Hesperidin-pectin graft copolymer as well as preparation method and application thereof
Grafting hesperidin onto pectin through horseradish peroxidase and H2O2 catalytic system solves the problems of insufficient biological activity and environmental pollution, and achieves efficient improvement of antioxidant activity and green modification. It is suitable for Food and medicine.
Patent Information
- Application Number
- CN202410900401.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, pectin has weak biological activity and chemical coupling methods have environmental pollution problems. The free radical mediated grafting efficiency is low. Although enzymatic grafting is economical and environmentally friendly, the grafting rate is low, and no pectin is found. Reports of graft copolymers with horseradish peroxidase method.
Hesperidin is grafted onto pectin by horseradish peroxidase (HRP) and H2O2 catalytic system, and the semiquinone free radical is formed through single electron oxidation to participate in the grafting reaction, enhancing the hydrogen or electron supply capacity of pectin. Form a hesperidin-pectin graft copolymer.
It improves the antioxidant activity of pectin and provides a green and economical modification method, suitable for food and medicine fields, and has a controllable graft rate.
Smart Images

Figure CN118879810A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of pectin modification, and in particular to a hesperidin-pectin graft copolymer and a preparation method and application thereof. Background Art
[0002] Pectin, as a natural macromolecular substance, has been widely used in food, medicine and other fields due to its advantages such as easy degradation, good compatibility and good safety. However, the weak biological activity of pectin limits its application. On the other hand, the presence of a large number of functional groups such as hydroxyl and carboxyl groups on the main chain of pectin enables it to undergo many modifications. The grafting of polyphenols and polysaccharides is considered to be one of the most attractive methods to improve the physical, chemical and functional properties of pectin.
[0003] Citrus flavonoids can be divided into flavonoids, flavanones, flavonols, flavanols and anthocyanins according to their structures. Among them, flavanones are the most abundant. Hesperidin is a typical flavanone and is widely found in citrus fruits such as oranges, oranges and lemons. my country has a large output of oranges, which are mainly eaten fresh, and a small part is processed into canned goods and juices. Orange peel is a by-product of orange processing, and about 10 million tons of orange peel are produced each year. Among them, 90% of orange peels are discarded, causing environmental pollution and waste of resources. Hesperidin has the highest content in orange peel and is of great value for extraction and utilization. Citrus flavonoids have been shown to have multiple physiological activities, including antioxidant, anti-inflammatory, neuroprotective, anti-cancer and anti-obesity activities. It is reported that the graft copolymerization of flavonoids with polysaccharides can greatly improve the solubility of flavonoids and increase its bioavailability.
[0004] So far, different grafting copolymerization methods such as chemical coupling, free radical mediation and enzyme-catalyzed synthesis have been successfully used for the covalent connection of polysaccharides and polyphenols. However, the chemical coupling method usually requires the use of a variety of chemical reagents during the reaction, which is not only expensive, but also toxic and environmentally unfriendly. The free radical-mediated grafting method is widely used because it is more economical and environmentally friendly, and can avoid the oxidation and degradation of phenolic acid during the reaction. However, the grafting efficiency of the free radical grafting method is relatively low and difficult to mass produce. Enzymatic grafting not only has the advantages of economy, environmental protection, non-toxicity and mild reaction conditions, but also has a high grafting rate of grafted copolymers after enzyme catalysis. For example, Yin Lijun et al. (2021) grafted ferulic acid with pectin through laccase catalysis to obtain copolymers with strong antioxidant activity; Yong et al. (2022) covalently grafted myricetin, quercetin and kaempferol with chitosan oligosaccharides through horseradish peroxidase catalysis, and the grafting reaction enhanced the antioxidant activity of chitosan oligosaccharides. At present, there is no report on the graft copolymer of pectin and horseradish peroxidase. Summary of the invention
[0005] Based on this, the present invention proposes a simple green preparation method, in which hesperidin is grafted onto pectin through horseradish peroxidase (HRP) and H2O2 catalytic system. The present invention provides a new idea for the copolymerization of pectin and flavonoid polyphenols. In addition, the microstructure, thermal stability and antioxidant properties of the pectin-hesperidin graft copolymer prepared by the method are evaluated, providing a basis for its application in the food or medical fields.
[0006] Part I:
[0007] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0008] dissolving and mixing pectin and hesperidin to obtain a pectin-hesperidin mixed solution;
[0009] The pectin-hesperidin mixed solution is mixed with horseradish peroxidase (HRP) and H2O2 to carry out graft copolymerization reaction to obtain a hesperidin-pectin graft copolymer.
[0010] The invention provides a method for preparing a pectin graft copolymer, comprising mixing pectin, hesperidin and a solvent to obtain a mixed solution; mixing the mixed solution with HRP in a water bath to obtain a mixed solution, and mixing a H2O2 solution with the mixed solution to perform a graft copolymerization reaction to obtain a hesperidin-pectin graft copolymer. The invention combines an enzyme catalytic system (HRP and H2O2) with graft modification, and uses hesperidin pectin for graft copolymerization. During the graft copolymerization process, under the action of H2O2, HRP can oxidize hesperidin into a semiquinone free radical through a single electron, participate in the graft reaction, and connect with the hydroxyl group on the pectin chain and a hydrogen bond to form a graft copolymer, thereby enhancing the hydrogen or electron supply capacity of pectin, thereby increasing the antioxidant activity of pectin.
[0011] As a preferred embodiment, the mass ratio of the pectin to the hesperidin is 1:(0.1-0.5).
[0012] As a preferred embodiment, the pectin is citrus pectin.
[0013] As a preferred embodiment, the pectin is dissolved in a phosphate buffer with a pH of 6-7; and the hesperidin is dissolved in methanol.
[0014] As a preferred embodiment, in the pectin-hesperidin mixed solution, the added amount of horseradish peroxidase (HRP) is 0.005-0.05 g / L, and the added amount of H2O2 is 5-15 mol / L.
[0015] As a preferred embodiment, the temperature of the graft copolymerization reaction is 30-50° C., and the reaction time is 1-5 h.
[0016] As a preferred embodiment, the preparation method further comprises, after the graft copolymerization reaction is completed, sequentially subjecting the hesperidin-pectin graft copolymer to alcohol precipitation, suction filtration, rotary evaporation, centrifugation, dialysis and drying to obtain a pure hesperidin-pectin graft copolymer;
[0017] The alcohol precipitation is carried out with ethanol, and the volume of the ethanol is 4 times that of the hesperidin-pectin graft copolymer. The filtration is vacuum filtration, the rotary evaporation condition is 40°C, the centrifugation condition is 10000rpm, 20min, the dialysis is carried out with distilled water, the molecular weight cutoff is not more than 14kDa, the time is 48h, during which the water is changed every 24h, the drying is freeze-drying, the freeze-drying temperature is -40 to 30°C, and the time is 31 to 40h.
[0018] Part II:
[0019] A hesperidin-pectin graft copolymer prepared by the preparation method described in the first part, wherein the grafting rate of pectin is 30-650 mg / g.
[0020] Part III:
[0021] An application of the hesperidin-pectin graft copolymer described in the second part in food, health products or medicines. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is the Fourier transform infrared spectra of citrus pectin and hesperidin-pectin copolymer in Example 5;
[0023] Figure 2 is the H NMR spectrum of citrus pectin and hesperidin-pectin copolymer in Example 5;
[0024] Figure 3 is a scanning electron micrograph of citrus pectin, hesperidin and hesperidin-pectin copolymer in Example 5;
[0025] Figure 4 The thermogravimetric diagrams of citrus pectin, hesperidin and hesperidin-pectin copolymer in Example 5. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing a hesperidin-pectin graft copolymer, comprising the following steps:
[0027] Pectin is dissolved in a phosphate buffer with a pH of 6-7 to form a pectin solution, hesperidin is dissolved in methanol and ultrasonicated to form a hesperidin solution, and after the pectin and hesperidin are completely dissolved, the hesperidin solution is evenly dispersed in the pectin solution to obtain a pectin-hesperidin mixed solution, wherein the mass ratio of pectin to hesperidin is preferably 1:(0.1-0.5), more preferably 1:(0.15-0.25), and further preferably 1:0.2; the pectin is preferably citrus pectin, and commercially available citrus pectin or self-extracted citrus pectin can be used.
[0028] HRP and H2O2 are added to the pectin-hesperidin mixed solution, and the mixture is mixed and grafted copolymerized in a water bath to obtain a hesperidin-pectin grafted copolymer. The reaction temperature is preferably 30-50°C, more preferably 30-40°C, and further preferably 40°C; the reaction time is preferably 1-5h, more preferably 2.5-3.5h, and further preferably 2.5h; in the grafting reaction system, the concentration of HRP is 0.005-0.05g / L, preferably 0.01g / L, and the concentration of H2O2 is 5-15mol / L, and preferably 10mol / L.
[0029] After the graft copolymerization reaction is completed, the method further includes sequentially subjecting the hesperidin-pectin graft copolymer to alcohol precipitation, suction filtration, rotary evaporation, centrifugation, dialysis and drying to obtain a pure hesperidin-pectin graft copolymer; the alcohol precipitation is carried out with ethanol, the ethanol is 4 times the volume of the hesperidin-pectin graft copolymer, the suction filtration is vacuum filtration, the rotary evaporation condition is preferably 40° C., the centrifugation condition is 10000 rpm, 20 min, the dialysis is carried out with distilled water, the molecular weight cutoff is not more than 14 kDa, the time is 48 hours, the water is changed every 24 hours during the period, the drying is freeze drying, the freeze drying temperature is -40 to 30° C., and the time is 31 to 40 hours.
[0030] In the hesperidin-pectin graft copolymer prepared by the present invention, the grafting rate of pectin is 30-650 mg / g and can be applied to food, health products or medicines.
[0031] Example 1
[0032] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0033] Accurately weigh 1g of citrus pectin and completely dissolve it in 90mL of pH 6.5 phosphate buffer to obtain a pectin solution; then dissolve 0.1g of hesperidin in 10mL of methanol and ultrasonicate for 5min to obtain a hesperidin solution; add the completely dissolved hesperidin solution to the pectin solution and stir evenly. Add 1mg of HRP and H2O2 in a 30℃ water bath, and control the concentration of H2O2 in the reaction system to 10mol / L, and react for 3h.
[0034] After the reaction, add 4 times the volume of the reaction system of anhydrous ethanol, and then use a vacuum pump to filter twice. The filtrate is rotary evaporated at 40 ° C to obtain a concentrated solution, and centrifuged at 10000r / min for 20 minutes. The supernatant is placed in a dialysis bag with a molecular weight cutoff of 14kDa and dialyzed with distilled water for 48 hours, and the water is changed every 24 hours. Finally, the obtained solution is freeze-dried at 0 ° C for 37 hours to obtain the hesperidin-pectin graft copolymer.
[0035] Example 2
[0036] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0037] Accurately weigh 1g of citrus pectin and completely dissolve it in 90mL of pH 6 phosphate buffer to obtain a pectin solution; then dissolve 0.2g of hesperidin in 10mL of methanol and ultrasonicate for 5min to obtain a hesperidin solution; add the completely dissolved hesperidin solution to the pectin solution and stir evenly. Add 5mg of HRP and H2O2 in a 30℃ water bath, and control the concentration of H2O2 in the reaction system to 5mol / L, and react for 3h.
[0038] After the reaction, add anhydrous ethanol 4 times the volume of the reaction system, and then filter twice with a vacuum pump. The filtrate is rotary evaporated at 40°C to obtain a concentrated solution, and centrifuged at 10000r / min for 20min. The supernatant is placed in a dialysis bag with a molecular weight cutoff of 14kDa and dialyzed with distilled water for 48h, with the water changed every 24h. Finally, the obtained solution is freeze-dried at -20°C for 30h to obtain the hesperidin-pectin graft copolymer.
[0039] Example 3
[0040] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0041] Accurately weigh 1g of citrus pectin and completely dissolve it in 90mL of pH 7 phosphate buffer to obtain a pectin solution; then dissolve 0.3g of hesperidin in 10mL of methanol and ultrasonicate for 5min to obtain a hesperidin solution; add the completely dissolved hesperidin solution to the pectin solution and stir evenly. Add 3mg of HRP and H2O2 in a 30℃ water bath, and control the concentration of H2O2 in the reaction system to 8mol / L for 3h.
[0042] After the reaction, add 4 times the volume of the reaction system of anhydrous ethanol, and then use a vacuum pump to filter twice. The filtrate is rotary evaporated at 40 ° C to obtain a concentrated solution, and centrifuged at 10000r / min for 20 minutes. The supernatant is placed in a dialysis bag with a molecular weight cutoff of 14kDa and dialyzed with distilled water for 48 hours, and the water is changed every 24 hours. Finally, the obtained solution is freeze-dried at -40 ° C for 35 hours to obtain the hesperidin-pectin graft copolymer.
[0043] Example 4
[0044] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0045] Accurately weigh 1g of citrus pectin and completely dissolve it in 90mL of pH 6.5 phosphate buffer to obtain a pectin solution; then dissolve 0.1g of hesperidin in 10mL of methanol and ultrasonicate for 5min to obtain a hesperidin solution; add the completely dissolved hesperidin solution to the pectin solution and stir evenly. Add 0.5mg of HRP and H2O2 in a 40℃ water bath, and control the concentration of H2O2 in the reaction system to 15mol / L, and react for 3h.
[0046] After the reaction, add anhydrous ethanol 4 times the volume of the reaction system, and then filter twice with a vacuum pump. The filtrate is rotary evaporated at 40°C to obtain a concentrated solution, and centrifuged at 10000r / min for 20min. The supernatant is placed in a dialysis bag with a molecular weight cutoff of 14kDa and dialyzed with distilled water for 48h, with the water changed every 24h. Finally, the obtained solution is freeze-dried at 30°C for 40h to obtain the hesperidin-pectin graft copolymer.
[0047] Example 5
[0048] A method for preparing a hesperidin-pectin graft copolymer comprises the following steps:
[0049] Accurately weigh 1g of citrus pectin and completely dissolve it in 90mL of pH 6 phosphate buffer to obtain a pectin solution; then dissolve 0.1g of hesperidin in 10mL of methanol and ultrasonicate for 5min to obtain a hesperidin solution; add the completely dissolved hesperidin solution to the pectin solution and stir evenly. Add 0.8mg of HRP and H2O2 in a 30℃ water bath, and control the concentration of H2O2 in the reaction system to 12mol / L, and react for 5h.
[0050] After the reaction, add 4 times the volume of the reaction system of anhydrous ethanol, and then use a vacuum pump to filter twice. The filtrate is rotary evaporated at 40 ° C to obtain a concentrated solution, and centrifuged at 10000r / min for 20 minutes. The supernatant is placed in a dialysis bag with a molecular weight cutoff of 14kDa and dialyzed with distilled water for 48 hours, and the water is changed every 24 hours. Finally, the obtained solution is freeze-dried at 0 ° C for 33 hours to obtain the hesperidin-pectin graft copolymer.
[0051] The obtained hesperidin-pectin graft copolymer and citrus pectin were analyzed by Fourier transform infrared spectroscopy and hydrogen nuclear magnetic resonance, and the hesperidin-pectin graft copolymer, citrus pectin and hesperidin were analyzed by scanning electron microscopy and thermogravimetric analysis.
[0052] Depend on Figure 1 It can be seen that the pectin-hesperidin graft copolymer is at 1520 cm -1 Compared with citrus pectin, a new peak appears, and this peak is a characteristic peak of the aromatic ring of hesperidin, thus proving that hesperidin has been successfully grafted onto pectin. Figure 2 Compared with citrus pectin, new hydrogen signals appeared in the mesopectin-hesperidin grafted copolymer, which also verified the successful occurrence of the grafting reaction. Figure 3 It can be seen that compared with citrus pectin and hesperidin, the surface structure of hesperidin-pectin graft copolymer is denser and smoother. Figure 4 It can be seen that compared with citrus pectin and hesperidin, the thermal stability of hesperidin-pectin graft copolymer is significantly enhanced.
[0053] Example 6
[0054] The grafting rates of the hesperidin-pectin graft copolymers prepared in Examples 1 to 5 were measured.
[0055] Determination of grafting rate of grafted complex: The grafting rate of the sample was determined according to the Folin-Ciocalteu method. 1 mL of 0.1 mg / mL hesperidin-pectin graft copolymer solution (solvent is dimethyl sulfoxide) was reacted with 1 mL of Folin phenol reagent (10 times diluted) at 30°C in the dark for 5 minutes. Then 5 mL of saturated sodium carbonate solution was added and reacted at 30°C in the dark for 2 hours. Finally, the absorbance of the reaction mixture was measured at 760 nm. The grafting rate of the grafted complex was calculated based on the hesperidin standard curve, and the results were expressed in milligrams of hesperidin equivalents contained in each gram of grafted complex (mg / g). The results are shown in Table 1.
[0056] Table 1 Grafting rate of hesperidin-pectin graft copolymers prepared in Examples 1 to 5
[0057] Example Grafting rate (mg / g) 1 73.39±2.49 2 141.02±4.32 3 96.42±2.49 4 79.15±4.98 5 178.43±6.59
[0058] It can be seen from Table 1 that the grafting rate can be changed by changing the amount of hesperidin added, the reaction temperature and the reaction time. The lowest is 73.39 mg / g and the highest is 178.43 mg / g, which shows that the grafting rate of hesperidin-pectin graft copolymer is controllable.
[0059] Example 7
[0060] The antioxidant activity of the hesperidin-pectin graft copolymers prepared in Examples 1 to 5 was tested, and the antioxidant activity was tested by DPPH free radical scavenging ability, hydroxyl free radical scavenging ability and reducing ability, respectively. The specific test method is as follows (in the following method, unless otherwise specified, the solvents in the sample solution and the reagent solution are distilled water):
[0061] Hydroxyl radical scavenging ability: accurately prepare 1.0 mg / mL hesperidin-pectin graft copolymer and Vc solution, and perform gradient dilution (0.2, 0.4, 0.6, 0.8 mg / mL). Add 1 mL of 9 mmol / L FeSO4 solution to the test tube, then add 1 mL of 9 mmol / L salicylic acid-ethanol solution, shake well, add 1 mL of sample solution of different concentrations, and finally add 1 mL of 8.8 mmol / L H2O2 solution to mix, let stand in a 37°C constant temperature water bath for 30 minutes, cool to room temperature, measure the absorbance at a wavelength of 510 nm, and use Vc as a positive control. The scavenging rate calculation formula for hydroxyl radicals is obtained:
[0062] Hydroxyl radical scavenging rate (%) = {1-(A3-A2) / A1}×100%
[0063] Where A1 is the absorbance of the sample solution replaced by distilled water;
[0064] A2 is the absorbance of the solution with distilled water instead of H2O2;
[0065] A3 is the absorbance of the sample solution.
[0066] DPPH free radical scavenging ability: accurately prepare 1.0 mg / mL hesperidin-pectin graft copolymer and Vc solution, and perform gradient dilution (0.2, 0.4, 0.6, 0.8 mg / mL). Take 2 mL of sample solution and 2 mL of 0.04 mg / mL DPPH reserve solution (DPPH reagent as solute, anhydrous ethanol as solvent), shake well, react at room temperature in dark conditions for 30 minutes, and measure the absorbance at a wavelength of 517 nm, with Vc as a positive control. The calculation formula for the scavenging rate of the sample solution for DPPH free radicals is obtained:
[0067] DPPH free radical scavenging rate (%) = {1-(A1-A3) / A2} × 100%
[0068] Wherein, A1 is the absorbance of the sample solution;
[0069] A2 is the absorbance of the sample solution replaced by anhydrous ethanol;
[0070] A3 is the absorbance of the DPPH stock solution replaced by anhydrous ethanol.
[0071] Reducing power: accurately prepare 1.0mg / mL hesperidin-pectin graft copolymer and Vc solution, and perform gradient dilution (0.2, 0.4, 0.6, 0.8mg / mL). Take 0.5mL of sample solution, 1% potassium ferricyanide solution and phosphate buffer solution (0.2mol / L, pH=6.7) respectively, add them into the test tube and mix them evenly. After standing for 20 minutes in a 50℃ constant temperature water bath, quickly cool and add 0.5mL 10% trichloroacetic acid solution. At the same time, absorb 0.5mL 0.1% FeCl3 solution and 2.0mL distilled water, shake well, stand at room temperature for 10 minutes, and measure the absorbance at a wavelength of 700mm. Vc is used as a positive control. The reducing power is proportional to the absorbance of the solution.
[0072] The test results of hydroxyl radical scavenging ability, DPPH radical scavenging ability and reducing ability are shown in Table 2:
[0073] Table 2 Antioxidant activity test results (1.0 mg / mL)
[0074]
[0075] From the data in Table 2, it can be seen that the antioxidant activity of hesperidin-pectin graft copolymer is significantly improved compared with untreated pectin. The hydroxyl radical scavenging rate is increased from 32.39±0.11% to 45.97±0.29%, the DPPH radical scavenging rate is increased from 11.50±0.35% to 70.24±0.34, and the reducing power is increased from 0.037±0.001 to 0.782±0.037. It can be seen that grafting hesperidin onto pectin can significantly improve the antioxidant activity of pectin, and the higher the grafting rate, the stronger the antioxidant activity.
[0076] Example 8
[0077] Effects of reactant ratio, reaction temperature and reaction time on the grafting rate of hesperidin-pectin graft copolymer
[0078] (1) Ratio of reactants
[0079] The effect of different reactant mass ratios (pectin: hesperidin) on the grafting rate of hesperidin-pectin graft copolymer was investigated. The reaction temperature was fixed at 30°C and the reaction time was 3h. The other steps were exactly the same as in Example 1. The results are shown in Table 3.
[0080] Table 3 Effect of reactant ratio on grafting rate of hesperidin-pectin graft copolymer
[0081]
[0082]
[0083] (2) Reaction temperature
[0084] The effect of different reaction temperatures on the grafting rate of hesperidin-pectin graft copolymer was investigated. The reactant ratio was fixed, the reaction time was 3 h, and the other steps were exactly the same as in Example 1. The results are shown in Table 4.
[0085] Table 4 Effect of reaction temperature on grafting rate of hesperidin-pectin graft copolymer
[0086] Reaction temperature (℃) Grafting rate (mg / g) 30 56.13±2.49 35 102.17±4.32 40 79.15±4.98 45 43.18±2.49 50 30.23±4.98
[0087] (3) Response time
[0088] The effect of different reaction times on the grafting rate of hesperidin-pectin graft copolymer was investigated. The reactant ratio was fixed, the reaction temperature was 30° C., and the other steps were exactly the same as in Example 1. The results are shown in Table 5.
[0089] Table 5 Effect of reaction time on grafting rate of hesperidin-pectin graft copolymer
[0090] Reaction time (h) Grafting rate (mg / g) 30 56.13±2.49 35 102.17±4.32 40 79.15±4.98 45 43.18±2.49 50 30.23±4.98
[0091] (4) Orthogonal experiment
[0092] Select three influencing factors, namely, the mass ratio of reactants A, the reaction temperature B and the reaction time C, and conduct L9(3 3 ) orthogonal test, the remaining steps are exactly the same as in Example 1, and the results are shown in Tables 7 to 8.
[0093] Table 6 Orthogonal test factors and levels
[0094]
[0095] Table 7 Orthogonal test results
[0096]
[0097]
[0098] Table 8 Results of three-factor variance analysis
[0099]
[0100] According to the results in Table 7, it can be seen that the order of factors affecting the grafting rate of hesperidin-citrus pectin graft copolymer is C>B>A.
[0101] As shown in Table 8, the three-factor variance analysis was used to study the effect of hesperidin addition, reaction temperature and reaction time on the grafting rate. It can be seen from the above table that the amount of hesperidin, reaction temperature and reaction time did not show significant difference (p>0.05, R 2 =0.909), indicating that the above factors have different effects on the grafting rate.
[0102] Based on the results of range analysis and variance analysis, it can be concluded that the best synthesis scheme is 0.2g of hesperidin, the reaction temperature is 40℃, and the reaction time is 2.5h. Therefore, the optimal combination is A2B3C1, and the grafting rate is 608.25±20.58mg / g.
[0103] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. For ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a hesperidin-pectin graft copolymer, It is characterized in that The steps include: dissolving and mixing pectin and hesperidin to obtain a pectin-hesperidin mixed solution; The pectin-hesperidin mixed solution was mixed with horseradish peroxidase (HRP), H 2 O 2 The mixture is mixed and subjected to graft copolymerization reaction to obtain a hesperidin-pectin graft copolymer.
2. A method for preparing a hesperidin-pectin graft copolymer according to claim 1, It is characterized in that The mass ratio of the pectin to the hesperidin is 1:(0.1-0.5).
3. A method for preparing a hesperidin-pectin graft copolymer according to claim 2, It is characterized in that The pectin is citrus pectin.
4. The method for preparing a hesperidin-pectin graft copolymer according to claim 1, It is characterized in that The pectin is dissolved in a phosphate buffer with a pH of 6-7; and the hesperidin is dissolved in methanol.
5. The method for preparing a hesperidin-pectin graft copolymer according to claim 1, It is characterized in that In the pectin-hesperidin mixed solution, the added amount of horseradish peroxidase (HRP) is 0.005-0.05 g / L. 2 O 2 The amount added is 5~15mol / L.
6. The method for preparing a hesperidin-pectin graft copolymer according to claim 1, It is characterized in that The temperature of the graft copolymerization reaction is 30-50° C., and the reaction time is 1-5 hours.
7. The method for preparing a hesperidin-pectin graft copolymer according to claim 1, It is characterized in that The preparation method further comprises, after the graft copolymerization reaction is completed, sequentially subjecting the hesperidin-pectin graft copolymer to alcohol precipitation, suction filtration, rotary evaporation, centrifugation, dialysis and drying to obtain a pure hesperidin-pectin graft copolymer; The alcohol precipitation is carried out with ethanol, and the volume of the ethanol is 4 times that of the hesperidin-pectin graft copolymer. The filtration is vacuum filtration, the rotary evaporation condition is 40°C, the centrifugation condition is 10000rpm, 20min, the dialysis is carried out with distilled water, the molecular weight cutoff is not more than 14kDa, the time is 48h, during which the water is changed every 24h, the drying is freeze-drying, the freeze-drying temperature is -40 to 30°C, and the time is 31 to 40h.
8. A hesperidin-pectin graft copolymer prepared by the preparation method according to any one of claims 1 to 7, It is characterized in that The grafting rate of pectin is 30-650 mg / g.
9. Use of the hesperidin-pectin graft copolymer according to claim 8 in food, health products or medicines.