Magnetic composite bio-based luminescent material as well as reinforced orientation uniformity preparation method and application thereof
Through the weak magnetic field and superparamagnetic Fe3O4 NP, the orderly arrangement of cellulose nanocrystals is synergistically induced, and the photoluminescence performance reduction caused by disordered cellulose nanocrystal orientation is solved, achieving efficient photoluminescence performance improvement and magnetic response The granting of characteristics has expanded its application in the fields of intelligent sensing and optical anti-counterfeiting.
Patent Information
- Application Number
- CN202410906406.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
Cellulose nanocrystals are disorderly oriented during evaporation-induced self-assembly, resulting in a reduced photoluminescence performance, limiting their application in the field of optical.
The weak magnetic field and superparamagnetic Fe3O4 NP jointly induce the orderly arrangement of cellulose nanocrystals of different aspect ratios. The suspension of cellulose nanocrystals with low aspect ratio and high aspect ratio is prepared by sulfuric acid hydrolysis, and the cellulose nanocrystals is carried out in the magnetic field. Ultrasonic treatment and assembly ensure the orientation uniformity of cellulose nanocrystals.
It significantly improves the photoluminescence performance of cellulose nanocrystals, enhances the luminescence intensity, and imparts the magnetic response characteristics of the material, expanding its application potential in the fields of intelligent sensing and optical anti-counterfeiting.
Smart Images

Figure CN118879307A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional composite luminescent materials, and relates to a magnetic composite bio-based luminescent material and a method for preparing the material with enhanced orientation uniformity and application thereof. Background Art
[0002] Cellulose nanocrystals are a kind of bio-based material with broad application prospects. Due to their advantages such as high aspect ratio, high specific surface area, excellent mechanical properties, biodegradability and self-assembly characteristics, cellulose nanocrystals have become a hot topic in the field of cellulose material research and have been applied in the fields of food packaging, drug delivery, optical anti-counterfeiting and stimuli-responsive devices. Cellulose nanocrystal suspensions are isotropic at low concentrations; above the critical concentration, cellulose nanocrystals self-assemble in the suspension to form a chiral nematic liquid crystal structure. After the solvent evaporates, the chiral nematic liquid crystal structure of the cellulose nanocrystal suspension can be well preserved to form a structural color photonic film. Evaporation-induced self-assembly is one of the main methods for preparing cellulose nanocrystal films, but the agglomeration effect that occurs during the assembly process usually leads to disordered orientation, which in turn causes many defects in the assembled material and reduces the photoluminescence performance, limiting its wider application. Therefore, precisely controlling the orientation arrangement of cellulose nanocrystals during the evaporation-induced self-assembly process and realizing an ordered arrangement structure at the nanoscale is the key to improving the mechanical and optical properties of cellulose nanocrystal composites and the core of fully utilizing and amplifying their performance potential.
[0003] Responsive photonic crystals have the ability to actively adjust their optical properties when subjected to external stimuli such as mechanical, electrical, magnetic and optical stimuli. Therefore, they have attracted extensive attention in basic scientific research and practical applications. Among various types of photonic crystal materials, cellulose nanocrystals have become one of the most promising candidate materials due to their reproducibility, simple preparation process and unique chiral characteristics. The fusion of photonic crystals and functional nanomaterials not only expands the functions and application scope of photonic crystals, but also provides new ideas for the development of smart sensors and photonic composites. By embedding stimulus-responsive elements in the helical structure of cellulose nanocrystals, CNC-based photonic crystal materials that are sensitive to humidity, steam, pH, solvents, temperature, light, electric fields and magnetic fields can be developed. However, there are still many challenges in the design and application of responsive materials based on cellulose nanocrystals. For example, magnetically responsive materials based on cellulose nanocrystals face the problem of reduced luminescence intensity, which limits their application in the optical field. Summary of the invention
[0004] In view of this, one of the objects of the present invention is to provide a method for preparing a magnetic composite bio-based luminescent material with uniform enhanced orientation, utilizing and developing the theory that weak magnetic field and high aspect ratio cellulose nanocrystals synergistically induce orderly arrangement of low aspect ratio cellulose nanocrystals, so as to solve the problem that magnetic response materials based on cellulose nanocrystals are faced with reduced luminescence intensity, which limits their application in the optical field. The second object of the present invention is to provide a magnetic bio-based rod-shaped particle luminescent material product prepared based on the method for preparing a magnetic composite bio-based high-intensity luminescent material with uniform orientation. The third object of the present invention is to provide the application of the magnetic bio-based rod-shaped particle luminescent material product in the fields of stimulus-responsive intelligent sensing and optical anti-counterfeiting.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation comprises the following steps:
[0007] S11, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively;
[0008] S12, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method;
[0009] S13. Preparing a magnetic film material with uniform orientation of cellulose nanocrystals: uniformly mixing the magnetic nanoparticle dispersion prepared in step S12 and the sCNC and hCNC suspensions prepared in step S11, respectively, and ultrasonically treating them, and dripping them into molds respectively; placing the molds respectively containing the sCNC and hCNC suspensions containing magnetic nanoparticles in a magnetic field, ensuring that the long axis of the mold is parallel to the direction of the magnetic field; and performing induced orientation assembly under the conditions of a uniform magnetic field with a magnetic field strength ranging from 0 to 70 mT, an assembly temperature of room temperature, and an assembly time of about 2 to 3 days to obtain sCNC magnetic film materials and hCNC magnetic film materials with uniform orientation.
[0010] A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation comprises the following steps:
[0011] S21, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively;
[0012] S22, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method;
[0013] S23. Preparation of uniformly oriented magnetic bio-based composite materials with enhanced photoluminescence performance: the magnetic nanoparticle dispersion prepared in step S22 and the hCNC suspension and sCNC suspension prepared in step S21 are uniformly mixed in a ratio of 0.2 to 0.6, and then ultrasonically treated and dripped into a mold, and the mold containing the hCNC and sCNC composite magnetic nanoparticle suspension is placed in a magnetic field to ensure that the long axis of the mold is parallel to the direction of the magnetic field, and in a uniform magnetic field with a magnetic field strength range of 0 to 70 mT, an assembly temperature of room temperature, and an assembly time of about 2 to 3 days, high aspect ratio cellulose nanocrystals hCNC are used to induce and promote the orientation arrangement of low aspect ratio cellulose nanocrystals sCNC to obtain a uniformly oriented magnetic bio-based composite material with enhanced photoluminescence performance.
[0014] A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation comprises the following steps:
[0015] S31, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively;
[0016] S32, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method;
[0017] S33. Prepare a bio-based functional integrated material with enhanced toughness, good luminescence performance and magnetic response: uniformly mix the hCNC and sCNC suspension mixture prepared in step S31, the magnetic nanoparticle dispersion and the flexible polymer solution prepared in step S32, perform ultrasonic treatment, and drip into a mold, wherein the ratio of hCNC suspension to sCNC suspension is 0.2-0.6; place the mold containing the hCNC and sCNC composite suspension containing flexible polymer and magnetic nanoparticles in a magnetic field to ensure that the long axis of the mold is parallel to the direction of the magnetic field; in a uniform magnetic field with a magnetic field strength range of 0-70 mT, an assembly temperature of room temperature and an assembly time of about 2-3 days, use high aspect ratio cellulose nanocrystals hCNC to induce and promote the orientation of low aspect ratio cellulose nanocrystals sCNC, and evaporate and assemble to obtain a bio-based functional integrated material with enhanced toughness, good luminescence performance and magnetic response.
[0018] Furthermore, in step S11, step S21 and step S31, the biomass source of low aspect ratio sCNC is one or a mixture of cotton linter, coniferous wood, bamboo fiber, corn cob or sugarcane bagasse; the biomass source of high aspect ratio hCNC is one or a mixture of ascidian and bacterial cellulose.
[0019] Furthermore, the biomass of different cellulose sources in step S11, step S21 and step S31 has high thermal stability, so the cellulose nanocrystals are prepared by sulfuric acid hydrolysis method, wherein the sulfuric acid concentration in the sulfuric acid hydrolysis method is 64-65%, the treatment temperature is 45-60°C, and the treatment time is 60-240min. After centrifugal washing and dialysis treatment, low aspect ratio sCNC with a length of 50-300nm and an aspect ratio of 15-30 or high aspect ratio hCNC with a length of 0.5-2μm and an aspect ratio of 50-100 is obtained according to the type of biomass. After concentration or dilution, the concentration of the low aspect ratio sCNC suspension is controlled to be 1±0.5wt%, and the concentration of the high aspect ratio hCNC suspension is controlled to be 0.30±0.1wt%.
[0020] Furthermore, the magnetic nanoparticles in step S12, step S22 and step S32 are superparamagnetic, paramagnetic or ferromagnetic metals and metal oxides, selected from one of the nanoparticles of Fe3O4, Fe2O3, CoFe2O4, MnFe2O4 and NiFe2O4.
[0021] Furthermore, the magnetic nanoparticles in step S12, step S22 and step S32 are superparamagnetic Fe3O4 NPs, and the preparation method thereof is a coprecipitation method, that is, ferrous chloride and ferric chloride are placed in an alkaline environment created by ammonia water or sodium hydroxide and an inert gas environment of nitrogen or argon in a molar ratio of 1:2, and carboxyl modification is performed by adding citric acid solution to obtain superparamagnetic ferroferric oxide nanoparticles (Fe3O4 NPs) with a particle size of 10 to 20 nm.
[0022] Furthermore, in step S23 and step S33, the ratio of the hCNC suspension to the sCNC suspension is 3:7.
[0023] Furthermore, in step S33, the flexible polymer is one of polyvinyl alcohol, polyester, polyether, and sodium alginate, and the mass fraction of the flexible polymer solution is 10 wt%.
[0024] A magnetic bio-based rod-shaped particle luminescent material product is prepared according to the above-mentioned method for preparing a uniformly oriented magnetic bio-based composite material.
[0025] The above-mentioned magnetic bio-based rod-shaped particle luminescent material products are used in the fields of stimulus-responsive intelligent sensing and optical anti-counterfeiting.
[0026] The beneficial effects of the present invention are:
[0027] 1. The method for preparing the uniform orientation of the magnetic composite bio-based luminescent material disclosed in the present invention is to use superparamagnetic Fe3O4 NP to enhance the magnetic susceptibility of sCNC and hCNC with the same one-dimensional rod-shaped structure but different length and aspect ratio from different cellulose sources, and to control the self-assembly conditions of the mixed suspension, adopt a weak magnetic field and Fe3O4 The strategy of NP synergistically inducing orderly arrangement of cellulose nanocrystals was developed, and a method for weak magnetic field regulation of cellulose nanocrystals to uniformly orientate was developed, which is applicable to low aspect ratio sCNC and high aspect ratio hCNC, and a magnetic film material with uniform orientation of cellulose nanocrystals was obtained; it is worth mentioning that the luminescence intensity of the luminescent film material with good sCNC orientation structure was enhanced by 14.04%; compared with short aspect ratio sCNC, weak magnetic field is easier to regulate the orientation structure of high aspect ratio hCNC, and the arrangement of hCNC under weak magnetic field is more orderly and has a wider range of order, and its orientation order parameter can reach up to 0.90; based on this characteristic, an innovative idea of high aspect ratio hCNC assisting in guiding the orderly arrangement of low aspect ratio sCNC was developed, and a magnetic luminescent material with uniform orientation and significantly enhanced luminescence intensity was assembled, and the photoluminescence performance of the material was improved by 291.4%; in addition, Fe3O4 The introduction of NPs gives the film magnetic response properties, exploring the application potential of cellulose nanocrystals in the field of magnetic stimulus response; by utilizing the co-assembly of flexible polymer chains and mixed suspensions, evaporation self-assembly is used to obtain a bio-based integrated luminescent material with enhanced toughness, good luminescence performance and magnetic response. This material has application potential in the fields of stimulus-responsive intelligent sensing and optical anti-counterfeiting.
[0028] 2. The method for preparing the uniform and enhanced orientation of magnetic composite bio-based luminescent materials disclosed in the present invention provides a weak magnetic field regulation method for bio-based rod-shaped particle uniaxial array materials, explores the feasibility of inducing orderly arrangement of cellulose nanocrystals by weak magnetic field and magnetic particles, reveals the mechanism of magnetic field regulation of cellulose nanocrystal orientation, and provides theoretical guidance for the effective induction of cellulose nanocrystal orientation by weak magnetic field; develops a method for high aspect ratio hCNC to assist in guiding the orientation of low aspect ratio sCNC under weak magnetic field, achieves significant improvement in the photoluminescence performance of magnetic luminescent films, studies the co-assembly system of cellulose nanocrystals and flexible polymers, enriches the application system of cellulose nanocrystal materials in the fields of optical anti-counterfeiting and stimulus response, and the prepared bio-based integrated materials meet the requirements of optical anti-counterfeiting, stimulus response and other application fields for the photoluminescence performance of luminescent materials.
[0029] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0031] Figure 1 (a) is an atomic force microscope image of the low aspect ratio sCNC prepared in Example 1; Figure 1 (b) is an atomic force microscope image of the high aspect ratio hCNC prepared in Example 1;
[0032] Figure 2 (a) is an atomic force microscope image of superparamagnetic Fe3O4 NP prepared in Example 1; Figure 2 (b) is the particle size distribution diagram of superparamagnetic Fe3O4 NP prepared in Example 1;
[0033] Figure 3 (a) is an atomic force microscope image of the film assembled by low aspect ratio sCNC under a weak magnetic field in Example 1; Figure 3 (b) is a comparison of the fluorescence spectra of the low aspect ratio sCNC film assembled under a weak magnetic field and the film assembled under no magnetic field in Example 1;
[0034] Figure 4 (a) is an atomic force microscope image of a high aspect ratio hCNC film assembled under a weak magnetic field in Example 1; Figure 4 (b) is an analysis diagram of the orientation order parameters of the high aspect ratio hCNC film assembled under a weak magnetic field in Example 1;
[0035] Figure 5 (a) is an atomic force microscope image of the self-assembled film induced by evaporation under a weak magnetic field in Example 2; Figure 5 (b) is a fluorescence spectrum of the film assembled under a weak magnetic field and the film assembled under no magnetic field in Example 2;
[0036] Figure 6 (a) is the fluorescence spectrum of the bio-based integrated luminescent material in Example 3 in a magnetic field environment and a non-magnetic field environment; Figure 6 (b) is the stress-strain curve of the bio-based integrated luminescent material in Example 3. DETAILED DESCRIPTION
[0037] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0038] Embodiment 1
[0039] sCNC is a low aspect ratio cellulose nanocrystal, hCNC is a high aspect ratio cellulose nanocrystal, Fe3O4 NP is a superparamagnetic iron oxide nanoparticle, and PLA is polylactic acid.
[0040] A thin film material with orderly oriented magnetic cellulose nanocrystals, the preparation method of which comprises the following steps:
[0041] S11. Preparation of cellulose nanocrystals with different aspect ratios
[0042] Using natural cotton linters as raw materials, 50 g of cotton linters were immersed in 2 L of 2 wt% NaOH solution, treated at room temperature (25°C) for 12 h, washed with distilled water until neutral, and dried in a forced air drying oven at 45°C; 12.5 g of dried alkali-treated cotton was weighed, treated with 250 mL of 64 wt% H2SO4 solution at 45°C for 60 min, washed, centrifuged, and dialyzed until neutral to obtain a low aspect ratio cellulose nanocrystal (sCNC) suspension for use, and its atomic force microscope image is shown in FIG. Figure 1 (a) shown.
[0043] Using sea squirt as cellulose source, wash the sea squirt capsule and dry it in a 55℃ oven, crush it and sieve it to obtain brown sea squirt powder; prepare 300mL of 5wt% KOH solution and add 10.0g sea squirt powder, and stir mechanically at 80℃ for 24h. Then transfer the mixed solution to a Buchner funnel, wash with distilled water until the filtrate is neutral, and then dry the filter cake in a 55℃ oven, repeat the alkali treatment operation twice; take 4.0g of alkali-treated powder, add 0.5mL CH3COOH, 1mL NaClO and 100mL distilled water, and bleach it at 60℃ with mechanical stirring (350rpm) for 1h. The mixed solution was then transferred to a Buchner funnel, washed with distilled water until the filtrate was neutral, and then the filter cake was dried in an oven at 55°C, and the bleaching operation was repeated twice; 4.0 g of bleaching powder was taken, 400 mL of distilled water was added, and then placed in a grinder, and processed at a low speed (120 r / min) for 2 min, and at a high speed (240 r / min) for 4 min. The suspension was then transferred to a beaker, 271 mL of concentrated sulfuric acid was added, mechanically stirred at 50°C (350 rpm) for 2 h, and washed with distilled water by centrifugation (5000 rpm, 5 min) until neutral, and the acid treatment operation was repeated twice. The precipitate after centrifugation was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 14,000 until the dialysate was neutral to obtain a high aspect ratio cellulose nanocrystal (hCNC) suspension. The hCNC suspension was concentrated to a concentration of 0.3 wt% by a rotary evaporator and stored at 4°C for later use. Its atomic force microscope image is as shown below. Figure 1 (b) as shown.
[0044] S12. Preparation of superparamagnetic Fe3O4 NPs
[0045] Weigh FeCl2·4H2O (1.99 g, 0.01 mol) and FeCl3·6H2O (5.41 g, 0.02 mol), add to 100 mL of distilled water, and mechanically stir (250 rpm) for 30 min under nitrogen protection and room temperature. Then, 12 mL of NH3·H2O was mixed and diluted with 6 mL of distilled water, slowly dripped into the suspension, and stirred for 30 min. Then, citric acid solution (0.75 g / mL) was added and continued to stir for 2 h. After the reaction was completed, Fe3O4 NP was centrifuged and washed with distilled water several times (10000 rpm / min, 5 min) until the supernatant was neutral. The precipitate was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 3500 until the dialyzate was neutral, and finally a superparamagnetic Fe3O4 NP dispersion was obtained. The superparamagnetic Fe3O4 NP dispersion was concentrated to 0.5 wt% by rotary evaporation. The superparamagnetic Fe3O4 NP dispersion was sonicated by a cell crusher (600 W, 20 min) and stored at 4°C for future use. Figure 2 (a) shows the particle size distribution of superparamagnetic Fe3O4 NPs. Figure 2 As shown in (b), it can be seen that the particle size of superparamagnetic Fe3O4 NPs is relatively uniform, mostly distributed in the range of 10 to 20 nm.
[0046] S13. Preparation of magnetic thin film materials with orderly oriented cellulose nanocrystals with different aspect ratios
[0047] S131. Preparation of uniformly oriented sCNC magnetic thin film materials
[0048] Take 20mL of 1.00wt% sCNC suspension and 100μL of 0.50wt% Fe3O4 NP dispersion, respectively, and mix them after ultrasonic treatment. After the plasma-cleaned glass slide is vertically inserted into the polylactic acid (PLA) mold, take 1mL of the mixed suspension after ultrasonic treatment and drop it on the glass slide of the polylactic acid (PLA) mold. Place the PLA mold in a magnetic field, ensure that the glass slide is parallel to the magnetic field direction, and perform evaporation-induced self-assembly film formation under a magnetic field strength of 50mT to obtain a uniformly oriented sCNC thin film material. The atomic force microscope image of the low aspect ratio sCNC assembled film under a weak magnetic field is shown in Figure 1. Figure 3 As shown in (a), it can be seen that the orientation of sCNC is relatively uniform. The fluorescence spectra of the low aspect ratio sCNC film assembled under a weak magnetic field and the film assembled without a magnetic field are compared as shown in Figure 3 As shown in (b), it can be seen that the luminescence intensity of the uniformly oriented magnetic luminescent material is enhanced by 14.04%.
[0049] S132. Preparation of hCNC magnetic thin film materials with uniform orientation
[0050] Take 20mL of 0.30wt% hCNC suspension and 100μL of 0.50wt% Fe3O4 NP dispersion, respectively, and mix them after ultrasonic treatment. After vertically inserting the plasma-cleaned glass slide into the polylactic acid (PLA) mold, take 1mL of the mixed suspension after ultrasonic treatment and drop it on the glass slide of the polylactic acid (PLA) mold. Place the PLA mold in a magnetic field to ensure that the glass slide is parallel to the magnetic field. Evaporation-induced self-assembly film is carried out under a magnetic field strength of 50mT to obtain a uniformly oriented hCNC thin film material. The atomic force microscope image of the high aspect ratio hCNC assembled film under a weak magnetic field is shown in Figure 2. Figure 4 As shown in (a), it can be seen that hCNC has uniform orientation. The inset in the lower left corner is the distribution angle diagram of hCNC. Under this magnetic field condition, Fe3O4 NP can effectively guide hCNC to arrange in an orderly manner along a specific direction without excessive agglomeration. Most hCNCs are distributed in the range of 140°-160°. The orientation order parameter analysis diagram of high aspect ratio hCNC assembled film under weak magnetic field is shown in Figure 4 As shown in (b), it can be seen that the hCNC orientation order parameter is as high as 0.90.
[0051] Embodiment 2
[0052] A uniformly oriented magnetic bio-based composite material of a mixture of sCNC and hCNC. The difference between Example 2 and Example 1 is that a strategy of using high aspect ratio hCNC to assist in guiding the orderly arrangement of low aspect ratio sCNC is adopted to achieve a more orderly orientation of sCNC under a weak magnetic field. The preparation method of the magnetically responsive bio-based material with significantly enhanced luminescence is as follows:
[0053] A uniformly oriented magnetic bio-based composite material with enhanced photoluminescence performance, the preparation method of which comprises the following steps:
[0054] S21. Preparation of cellulose nanocrystals with different aspect ratios
[0055] Taking natural cotton linters as raw materials, 50 g of cotton linters were immersed in 2 L of 2 wt% NaOH solution, treated at room temperature (25 ° C) for 12 h, washed with distilled water until neutral, and dried in a forced air drying oven at 45 ° C; 12.5 g of dried alkali-treated cotton was weighed, treated with 250 mL of 64 wt% H2SO4 solution at 45 ° C for 60 min, washed, centrifuged and dialyzed to neutral to obtain a low aspect ratio cellulose nanocrystal (sCNC) suspension for use.
[0056] Using sea squirt as cellulose source, wash the sea squirt capsule and dry it in a 55℃ oven, crush it and sieve it to obtain brown sea squirt powder; prepare 300mL of 5wt% KOH solution and add 10.0g sea squirt powder, and stir mechanically at 80℃ for 24h. Then transfer the mixed solution to a Buchner funnel, wash with distilled water until the filtrate is neutral, and then dry the filter cake in a 55℃ oven, repeat the alkali treatment operation twice; take 4.0g of alkali-treated powder, add 0.5mL CH3COOH, 1mL NaClO and 100mL distilled water, and bleach it at 60℃ with mechanical stirring (350rpm) for 1h. The mixed solution was then transferred to a Buchner funnel, washed with distilled water until the filtrate was neutral, and then the filter cake was dried in an oven at 55°C, and the bleaching operation was repeated twice; 4.0 g of bleached powder was taken, 400 mL of distilled water was added, and then placed in a grinder, and processed at a low speed (120 r / min) for 2 min, and at a high speed (240 r / min) for 4 min. The suspension was then transferred to a beaker, 271 mL of concentrated sulfuric acid was added, mechanically stirred at 50°C (350 rpm) for 2 h, and washed with distilled water centrifugation (5000 rpm, 5 min) until neutral, and the acid treatment operation was repeated twice. The precipitate after centrifugation was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 14,000 until the dialyzate was neutral to obtain a high aspect ratio cellulose nanocrystal (hCNC) suspension. The hCNC suspension was concentrated to a concentration of 0.3 wt% by a rotary evaporator and stored at 4°C for later use.
[0057] S22. Preparation of superparamagnetic Fe3O4 NPs
[0058] Weigh FeCl2·4H2O (1.99 g, 0.01 mol) and FeCl3·6H2O (5.41 g, 0.02 mol), add to 100 mL of distilled water, and mechanically stir (250 rpm) for 30 min under nitrogen protection and room temperature. Then, 12 mL of NH3·H2O was mixed and diluted with 6 mL of distilled water, slowly dripped into the suspension, and stirred for 30 min. Then, citric acid solution (0.75 g / mL) was added and continued to stir for 2 h. After the reaction was completed, Fe3O4 NP was centrifuged and washed with distilled water several times (10000 rpm / min, 5 min) until the supernatant was neutral. The precipitate was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 3500 until the dialyzate was neutral, and finally a superparamagnetic Fe3O4 NP dispersion was obtained. The concentration of the superparamagnetic Fe3O4 NP dispersion was concentrated to 0.5 wt% by a rotary evaporator, and the superparamagnetic Fe3O4 NP dispersion was sonicated by a cell crusher (600 W, 20 min) and stored at 4°C for future use.
[0059] S23. Preparation of uniformly oriented magnetic bio-based composite materials
[0060] Take 20 mL of the sCNC suspension with a concentration of 1.00 wt% prepared in step S21, 20 mL of the hCNC suspension with a concentration of 0.30 wt% and 1 mL of the Fe3O4 NP dispersion with a concentration of 0.50 wt% prepared in step S22, respectively, and mix them after ultrasonic treatment. After vertically inserting the plasma-cleaned glass slide into the polylactic acid (PLA) mold, take 1 mL of the mixed suspension after ultrasonic treatment and drop it into the mold, place the PLA mold in a magnetic field, ensure that the glass slide is parallel to the magnetic field direction, and perform evaporation-induced self-assembly film formation under a magnetic field intensity of 50 mT to obtain an oriented uniform magnetic bio-based composite material with enhanced photoluminescence performance. The atomic force microscope image of the oriented uniform magnetic bio-based composite film induced by evaporation under a weak magnetic field is as follows: Figure 5 As shown in (a), it can be seen that the orderly arrangement of sCNC is achieved with the assistance of high aspect ratio hCNC. The fluorescence spectra of the film assembled under a weak magnetic field and the film assembled under no magnetic field are shown in Figure 5 As shown in (b), it can be seen that the luminescence intensity of the assembled film with uniform sCNC orientation is enhanced by 291.4%. The synergistic induction of high aspect ratio cellulose nanocrystals hCNC and weak magnetic field promotes the orderly arrangement of low aspect ratio cellulose nanocrystals sCNC, further enhancing the orientation degree of sCNC in the uniformly oriented magnetic bio-based composite film, thereby greatly increasing the photoluminescence performance of the material.
[0061] Embodiment 3
[0062] A uniformly oriented magnetic bio-based composite material, the preparation method of which comprises the following steps:
[0063] S31. Preparation of cellulose nanocrystals with different aspect ratios
[0064] Taking natural cotton linters as raw materials, 50 g of cotton linters were immersed in 2 L of 2 wt% NaOH solution, treated at room temperature (25 ° C) for 12 h, washed with distilled water until neutral, and dried in a forced air drying oven at 45 ° C; 12.5 g of dried alkali-treated cotton was weighed, treated with 250 mL of 64 wt% H2SO4 solution at 45 ° C for 60 min, washed, centrifuged and dialyzed to neutral to obtain a low aspect ratio cellulose nanocrystal (sCNC) suspension for use.
[0065] Using sea squirt as cellulose source, wash the sea squirt capsule and dry it in a 55℃ oven, crush it and sieve it to obtain brown sea squirt powder; prepare 300mL of 5wt% KOH solution and add 10.0g sea squirt powder, and stir mechanically at 80℃ for 24h. Then transfer the mixed solution to a Buchner funnel, wash with distilled water until the filtrate is neutral, and then dry the filter cake in a 55℃ oven, repeat the alkali treatment operation twice; take 4.0g of alkali-treated powder, add 0.5mL CH3COOH, 1mL NaClO and 100mL distilled water, and bleach it at 60℃ with mechanical stirring (350rpm) for 1h. The mixed solution was then transferred to a Buchner funnel, washed with distilled water until the filtrate was neutral, and then the filter cake was dried in an oven at 55°C, and the bleaching operation was repeated twice; 4.0 g of bleached powder was taken, 400 mL of distilled water was added, and then placed in a grinder, and processed at a low speed (120 r / min) for 2 min, and at a high speed (240 r / min) for 4 min. The suspension was then transferred to a beaker, 271 mL of concentrated sulfuric acid was added, mechanically stirred at 50°C (350 rpm) for 2 h, and washed with distilled water centrifugation (5000 rpm, 5 min) until neutral, and the acid treatment operation was repeated twice. The precipitate after centrifugation was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 14,000 until the dialyzate was neutral to obtain a high aspect ratio cellulose nanocrystal (hCNC) suspension. The hCNC suspension was concentrated to a concentration of 0.3 wt% by a rotary evaporator and stored at 4°C for later use.
[0066] S32. Preparation of superparamagnetic Fe3O4 NPs
[0067] Weigh FeCl2·4H2O (1.99 g, 0.01 mol) and FeCl3·6H2O (5.41 g, 0.02 mol), add to 100 mL of distilled water, and mechanically stir (250 rpm) for 30 min under nitrogen protection and room temperature. Then, 12 mL of NH3·H2O was mixed and diluted with 6 mL of distilled water, slowly dripped into the suspension, and stirred for 30 min. Then, citric acid solution (0.75 g / mL) was added and continued to stir for 2 h. After the reaction was completed, Fe3O4 NP was centrifuged and washed with distilled water several times (10000 rpm / min, 5 min) until the supernatant was neutral. The precipitate was redispersed in distilled water and dialyzed in a dialysis bag with a molecular weight of 3500 until the dialyzate was neutral, and finally a superparamagnetic Fe3O4 NP dispersion was obtained. The concentration of the superparamagnetic Fe3O4 NP dispersion was concentrated to 0.5 wt% by a rotary evaporator, and the superparamagnetic Fe3O4 NP dispersion was sonicated by a cell crusher (600 W, 20 min) and stored at 4°C for future use.
[0068] S33. Preparation of bio-based integrated luminescent materials
[0069] S331. Weigh 20.0 g of polyvinyl alcohol (PVA) and add 180.0 g of distilled water. Stir mechanically (500 rpm) at 100°C until the PVA is completely dissolved. Note condensation and reflux. After the PVA is completely dissolved, transfer the 10.0 wt% PVA solution to a wire-top reagent bottle, cool it to room temperature, and store it at 4°C for later use.
[0070] S332, take 20mL of the sCNC suspension with a concentration of 1.00wt% prepared in step S31, 20mL of the hCNC suspension with a concentration of 0.30wt%, 1mL of the Fe3O4 NP dispersion with a concentration of 0.50wt% prepared in step S32, and 10mL of the PVA solution with a concentration of 10wt% prepared in the above step S331, respectively, and mix them after ultrasonic treatment. After vertically inserting the plasma-cleaned glass slide into the polylactic acid (PLA) mold, take 1mL of the mixed suspension after ultrasonic treatment and drop it into the mold, place the PLA mold in a magnetic field, ensure that the glass slide is parallel to the magnetic field direction, and perform evaporation-induced self-assembly film formation at a magnetic field strength of 50mT, and evaporation assembly obtains a bio-based functional integrated material with enhanced toughness, good luminescence performance and magnetic response.
[0071] The fluorescence spectra of the bio-based integrated luminescent material in a magnetic field environment and a non-magnetic field environment are shown in the figure below. Figure 6 As shown in (a), it can be seen that the magnetic luminescent material has magnetic response characteristics. The stress-strain curve of the bio-based integrated luminescent material is shown in Figure 6 (b) As shown. Neither sCNC nor hCNC has good toughness. Among them, the elongation at break of sCNC is only 0.60%, and the elongation at break of hCNC is 0.99%. After adding the flexible polymer PVA, the toughness of the bio-based integrated luminescent material film is significantly improved, and the elongation at break of the film reaches 444.11%, indicating that the magnetic luminescent material has excellent mechanical properties.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation, characterized in that: The steps include: S11, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively; S12, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method; S13. Preparing a magnetic film material with uniform orientation of cellulose nanocrystals: uniformly mixing the magnetic nanoparticle dispersion prepared in step S12 and the sCNC and hCNC suspensions prepared in step S11, respectively, and ultrasonically treating them, and dripping them into molds respectively; placing the molds respectively containing the sCNC and hCNC suspensions containing magnetic nanoparticles in a magnetic field, ensuring that the long axis of the mold is parallel to the direction of the magnetic field; and performing induced orientation assembly under the conditions of a uniform magnetic field with a magnetic field strength ranging from 0 to 70 mT, an assembly temperature of room temperature, and an assembly time of about 2 to 3 days to obtain sCNC magnetic film materials and hCNC magnetic film materials with uniform orientation.
2. A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation, characterized in that: The steps include: S21, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively; S22, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method; S23. Preparation of uniformly oriented magnetic bio-based composite materials with enhanced photoluminescence performance: the magnetic nanoparticle dispersion prepared in step S22 and the hCNC suspension and sCNC suspension prepared in step S21 are uniformly mixed in a ratio of 0.2 to 0.6, and then ultrasonically treated and dripped into a mold, and the mold containing the hCNC and sCNC composite magnetic nanoparticle suspension is placed in a magnetic field to ensure that the long axis of the mold is parallel to the direction of the magnetic field, and in a uniform magnetic field with a magnetic field strength range of 0 to 70 mT, an assembly temperature of room temperature, and an assembly time of about 2 to 3 days, high aspect ratio cellulose nanocrystals hCNC are used to induce and promote the orientation arrangement of low aspect ratio cellulose nanocrystals sCNC to obtain a uniformly oriented magnetic bio-based composite material with enhanced photoluminescence performance.
3. A method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation, characterized in that: The steps include: S31, preparing rod-shaped cellulose nanocrystals with different aspect ratios: treating biomass from different cellulose sources by sulfuric acid hydrolysis to obtain one-dimensional rod-shaped low aspect ratio cellulose nanocrystal (sCNC) suspension and high aspect ratio cellulose nanocrystal (hCNC) suspension for use respectively; S32, preparing magnetic nanoparticles: preparing a magnetic nanoparticle dispersion by a coprecipitation method or a hydrothermal method; S33. Prepare a bio-based functional integrated material with enhanced toughness, good luminescence performance and magnetic response: uniformly mix the hCNC and sCNC suspension mixture prepared in step S31, the magnetic nanoparticle dispersion and the flexible polymer solution prepared in step S32, perform ultrasonic treatment, and drip into a mold, wherein the ratio of hCNC suspension to sCNC suspension is 0.2-0.6; place the mold containing the hCNC and sCNC composite suspension containing flexible polymer and magnetic nanoparticles in a magnetic field to ensure that the long axis of the mold is parallel to the direction of the magnetic field; in a uniform magnetic field with a magnetic field strength range of 0-70 mT, an assembly temperature of room temperature and an assembly time of about 2-3 days, use high aspect ratio cellulose nanocrystals hCNC to induce and promote the orientation of low aspect ratio cellulose nanocrystals sCNC, and evaporate and assemble to obtain a bio-based functional integrated material with enhanced toughness, good luminescence performance and magnetic response.
4. The method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation according to any one of claims 1 to 3, characterized in that: In step S11, step S21 and step S31, the biomass source of low aspect ratio sCNC is one or a mixture of cotton linter, coniferous wood, bamboo fiber, corn cob or sugarcane bagasse; the biomass source of high aspect ratio hCNC is one or a mixture of ascidian and bacterial cellulose.
5. The method for preparing a magnetic composite bio-based luminescent material with enhanced orientation uniformity according to any one of claims 1 to 3, characterized in that: In step S11, step S21 and step S31, the biomass of different cellulose sources has high thermal stability, so the sulfuric acid hydrolysis method is used to prepare cellulose nanocrystals, wherein the sulfuric acid concentration in the sulfuric acid hydrolysis method is 64-65%, the treatment temperature is 45-60°C, and the treatment time is 60-240min. After centrifugal washing and dialysis treatment, a low aspect ratio sCNC with a length of 50-300nm and an aspect ratio of 15-30 or a high aspect ratio hCNC with a length of 0.5-2μm and an aspect ratio of 50-100 is obtained according to the type of biomass. After concentration or dilution, the concentration of the low aspect ratio sCNC suspension is controlled to be 1±0.5wt%, and the concentration of the high aspect ratio hCNC suspension is controlled to be 0.30±0.1wt%.
6. The method for uniformly preparing a magnetic composite bio-based luminescent material with enhanced orientation according to any one of claims 1 to 3, characterized in that: The magnetic nanoparticles in step S12, step S22 and step S32 are superparamagnetic, paramagnetic or ferromagnetic metals and metal oxides, selected from one of the nanoparticles of Fe3O4, Fe2O3, CoFe2O4, MnFe2O4 and NiFe2O4.
7. The method for preparing a magnetic composite bio-based luminescent material with enhanced orientation uniformity according to any one of claims 1 to 3, characterized in that: The magnetic nanoparticles in step S12, step S22 and step S32 are superparamagnetic Fe3O4 nanoparticles, which are prepared by a coprecipitation method, that is, ferrous chloride and ferric chloride in a molar ratio of 1:2 are placed in an alkaline environment created by ammonia water or sodium hydroxide and an inert gas environment of nitrogen or argon, and carboxyl modification is performed by adding citric acid solution to obtain superparamagnetic ferroferric oxide nanoparticles (Fe3O4 NP) with a particle size of 10 to 20 nm.
8. The method for preparing the magnetic composite bio-based luminescent material with enhanced orientation uniformity according to claim 3, characterized in that: In step S33, the flexible polymer is one of polyvinyl alcohol, polyester, polyether, and sodium alginate, and the mass fraction of the flexible polymer solution is 10wt%.
9. A magnetic bio-based rod-shaped particle luminescent material product prepared by the method for uniformly preparing the magnetic composite bio-based luminescent material in enhanced orientation according to claim 1.
10. Application of the magnetic bio-based rod-shaped particle luminescent material product as claimed in claim 9 in the fields of stimulus-responsive intelligent sensing and optical anti-counterfeiting.