invention
[0005] The present invention aims to provide a thermochromic iodine bismuth salt hybrid to solve the technical problem of the lack of iodine bismuth salt organic-inorganic hybrid materials with excellent performance in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] Thermochromic iodine bismuth salt hybrid, its molecular formula is [(C2H8N)3][BiI6], and its space group is R-3.
[0008] Furthermore, the thermochromic iodine bismuthate hybrid is a trigonal crystal system, and its unit cell parameters are:
[0009] Further, a thermochromic iodine bismuthate hybrid, which is composed of [BiI6] 3- Anion and (C2H8N) + Cations are formed by electrostatic interactions and hydrogen bonds.
[0010] The thermochromic iodine bismuth salt hybrid prepared by this scheme can undergo obvious color changes in an environment of ≥80°C, and at this temperature, the color change process can be completed after being placed for 5s (that is, the color of the crystal material changes sufficiently, and after being placed for more than 5s, the color no longer changes further and remains at a stable level, which is convenient for operation and observation). Compared with other calorific value phase change materials in the prior art, the materials of this scheme only need to be heated to 80°C or above to achieve obvious color changes relative to the color of the materials at room temperature. The required temperature is relatively low and easy to operate. If heated to 150°C or above, the color change will be more obvious and easy to judge. Moreover, the material can achieve complete color change in a very short time under the set temperature environment, further increasing the convenience of operation. In addition, the materials of this scheme can be reused (repeated heating and cooling to achieve color change), and the repeatability can reach more than 500 times.
[0011] Therefore, the iodine bismuth salt hybrid of this scheme is an ideal thermochromic material and can be used as a temperature indicating material with a temperature indication range of 77K (-196°C)-503K (230°C).
[0012] The technical solution also provides a method for preparing a thermochromic iodine bismuth salt hybrid, wherein cyanopyridine, hydroiodic acid, and bismuth iodide are mixed in a solvent and then allowed to stand to precipitate crystals.
[0013] Further, the cyanopyridine includes at least one of 2-cyanopyridine, 3-cyanopyridine and 4-cyanopyridine.
[0014] Furthermore, the solvent is acetonitrile or N,N-dimethylformamide.
[0015] Furthermore, the usage ratio of cyanopyridine, hydroiodic acid, bismuth iodide and solvent is: 0.3-0.5mmol: 0.5-6.0mmol: 0.3-0.5mmol: 4.0-10.0ml.
[0016] The technical solution also provides the use of thermochromic iodine bismuth salt hybrids in thermochromic films or thermochromic inks.
[0017] Furthermore, the raw materials of the thermochromic film include a thermochromic iodine bismuth salt hybrid and a polymer material; the addition amount of the thermochromic iodine bismuth salt hybrid in the thermochromic film is 15-50%; and the polymer material is one of polyvinylidene fluoride, polyimide, polysulfone resin, polyethylene, and polypropylene.
[0018] Furthermore, the raw materials of the thermochromic ink include a thermochromic iodine bismuth salt hybrid and ink; the addition amount of the thermochromic iodine bismuth salt hybrid in the thermochromic ink is 40-50%.
[0019] The principle and beneficial effects of this technical solution are:
[0020] This project takes the preparation and application of thermochromic crystalline materials and thermochromic thin film materials as the research direction, explores the relationship between nitrogen-containing organic cations and inorganic anions of iodine bismuth salts, and their potential thermochromic properties, and finally studies their applications in life. This study uses bismuth iodide as an inorganic component and 2-cyanopyridine / 3-cyanopyridine / 4-cyanopyridine as organic components. In a specific solvent, by changing the amount of hydroiodic acid (47%) in the system, it evaporates at room temperature to synthesize dark red transparent block crystals: [(C2H8N)3][BiI6]. The analysis of the experimental data shows that the addition of different amounts of hydroiodic acid (47%) has a great influence on the synthesis of the crystal and the color state of the crystal. The analysis and analysis of the crystal structure show that [BiI6] 3- The anion is an octahedral structure consisting of six iodine atoms surrounding one bismuth atom, similar to (C2H8N) +The cations are connected by electrostatic action and hydrogen bonds. After the crystal is heated, the bond angle of I-Bi-I in the structure is slightly distorted, resulting in a change in the color of the crystal. As the temperature drops, the color returns to its initial state. And through testing, this thermally induced change in the bond angle has excellent reversibility. Therefore, this study uses a polymer doping method and a method of mixing with a colorless ink to prepare thermochromic film materials and ink materials, respectively, which also have good fatigue resistance. Whether it is based on the synthesis of crystal [(C2H8N)3][BiI6] or the preparation of film materials and ink materials, it provides new methods and ideas for exploring the synthesis of organic-inorganic hybrid materials and their development and application in anti-counterfeiting materials. This technical solution is the first time that crystal [(C2H8N)3][BiI6] is applied to the preparation of film materials and ink materials, overcoming the gaps in the prior art and improving the application and promotion prospects of thermochromic crystalline materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the thermochromic behavior of the color-changing crystalline material film of Example 2.
[0022] Figure 2 Schematic diagram of the color change behavior of the thermotropic ink material in Example 3.
[0023] Figure 3 This is the asymmetric primitive diagram of [(C2H8N)3][BiI6] of Experimental Example 1.
[0024] Figure 4 This is the spatial stacking diagram of [(C2H8N)3][BiI6] in Experimental Example 1.
[0025] Figure 5 This is the infrared spectrum of [(C2H8N)3][BiI6] of Experimental Example 1.
[0026] Figure 6 This is the simulation / experimental comparison diagram of [(C2H8N)3][BiI6] of Experimental Example 1.
[0027] Figure 7 This is the color change and recolorization behavior of [(C2H8N)3][BiI6] at liquid nitrogen temperature in Experimental Example 1.
[0028] Figure 8 This is the thermochromic color-reversing behavior of [(C2H8N)3][BiI6] in Experimental Example 1.
[0029] Fig. 9 This is the variable temperature-UV spectrum of [(C2H8N)3][BiI6] of Experimental Example 1. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.
[0031] Example 1: Synthesis of iodine bismuth salt organic-inorganic hybrid (crystalline material)
[0032] The synthesis of iodobismuthate organic-inorganic hybrids (crystalline materials) comprises the following steps:
[0033] S1: Pipette 4.0-10.0 ml (preferably 5.0 ml) of acetonitrile / N,N-dimethylformamide reagent into a 25-100 ml (preferably 50 ml) beaker;
[0034] S2: Accurately weigh 0.3-0.5 mmol (0.0312-0.0521 g, preferably 0.5 mmol, 0.0521 g) of 2-cyanopyridine / 3-cyanopyridine / 4-cyanopyridine on an analytical balance and add it to the above beaker, add a magnet, and place it on a magnetic stirrer for stirring;
[0035] S3: Use a pipette to pipette a series of amounts of hydroiodic acid (47%) and add it to the above solution, and continue stirring;
[0036] S4: Accurately weigh 0.3-0.5 mmol (0.1770-0.2948 g, preferably 0.5 mmol, 0.2948 g) of bismuth iodide on an analytical balance and add it to the above solution, and continue stirring until all the solid is dissolved.
[0037] At this time, the solution is dark red / red-orange. Place it under a fume hood for 5-15 days, and dark red block crystals / red strip crystals precipitate from the solution. Use a vacuum pump to filter, and rinse with anhydrous ethanol 3-4 times during the filtration process to obtain dark red block crystals / red-orange block crystals. Finally, dry the crystals, weigh them, and store them to obtain [(C2H8N)3][BiI6] crystalline material.
[0038] The typical [(C2H8N)3][BiI6] crystalline material synthesized was tested. The structure of the material synthesized by the above method (three cyanopyridines and two different solvents) was consistent. The following table shows the data of the typical crystalline material synthesized. Under an optical microscope, a transparent block single crystal with a regular shape, good gloss and a size of 0.25×0.23×0.15mm was selected and fixed to one end of the glass fiber with glue. Then, an X-ray single crystal diffractometer was used at 100K to test and collect crystal ray data. Then, the ideal single crystal structure was obtained by direct analysis and refinement using Olex 2 software. The main crystallographic parameters, bond length and bond angle parameters of the organic-inorganic hybrid [(C2H8N)3][BiI6] are shown in Tables 1 and 2.
[0039] Table 1: Main crystal parameters of organic-inorganic hybrids
[0040]
[0041]
[0042] Table 2: Bond length and bond angle parameters of organic-inorganic hybrids
[0043]
[0044]
[0045] Example 2: Preparation of thermochromic film
[0046] Accurately weigh 15mg-60mg of the [(C2H8N)3][BiI6] crystalline material prepared in Example 1, grind it into powder with a mortar, add 1.2ml of anhydrous ethanol, seal the film, use a 240W power ultrasonic cleaner to ultrasonicate for 30 minutes, after the end of the ultrasonication, add 85mg-40mg of the polymer material polyvinylidene fluoride (Xia reagent, specification 10-60, batch number: Z05120, molecular weight 476.13, PVDF), seal the film and stir on a magnetic stirrer for 4 hours, then drip it onto a glass sheet with a rubber-tipped dropper, spread it evenly, and finally place it on a 120℃-160℃ constant temperature heating table (preferably 160℃) and heat it for 2-3 minutes, then remove it. See Table 3 for the doping ratio and color change effect. From the experimental data in Table 3, it can be seen that the ratio of [(C2H8N)3][BiI6] crystalline material powder to PVDF is 30-45:55-70, which can achieve obvious color change of the film with respect to temperature.
[0047] Table 3: Doping ratio of each substance in film preparation and color change effect
[0048] serial number Crystalline powder (mg) PVDF(mg) Anhydrous ethanol (ml) Color changing effect 1 15 85 1.2 Not obvious 2 20 80 1.2 Not obvious 3 25 75 1.2 Not obvious 4 30 70 1.2 obvious 5 35 65 1.2 obvious 6 40 60 1.2 obvious 7 45 55 1.2 obvious 8 50 50 1.2 Not obvious
[0049] Organic-inorganic hybrid crystalline material [(C2H8N)3][BiI6] was prepared by doping high molecular weight polyvinylidene fluoride (PVDF) to prepare a crystalline material film with thermochromic properties. The crystalline powder accounted for 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% of the mixture of crystalline powder and PVDF (see Table 3), and the appearance of the film was shown in Table 3. Figure 1 . The left side shows the color of the film material at room temperature, which is a single-layer film with a crystal powder content of 15%, 20%, 25%, 30%, 35%, 40%, 45%, and 50%, respectively, and its color deepens one by one. When the film is placed in a 150°C environment for 5s, an obvious color change can be observed, and the color of the film further deepens. When the film is placed back at room temperature, after 5s, the color of the film returns to the state before heating. However, the film material with a content below 25% has an unobvious color change effect, and the film material with a content above 50% is masked by the darker color of the original crystal powder. Therefore, the content of the crystal powder material is best between 25% and 50% (more preferably 30%-45%), and the color change effect is obvious, all changing from orange to dark red, and has excellent fatigue resistance (can change color multiple times), which provides certain practical significance for the preparation of thermochromic film materials and the research and application of thermochromic anti-counterfeiting film materials.
[0050] Example 3: Preparation of color-changing ink
[0051] By uniformly mixing ink printing material and crystalline material powder, a thermochromic anti-counterfeiting ink material is prepared. Different patterns or logos can be prepared by engraving. After heating, they will show a color different from room temperature, achieving an anti-counterfeiting effect. LLU is used as a seal, engraved with a pattern, and heated to change from yellow at room temperature to orange-red at 150°C. After cooling, it can almost return to the initial yellow state at room temperature ( Figure 2 ), and its color-changing and recoloring effect can reach hundreds of times, which can achieve the purpose of anti-counterfeiting (preparation of color-changing anti-counterfeiting labels). More specifically, the color-changing ink used in the above experiment is prepared by the following method: commercial white ink printing material (brand: Kaiyu, model: WD-22 white) and the crystalline material powder prepared in Example 1 are evenly mixed in a ratio of 40:60 to obtain a thermochromic anti-counterfeiting ink material (the amount of thermochromic iodine bismuth salt hybrid added to the thermochromic ink is 40-50%). The thermochromic anti-counterfeiting ink material is applied to the seal, and then the seal is used to print a pattern on paper, and then subsequent color change and recoloring experiments are carried out. The carrier printed with the pattern is placed in an environment of 150°C, and the color changes fully after 5s; then, the carrier printed with the pattern is placed at room temperature, and the color is restored after 5s (restored to the color at room temperature before being placed in an environment of 150°C, and the color is completely restored).
[0052] Experimental Example 1:
[0053] (1) Study on synthesis conditions
[0054] With reference to Example 1, in the experimental study process, acetonitrile was used as solvent, and 2-cyanopyridine (3-cyanopyridine or 4-cyanopyridine), 47% hydroiodic acid, and bismuth iodide were added in sequence for crystal synthesis. This experimental example explores the effect of 47% HI of different amounts of substances on the color and yield of the product. When the amount of substance of 47% hydroiodic acid is less than 2mmol, it is not easy to produce crystals. When it is higher than 3mmol, a small amount of dark red block crystals are generated (as the final product, formed after the solution evaporates completely; the crystal size of the crystals crystallized under the solvent used in this scheme is relatively large, so the color is relatively dark, but the crystal structure is consistent with the red-orange block crystals mentioned later, as shown in Tables 1 and 2; after the dark red block crystals or the red-orange block crystals are ground into powder, the color is consistent, there is no difference in appearance, and after being ground into powder, it is used for the preparation of subsequent film materials and ink materials). Experiments have shown that when the acidity of the system is low, it is not easy to synthesize crystals, and when the acidity is high, the yield of the product is still low. In this group of experiments, it can be found that cyanopyridine substituted at different positions has almost no effect on the synthesis of the target crystal. The experimental results are shown in Table 4.
[0055] Table 4: Comparison of experimental conditions and experimental results (acetonitrile as reaction solvent)
[0056]
[0057]
[0058] Referring to the above conditions, the solvent was changed to N, N-dimethylformamide (DMF), and the other reactants remained unchanged. Red-orange block crystals (the final product, formed after the solution evaporated completely) were synthesized through the experiment. However, when the acidity of the system is low, it is not easy to produce crystals or a small amount of crystals is produced. When the amount of hydroiodic acid (47%) is higher than 3mmol, the yield is higher. The comparative experiment shows that the use of N, N-dimethylformamide as a reaction solvent can improve the yield, and the amount of hydroiodic acid (47%) is the main factor affecting the product yield. In this group of experiments, the appearance of the crystals synthesized using three cyanopyridines is basically the same. The powder XRD diffraction pattern shows that the three crystals are the same hybrid. The experimental results are shown in Table 5. Therefore, the reaction solvent of this scheme is preferably DMF, and the amount of hydroiodic acid (47%) is 2-6 mmol, which can control the product yield at a higher level when 3-cyanopyridine and 4-cyanopyridine are used as reaction substrates; the amount of hydroiodic acid (47%) is 3-4 mmol, which can control the product yield at a higher level when 2-cyanopyridine is used as the reaction substrate.
[0059] Table 5: Comparison of experimental conditions and experimental results (DMF as reaction solvent)
[0060]
[0061]
[0062] (2) Crystal structure description
[0063] The organic-inorganic hybrid [(C2H8N)3][BiI6] prepared by Scheme 19-36 crystallizes in the R-3 space group of the trigonal system, such as Figure 3 The asymmetric structural unit diagram. Through the analysis and analysis of the crystal structure, it is shown that [BiI6] 3- The anion is an octahedral stacking structure consisting of six iodine atoms surrounding one bismuth atom (such as Figure 4 along the c-axis direction [C2H8N] + The cations are accumulated in space to form cation holes, which are connected by electrostatic interaction and hydrogen bonds to form iodine bismuth salt hybrid color-changing crystals. During the heating process, the bond angle of I-Bi-I in the structure of the crystal is slightly distorted. The bond lengths of Bi(1)-I(1), Bi(1)-I(2), Bi(1)-I(3), and Bi(2)-I(4) are 3.0702(3), 3.0361(3), 3.0975(3), and 3.0725(3), respectively. The bond angles of I-Bi-I range from 87.502(9) to 92.498(9) and 180.0; the bond lengths of N(1)-C(2), N(1)-C(1), N(2)-C(4), and N(2)-C(3) are 1.485(7), 1.487(7), 1.466(7), and 1.475(8), respectively. These bond length data are consistent with the characteristics of dimethylamine cation.
[0064] (3) Infrared spectroscopy
[0065] The infrared absorption spectrum of the hybrid [(C2H8N)3][BiI6] is as follows Figure 5 As shown in the spectrum, 3460cm -1 The peak is the stretching vibration region of the organic cation CN bond, 1558cm -1 The peak is the stretching vibration region of organic cation NH, 1008 cm -1 The peak of the out-of-plane bending vibration of NH is 756 cm -1 The stretching vibration of saturated CH bonds is at 2952 cm -1 In summary, it is confirmed that there is a dimethylamine cationic organic component in the sample.
[0066] (4) X-ray powder diffraction (XRD) pattern
[0067] like Figure 6 Shown are the experimental and simulated diffraction spectra of the X-ray powder diffraction (XRD) of the organic-inorganic hybrid [(C2H8N)3][BiI6] at 5-40°. The spectrum peaks of the crystalline material samples synthesized experimentally almost coincide with the spectrum peaks simulated by the computer, proving that the synthesized product is the target product with higher purity.
[0068] (5) Thermochromic properties
[0069] The organic-inorganic hybrid [(C2H8N)3][BiI6] can exhibit excellent low-temperature and high-temperature thermochromism, and has good color-changing and color-replicating properties. Figure 7 The color change of [(C2H8N)3][BiI6] hybrid crystal under liquid nitrogen conditions is shown, from orange-red to yellow at room temperature, and then from yellow to orange-red when the liquid nitrogen temperature is slowly restored to room temperature. More specifically, No. 1 is the color of the crystal immersed in liquid nitrogen, and No. 2-4 are the color changes of the crystal as the liquid nitrogen evaporates. The crystal is placed in a watch glass, and liquid nitrogen is poured in. As the liquid nitrogen evaporates, the color change of the crystal is photographed. Figure 8 It means that during the heating process, the crystal gradually changes from orange-red at room temperature to dark red, and as the temperature decreases, the color returns from dark red to red-orange at room temperature (during the experiment, the crystal material reaches the set temperature and maintains for 5 seconds to achieve complete color change, which is different from other temperature-controlled color-changing materials that require about 30 minutes or more of maintenance time at a specific color-changing temperature to ensure complete color change). More importantly, the crystal has good color-changing and color-replicating properties at 150°C, and the repeatability can reach more than 500 times. Its color-changing behavior may be due to the change in Bi-I bond length and bond angle in the structure caused by temperature.
[0070] like Fig. 9 As shown in the figure, the black, red and blue curves represent the ultraviolet reflection curves at 304K (about 31℃), 423K (about 150℃) and restored to 304K, respectively. When heated from 304K to 423K, the curve red-shifts from 550nm to 600nm, indicating that its color changes; when the temperature returns to 304K, the curve also returns to the initial state and coincides with it, indicating that its color is restored. In summary, the [(C2H8N)3][BiI6] crystalline hybrid can reversibly change color between 304K-423K, verifying the thermochromic properties of the crystal from the perspective of ultraviolet-reflection.
[0071] In summary, the crystal material of this scheme has a very wide response temperature range, and can produce color changes in the range of 77K (-196℃)-503K (230℃), and the above color changes are recoverable, and the color change process can be repeated. That is, the materials of this scheme can be used to indicate or warn within the above temperature range, and the temperature information is converted into intuitive visual information. However, most of the crystal materials in the prior art do not have the above-mentioned wide temperature response range. At present, the crystal materials for color changes in response to temperature are mainly focused on the research of color changes caused by high temperature. There are very few research reports on low-temperature color-changing crystal materials, and the research on the crystal materials of this scheme that can achieve obvious color changes at both high and low temperatures is even less, which further highlights the promotion and application value of the crystal materials of this scheme.
[0072] In addition, the crystal material of the present solution has a significant chromaticity difference. The crystal material appears yellow in a liquid nitrogen 77K environment, red at room temperature, and black-red at 503K. The crystal material of the present solution can be observed to have a significant chromaticity change by naked eyes when it is heated from room temperature to 80°C, while some crystal materials in the prior art need to be heated to a higher temperature to have a chromaticity change observable to naked eyes.
[0073] Finally, the color change response and fading time of the crystal material of this scheme are very short. After the crystal material reaches the specified temperature, the full color change (color change and complex color) can be achieved in about 5 seconds.
[0074] Comparative Example 1
[0075] In contrast, Chinese patent CN108949142A reports a metal organic hybrid material crystal with thermochromic properties and its application. The molecular formula of the material is (C 12 H 14 N2)2[Bi2Cl 10 I], and the [(C2H8N)3][BiI6] crystal material of this scheme have certain similarities, both containing nitrogen-containing organic cations and similar inorganic anions. However, there are significant differences in the performance of the two, especially in the performance of color change in response to temperature changes. In addition, (C 12 H 14 N2)2[Bi2Cl 10 I] is synthesized from 2,2'-bipyridine, hydroiodic acid, bismuth chloride, hydrochloric acid and methanol as raw materials, and [(C2H8N)3][BiI6] in this scheme is synthesized from cyanopyridine, hydroiodic acid, bismuth chloride and acetonitrile / N,N-dimethylformamide as raw materials. The former synthesis requires reaction at 145°C-190°C, while the present scheme adopts room temperature volatilization method to obtain the target product, and the synthesis conditions are milder.
[0076] (C 12 H 14 N2)2[Bi2Cl 10 I] can only achieve full color change after being placed at 200℃ for about 30 minutes, with poor sensitivity and limited application value. However, [(C2H8N)3][BiI6] in this scheme can achieve full color change after being placed at 80℃ for 5 seconds (the color change effect at 150℃ is even better), and is very sensitive to temperature changes, achieving unexpected technical effects. In addition, the color reproduction performance of the crystal material in this scheme is also very excellent. After returning to room temperature, it can quickly restore the original color (almost 5 seconds after the crystal material is cooled to room temperature), while (C 12 H 14 N2)2[Bi2Cl 10 I] needs to be placed at room temperature for 1 day to fade. The above comparison also shows that even if thermochromic crystalline materials have structural similarities, due to the differences in organic cations and halogen ions in inorganic components, when they are used as thermochromic materials, their sensitivity to temperature will be relatively different. It is difficult to predict the temperature sensitivity of new crystalline materials based solely on the structural composition. The [(C2H8N)3][BiI6] crystalline material of this solution can complete color changes at lower temperatures and in shorter times, and its excellent performance far exceeds the expectations of those skilled in the art.
[0077] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. Thermochromic iodine bismuthate hybrid, characterized in that: Its molecular formula is [(C2H8N)3][BiI6] and its space group is R-3.
2. The thermochromic iodine bismuthate hybrid according to claim 1, characterized in that: It is a trigonal crystal system, and its unit cell parameters are:
3. The thermochromic iodine bismuthate hybrid according to claim 2, characterized in that: It is [BiI6] 3- Anion and (C2H8N) + Cations are formed by electrostatic interactions and hydrogen bonds.
4. The method for preparing the thermochromic iodine bismuthate hybrid according to any one of claims 1 to 3, characterized in that: Cyanopyridine, hydroiodic acid and bismuth iodide are mixed in a solvent and then allowed to stand to precipitate crystals.
5. The method for preparing the thermochromic iodine bismuthate hybrid according to claim 4, characterized in that: The cyanopyridine includes at least one of 2-cyanopyridine, 3-cyanopyridine and 4-cyanopyridine.
6. The method for preparing the thermochromic iodine bismuthate hybrid according to claim 4, characterized in that: The solvent is acetonitrile or N,N-dimethylformamide.
7. The method for preparing the thermochromic iodine bismuthate hybrid according to claim 4, characterized in that: The usage ratio of cyanopyridine, hydroiodic acid, bismuth iodide and solvent is: 0.3-0.5mmol: 0.5-6.0mmol: 0.3-0.5mmol: 4.0-10.0ml.
8. Use of the thermochromic iodine bismuthate hybrid according to any one of claims 1 to 3 in thermochromic films or thermochromic inks.
9. The use of the thermochromic iodine bismuth salt hybrid according to claim 8 in a thermochromic film or a thermochromic ink, characterized in that: The raw materials of the thermochromic film include thermochromic iodine bismuth salt hybrid and polymer material; the addition amount of the thermochromic iodine bismuth salt hybrid in the thermochromic film is 15-50%; the polymer material is one of polyvinylidene fluoride, polyimide, polysulfone resin, polyethylene and polypropylene.
10. The use of the thermochromic iodine bismuth salt hybrid according to claim 8 in a thermochromic film or a thermochromic ink, characterized in that: The raw materials of the thermochromic ink include a thermochromic iodine bismuth salt hybrid and ink; the addition amount of the thermochromic iodine bismuth salt hybrid in the thermochromic ink is 40-50%.