Low-phosphorus converter smelting method for improving electric conductivity of wire rod for copper-clad steel wire, preparation method and produced wire rod
By using low-phosphorus converter smelting method and vacuum refining process in the smelting process of copper-clad steel wire, combined with the use of synthetic slag, the content and inclusions of impurities are controlled, and the problems of low conductivity and poor pulling performance in the prior art are solved. , the preparation of copper-clad steel wire strips with high conductivity and good drawing performance has been achieved.
Patent Information
- Application Number
- CN202410968904.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively control the content of impurity elements such as phosphorus, sulfur, oxygen, etc. during the smelting process of copper-clad steel wire, resulting in low conductivity and poor pulling performance. The high-temperature and slow-cooling process leads to coarse grains, affecting the conductivity. .
The low-phosphorus converter smelting method is adopted to control the carbon and oxygen content when the steel is discharged by the converter, combined with the use of lime, fluorite and calcium aluminosilicate ternary slag, dephosphorization is carried out, and optimized in vacuum refining and continuous casting processes. , control the impurity element content and inclusion type in molten steel, reduce oxygen content, and improve the rolling process to improve conductivity and pulling performance.
The preparation of copper-clad steel wire with ultra-low phosphorus and low impurity elements is realized, the conductivity and drawing performance are improved, the wire breaking rate is reduced, and the high-purity copper-clad steel wire strips are obtained.
Smart Images

Figure CN118879969A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-phosphorus converter smelting method for improving the conductivity of a wire rod for copper-clad steel wire, a preparation method and the produced wire rod, belonging to the technical field of metallurgy. Background Art
[0002] Copper clad steel is a metal composite material made of high-purity steel as the core, by copper plating, cladding or composite method. It has the characteristics of high conduction efficiency, low cost, high strength, corrosion resistance and wear resistance. It is an ideal alternative material to copper wire and has been widely used in telecommunications, electronics, public utilities, military and other fields.
[0003] Electrical conductivity is the primary indicator for measuring the quality of copper-clad steel wire. Under the condition of a certain copper layer conductivity, the higher the conductivity of the steel wire, the higher the conductivity of the copper-clad steel. It is also possible to reduce the thickness of the copper layer by increasing the conductivity of the steel wire, thereby reducing production costs while ensuring the performance of the copper-clad steel.
[0004] When producing copper-clad steel wire, it is found that the conductivity of a single element is the highest, so any alloy or impurity will reduce the conductivity. That is, to produce high-conductivity copper-clad steel, it is necessary to strictly control elements such as P, S, Cr, Cu, and Mo, and at the same time, conventional alloy elements such as C, Al, Si, and Mn also require very low contents, so its preparation is very difficult.
[0005] In the prior art, the patent with publication number CN106834591B provides a copper-clad steel smelting method, but the method cancels the hot metal desulfurization pretreatment and vacuum refining, and the sulfur content is difficult to control at an ultra-low S level, which increases the content of sulfide inclusions in the steel, reduces the plasticity and toughness of the steel, and has an adverse effect on the mechanical properties of the wire rod; in addition, the method produces high-basicity slag during the LF refining process, and the slag basicity is 8.0-12.0, which easily causes the high-melting-point brittle inclusions in the steel to exceed the standard, increasing the wire breakage rate of the wire rod drawing, and at the same time, due to the cancellation of KR desulfurization, RH vacuum treatment and other links, the overall control level of S, O, N and inclusions is poor, and high-conductivity copper-clad steel cannot be obtained. The patent with publication number CN107675068A provides a production method for steel wire rods for ultra-fine copper-clad steel wires, but in the smelting stage, the converter tapping temperature is extremely high, which is not conducive to dephosphorization, and at the same time, it is very harmful to the furnace body. Secondly, a large amount of aluminum shot or 70Ti is added for deoxidation after RH decarburization, and the total oxygen is removed to below 15ppm. The residual Al and Ti content in the molten steel is high, and the inclusions are mainly high-melting-point brittle inclusions such as aluminum oxide and titanium oxide, which have a great impact on the drawing performance. In addition, the content of impurity elements such as P, S, Mn, and N is also high overall, which has a great impact on the conductivity. In addition, the patent with publication number CN113857254A provides a production method for extremely low carbon steel wire rods for copper-clad steel conductors, but the content of impurity elements C, Si, Mn, P, and S is generally high, which has a great impact on the quality and conductivity of the wire rod. In addition, during the refining and spinning process, the temperature is controlled above 950°C, and the insulation cover is completely closed, and the fan is completely closed. Continuous high temperature and slow cooling may cause problems such as coarse grains, which will reduce the conductivity of the wire rod and the product.
[0006] Obviously, in order to prepare high-conductivity copper-clad steel with ultra-low carbon and extremely low alloy element content, controlling its oxygen content is one of the key technical difficulties; at the same time, ultra-low P, ultra-low S and extremely low impurity element content are required, and dephosphorization, desulfurization and raw and auxiliary material control are also very difficult; in addition, due to its overall high oxygen content, how to control the bubble problem of the ingot and the quality of the wire rod is also a control difficulty in the preparation of copper-clad steel. Summary of the invention
[0007] The present invention provides a low-phosphorus converter smelting method, a preparation method and the produced wire rod for improving the conductivity of copper-clad steel wire. The electrical conductivity of the copper-clad steel wire is improved and the wire breakage rate of the wire rod drawing is reduced through comprehensive design of steelmaking, continuous casting and rolling processes.
[0008] The technical solution adopted by the present invention to solve its technical problem is:
[0009] A low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire wire rods, wherein during converter smelting, the carbon content of converter steel is 0.025-0.055%, the oxygen content is 0.050-0.085%, P is less than or equal to 0.012%, and the steel tapping temperature is greater than or equal to 1620°C;
[0010] If the P of the tapped steel is ≤ 0.0060%, then lime, fluorite and calcium aluminosilicate ternary synthetic slag are directly added to the ladle;
[0011] If the P of the steel is greater than 0.0060%, dephosphorization treatment is continued during the steel tapping process. After the slag is cleaned, lime, fluorite and calcium aluminosilicate ternary synthetic slag are added;
[0012] As a further preferred embodiment of the present invention,
[0013] If P of converter steel is ≤0.0060%, 4.0-5.0kg / t of lime, 0.8-1.3kg / t of fluorite and 6.0-8.0kg / t of calcium silicate ternary synthetic slag are added into the ladle when 65-75% of converter steel is tapped. The bottom blowing flow rate of the ladle during tapping is 600-800NL / min. After tapping, the steel is transported to LF for heating.
[0014] As a further preferred embodiment of the present invention,
[0015] If the P of the converter steel is greater than 0.0060%, dephosphorization treatment is performed during the steel tapping process. The specific steps are:
[0016] Step 1: When 10% of the steel is tapped from the converter, fine lime and iron oxide powder are added to the ladle slag;
[0017] Among them, the amount of fine lime added is 3.0-4.0kg / t, the particle size of 1-5mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 10mm, the CaO content is ≥95%, and other unavoidable impurities; the amount of iron oxide powder added is 1.0-2.0kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 15mm, and the Fe oxide accounts for ≥80%;
[0018] Step 2: During the steel tapping process, the ladle bottom blowing flow rate is 600-800NL / min, and after the steel tapping is completed, it is set to 800-1000NL / min. After stirring for 3-5 minutes, the bottom blowing of argon is stopped, and slag removal is started. The slag removal rate is ≥90%, and the P content of the molten steel is ≤0.005%;
[0019] Step 3, adding lime, fluorite and calcium aluminosilicate ternary synthetic slag, the main components of calcium aluminosilicate ternary synthetic slag are CaO 50-55%, Al2O3 20-25%, SiO2 15-20%, MgO 3-5% and other inevitable components, among which 2CaO·Al2O3·SiO2 phase accounts for ≥80%, and then transporting to LF for refining and heating;
[0021] A method for preparing a wire rod for high-conductivity copper-clad steel wire comprises the following steps:
[0022] Step S1: Production preparation, a number of ladles are numbered from short to long according to their ages, and ladles numbered 1-20 are selected for desulfurization treatment;
[0023] The tapping holes used in the converter are numbered in sequence according to the order of use, and the tapping holes numbered 3-20 are selected; before the converter smelts copper-clad steel, ensure that the converter completes the smelting of at least two batches of ultra-low phosphorus and ultra-low sulfur steel grades, and after the smelting is completed, the slag is removed cleanly, and no slag splashing furnace protection operation is performed;
[0024] Before copper-clad steel is smelted in the converter, a furnace of boiling molten steel is used to clean and heat the vacuum chamber, and the cycle treatment is continued for 10-20 minutes;
[0025] LF refining bag covers, RH vacuum tank covers, and VD / VOD vacuum tank covers are all cleaned;
[0026] Prepare unused carbon-free ladles;
[0027] Prepare low carbon refractory and mold slag for continuous casting process;
[0028] Step S2: pre-treating the molten iron, performing deep desulfurization treatment on the molten iron, and forming desulfurization slag with sulfur elements in the molten iron;
[0029] Step S3: adopting the low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire wire rod, adding the molten iron from which the desulfurization slag is removed in step S2 into the converter and adding high-quality scrap steel for smelting;
[0030] Step S4: LF refining, LF refining is powered on and heated quickly to raise the temperature of the molten steel transported from the converter to greater than or equal to 1620°C;
[0031] Step S5: Vacuum refining, set the vacuum chamber working pressure ≤ 100Pa, decarburize for 15 minutes, add metal aluminum for deoxidation,
[0032] Among them, the amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel ,
[0033] M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of decarburization in the vacuum chamber, %; m O RH is the target oxygen content of molten steel, %; M steel is the weight of molten steel, kg; a is the oxygen supply coefficient of molten steel considering the influence of slag, vacuum tank wall and cold steel, 1.35-1.55;
[0034] After decarburization and deoxidation, the steel is discharged and transported to continuous casting;
[0035] Step S6: continuous casting of large square billets, setting the continuous casting section to 300 mm×390 mm, and adopting a strong cooling process;
[0036] Step S7: Opening and grinding, setting the heating furnace temperature and the opening temperature, dephosphorizing the surface of the ingot before opening, cleaning it and sending it to the heating furnace for the first heating. After the first heating is completed, the ingot is opened to obtain the ingot, and the ingot is subjected to magnetic particle inspection. According to the inspection results, local grinding is performed to ensure that there are no obvious defects on the surface, and then the ingot is sent to the heating furnace for the second heating to obtain a small square billet for preparing wire rod;
[0037] Step S8: high-speed wire rolling, setting the rolling start temperature and the wire laying temperature, performing controlled cooling on the Stelmor cooling line, presetting the Stelmor cooling line fan switch and air volume, and the number of insulation cover switches, performing slow cooling, and controlling the wire rod strength;
[0038] Step S9: Packing and transportation, the packing wire and the wire rod are separated by soft wear-resistant materials and wide packing tape is used.
[0040] Set the width to 3-5cm and the binding pressure to 20-40MPa;
[0041] As a further preferred embodiment of the present invention,
[0042] In step S1, after the ladle is charged with iron into the converter each time, the ladle is hoisted into the cleaning position, turned over, and the residue in the ladle is cleaned with a high-pressure air gun, and the nodules at the ladle mouth are cleaned with a bag unpacker;
[0043] Before the converter smelting copper clad steel operation, tap 2-3 furnaces continuously and clean the steel and slag at the tapping port;
[0044] The converter continuously smelts at least two batches of steel with P≤0.012% and S≤0.005%. After the converter smelting is completed, all the excess steel and slag shall be completely removed;
[0045] The prepared unused carbon-free ladle has a C content of ≤1.5%, a baking time of ≥30 hours, and a temperature of ≥1250°C;
[0046] The prepared low-carbon refractory materials include RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting. Among them, the C content of RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting is ≤10%;
[0047] The C content of mold slag is ≤2%;
[0048] As a further preferred embodiment of the present invention,
[0049] In step S2, during the pretreatment of molten iron, the elements in the incoming molten iron include C 4.2-4.5%, Si 0.20-0.65%, Mn≤0.30%, P≤0.10%, S≤0.050%, and Fe and other inevitable components, and the temperature is ≥1350°C;
[0050] When entering the station and reaching the processing position, first remove the blast furnace slag, and the slag removal rate should be ≥97%;
[0051] The S content of hot metal after desulfurization is ≤0.001%, the slag after desulfurization is removed, the slag removal rate is ≥96%, and the temperature is ≥1320℃
[0052] As a further preferred embodiment of the present invention,
[0053] In step S3, the converter double slag method is combined with the steel slag washing method during converter smelting;
[0054] The added high-quality scrap steel has a P content of ≤0.02%, S ≤0.005%, Al ≤0.05%, Ti ≤0.005%, Cr ≤0.05%, Mo ≤0.02%, V ≤0.035%, Sn ≤0.03%, As ≤0.015%, and the rest is Fe and other inevitable components;
[0055] As a further preferred embodiment of the present invention,
[0056] In step S3, when the blowing is stopped at the primary stage of converter smelting, the slag basicity is 1.8-2.5, the T.Fe content in the slag is 25-35%, the temperature is 1380-1420°C, and 70-80% of the slag is discharged; then slag making and blowing are continued, and at the end of blowing, the slag basicity is 3.5-5.5, the T.Fe content is 20-30%, and 60-70% of the slag is discharged first; steel tapping is continued, and the slide plate is used to block the slag, and the steel tapping hole slide plate is closed before the steel tapping and shaking furnace, and the slide plate is opened for steel tapping after the molten steel is completely immersed in the top of the slide plate for more than 30 cm;
[0057] As a further preferred embodiment of the present invention,
[0058] In step S4, based on the molten steel obtained by converter smelting in step S3 after slag dephosphorization, the ternary synthetic slag of lime, fluorite and calcium aluminosilicate is melted in the LF refining process, and 0.5-1.0 kg / t low carbon steel slag surface deoxidizer is added in the slagging process;
[0060] Among them, the main components of low carbon steel slag surface deoxidizer are Al 25-35%, CaO 40-50%, Al2O310-15%, SiO2≤5% and other inevitable components, and the oxygen content in the molten steel is controlled to be in the range of 0.040-0.065%. At the same time, the molten steel is heated to at least 1620℃ and transported to RH vacuum treatment, VD / VOD vacuum treatment;
[0061] As a further preferred embodiment of the present invention,
[0062] In step S5, the vacuum refining method includes RH vacuum treatment and VD / VOD vacuum treatment;
[0063] As a further preferred embodiment of the present invention,
[0064] During RH vacuum treatment, the ladle is placed in the treatment position, and vacuum is quickly evacuated for deep decarburization. After C in the molten steel is ≤0.0015%, deoxidizer is added for deoxidation, and then the net circulation is at least 8 minutes, the steel is broken out of the air, and it is left to stand for at least 10 minutes before being transported to the continuous casting;
[0065] Among them, the deoxidizer uses metal aluminum for deoxidation;
[0066] As a further preferred embodiment of the present invention,
[0067] During VD / VOD vacuum treatment, the ladle is placed in the treatment position, the bottom blowing argon is turned on, and the vacuum ladle cover is sealed and vacuuming is started. The bottom blowing argon flow rate is set to 400-600NL / min. After the C in the molten steel is ≤0.0015%, metal aluminum is added to the ladle for deoxidation, and then the bottom blowing pressure is reduced to 30-80NL / min, stirred for 5-10 minutes, broken, tapped, soft blown for at least 15 minutes, and transported to continuous casting;
[0068] As a further preferred embodiment of the present invention,
[0069] In step S6, during continuous casting of large square billets, the tundish superheat control range is 25-45°C, the pouring tonnage is ≥20 tons, the molten steel weight is ≥35 tons during normal pouring, and the tundish tonnage is ≥30 tons during continuous casting and ladle replacement;
[0070] As a further preferred embodiment of the present invention,
[0071] In step S6, during the continuous casting of the large square billet, the crystallizer is set with an electromagnetic stirring current of 300-500A, a frequency of 1.5-4.5HZ, a crystallizer water volume of 2900-3100NL / min, an inlet and outlet water temperature difference of ≤10°C, and a secondary cooling water volume of 0.38-0.42NL / kg;
[0072] As a further preferred embodiment of the present invention,
[0073] In step S6, during the continuous casting of the billet, the continuous casting speed is set to 0.5-0.8 m / min, and ultra-low carbon steel protection slag is used;
[0074] As a further preferred embodiment of the present invention, in step S6, during the continuous casting of the billet, a strong cooling process is adopted with a reduction of 18-22 mm;
[0075] As a further preferred embodiment of the present invention,
[0076] The pressing is distributed among 5-12 pairs of rollers, and the pressing amounts are set to 0.5-1.0mm, 2.0-2.5mm, 3.0-3.5mm, 4.0-4.5mm, 4.0-4.5mm, 2.0-3.0mm, 2.0-3.0mm, and 1.0-1.5mm respectively;
[0077] As a further preferred embodiment of the present invention,
[0078] In step S7, the surface of the ingot is dephosphorized before being opened, and the ingot is sent to the heating furnace after being cleaned. The heating furnace time is set to 150-180 minutes. The ingot is opened to obtain a 140 mm × 140 mm ingot. The ingot is sent to the heating furnace after magnetic particle inspection and automatic grinding;
[0079] As a further preferred embodiment of the present invention,
[0081] In step S7, the heating furnace temperature is set to 1150-1200°C, the blanking temperature is set to 1120-1150°C, and the grinding depth is set to ≥0.5mm;
[0082] As a further preferred embodiment of the present invention,
[0083] In step S8, during high-speed wire rolling, the rolling start temperature is set to 980-1000°C and the wire laying temperature is set to 880-920°C;
[0084] As a further preferred embodiment of the present invention,
[0085] In step S8, controlled cooling is performed on the Stelmor controlled cooling line during high-speed wire rolling, all fans on the Stelmor controlled cooling line are turned off, the roller table entrance speed is controlled at 12-18 m / min, the maximum speed is controlled at 24-30 m / min, the first section insulation cover is fully opened, the second section is opened 50% insulation cover is opened, the third to sixth sections insulation covers are all closed, and the insulation covers of each section from the seventh section and thereafter are all opened;
[0086] The wire rod produced by the preparation method comprises, by mass percentage, the following chemical compositions: C≤0.0020%, Si≤0.008%, Mn≤0.05%, Alt≤0.0035%, P≤0.006%, S≤0.0025%, TO≤0.0055%, N≤0.0020%, H≤0.00015%, Ti≤0.0007%, Cr≤0.01%, Mo≤0.005%, V≤0.006%, Sn≤0.01%, As≤0.008%, and the rest are Fe and other inevitable impurity components;
[0087] The maximum inclusion size in the wire rod is ≤10 μm, the brittle inclusion is ≤5 μm, and the tensile strength of the wire rod is ≤260 MPa;
[0088] As a further preferred embodiment of the present invention, the produced wire rod has a wire breakage rate of ≤0.12 times / ton and a conductivity of ≥17.0%.
[0089] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0090] 1. The low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire provided by the present invention controls the content of alloy elements and impurity elements through the process design of the whole smelting process, especially overcomes the problem of slightly greater difficulty in converter smelting dephosphorization, and achieves the control target of ultra-low phosphorus content through reasonable converter dephosphorization smelting process design;
[0091] 2. The method for preparing the high-conductivity copper-clad steel wire provided by the present invention further reduces the C content to an extremely low level by optimizing the design of the vacuum treatment process, and then controls the deoxidation and alloying process to achieve precise control of the type of inclusions, and combines the optimization of the vacuum treatment process and the treatment method to significantly remove inclusions in the molten steel and reduce the number and size of inclusions;
[0092] 3. The preparation method of the wire rod for high conductivity copper clad steel wire provided by the present invention optimizes the continuous casting process parameters, controls the surface and internal quality of the ingot, obtains the ingot with low defect rate, and strictly controls the surface quality and internal quality of the wire rod, and improves the rolling process, reduces the strength of the wire rod, makes it easy to draw, and comprehensively obtains the wire rod with good drawing performance and not easy to break. BRIEF DESCRIPTION OF THE DRAWINGS
[0093] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0094] Figure 1 It is an overall flow chart of the method for preparing the wire rod for high conductivity copper clad steel wire provided by the present invention. DETAILED DESCRIPTION
[0095] The present invention will now be described in further detail with reference to the accompanying drawings.
[0097] As described in the background technology, combined with various literature introductions and actual product conductivity application tests, the less impurity elements in the steel used for copper-clad steel, the higher the conductivity of the material, especially pure metal substances have the highest conductivity. At the same time, another point that this application should pay attention to is that the presence of certain elements (focusing on phosphorus and nitrogen elements) can also cause the material to become brittle, resulting in a "cold brittle" phenomenon.
[0098] Related elements such as C, as the carbon content increases, the welding performance of steel deteriorates, the cold brittleness and aging sensitivity increase, the atmospheric corrosion resistance decreases, and the conductivity is significantly reduced; Si can dissolve in ferrite and austenite to increase the hardness and strength of steel. Silicon can promote the growth of columnar crystals in cast steel, which will significantly reduce the plasticity, toughness and welding performance of steel. At the same time, silicon can also reduce the density, thermal conductivity and electrical conductivity of steel.
[0099] The main function of Mn is to combine with S to form MnS, which prevents the hot brittle phenomenon caused by the segregation of free S grain boundaries. At the same time, Mn can also play a certain deoxidation role, which is beneficial to reduce the melting point of inclusions and improve the plasticity of inclusions. However, too high Mn content will also reduce the conductivity. The present invention strictly controls the Mn content. However, the increase of manganese content will reduce the plasticity and welding performance of steel.
[0100] The main function of Al in steel is to refine the grains and fix the nitrogen in the steel, thereby significantly improving the impact toughness of the steel and reducing the cold brittleness tendency and aging tendency. Al is an important deoxidizing element, which can significantly reduce the oxygen content in the steel. At the same time, Al can also fix the free oxygen and free nitrogen in the steel, which can prevent the steel wire from aging embrittlement during the wire drawing process. However, too high Al content will reduce the conductivity. Aluminum oxygen reaction!
[0101] Although phosphorus can increase the strength and hardness of steel, it causes a significant decrease in plasticity and impact toughness. Especially at low temperatures, it makes steel significantly brittle, a phenomenon called "cold brittleness". Cold brittleness deteriorates the cold processing and weldability of steel. The higher the phosphorus content, the greater the cold brittleness. Phosphorus can also increase the resistivity of steel, so the phosphorus content in steel is strictly controlled.
[0102] Sulfur is a harmful element in most steels. Sulfur exists in steel in the form of iron sulfide (FeS), and FeS forms a low melting point (985°C) compound with Fe. The hot working temperature of steel is generally above 1150-1200°C, so when steel is hot worked, the workpiece will crack due to the premature melting of FeS compounds. This phenomenon is called "hot brittleness". It reduces the ductility and toughness of steel and causes cracks during forging and rolling. Sulfur is also detrimental to welding performance and reduces corrosion resistance.
[0103] O is a harmful element in steel. It naturally enters the steel during the decarburization process of steelmaking. The content of alloy elements in copper-clad steel is very low, and oxygen is difficult to remove. During the solidification of molten steel, oxygen and carbon in the solution react to generate CO, or oxygen saturation overflows, which can cause bubble defects. In addition to dissolved oxygen, oxygen in steel mainly exists in the form of FeO, MnO, SiO2, Al2O3 and other inclusions, which reduce the strength and plasticity of steel. In particular, it has a serious impact on fatigue strength and impact toughness.
[0104] The influence of N on the properties of steel is similar to that of carbon and phosphorus. With the increase of nitrogen content, the strength of steel can be significantly improved, while the plasticity, especially toughness, is significantly reduced, weldability is deteriorated, and cold brittleness is aggravated; at the same time, the aging tendency, cold brittleness and hot brittleness are increased, and the welding performance and cold bending performance of steel are damaged. Therefore, the nitrogen content in steel should be reduced and limited as much as possible.
[0106] Other elements are impurities, which will not only reduce the conductivity, but also reduce the plasticity or toughness of the wire rod and increase the tensile strength of the wire rod, which is not conducive to subsequent drawing and finished steel wire production. Their content should be reduced as much as possible when preparation conditions permit to meet the high conductivity requirements while taking into account the cost.
[0107] The present application firstly focuses on the smelting process in the production process of wire rod for high conductivity copper-clad steel. Through production tests, it is found that the smelting process adopts converter smelting, which has a great advantage in obtaining low N elements in all the above-mentioned elements that can affect the conductivity of steel materials in copper-clad steel. This is because the converter does not need to be powered on during smelting, and its highly oxidizing environment makes it easy to control the N content in the molten steel. The converter boils and taps steel, and the molten steel has strong oxidizing properties, which can reduce the absorption of N from the air during the tapping process. Subsequently, combined with vacuum treatment, N is further removed to obtain low-N molten steel.
[0108] However, after using converter smelting, phosphorus needs to be treated specially. Regarding phosphorus, the first innovation of this application is to provide a low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire wire rod. When converter smelting is performed, the carbon content of the converter steel is 0.025-0.055%, the oxygen content is 0.050-0.085%, P≤0.012%, and the steel tapping temperature is ≥1620°C.
[0109] If the P of steel tapping is ≤0.0060, 4.0-5.0kg / t of lime, 0.8-1.3kg / t of fluorite and 6.0-8.0kg / t of calcium silicate ternary synthetic slag are added into the ladle for slagging when 65-75% of the converter has been tapped. The bottom blowing flow rate of the ladle during the steel tapping process is 600-800NL / min. After the steel tapping is completed, it is transported to LF for heating.
[0110] If the P of the converter steel is greater than 0.0060%, dephosphorization treatment is performed during the steel tapping process. The specific steps are:
[0111] Step 1: When 10% of the steel is tapped from the converter, fine lime and iron oxide powder are added to the ladle slag;
[0112] Among them, the amount of fine lime added is 3.0-4.0kg / t, the particle size of 1-5mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 10mm, the CaO content is ≥95%, and other unavoidable impurities; the amount of iron oxide powder added is 1.0-2.0kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 15mm, and the Fe oxide accounts for ≥80%;
[0113] Step 2: During the steel tapping process, the ladle bottom blowing flow rate is 600-800NL / min, and after the steel tapping is completed, it is set to 800-1000NL / min. After stirring for 3-5 minutes, the bottom blowing of argon is stopped, and slag removal is started. The slag removal rate is ≥90%, and the P content of the molten steel is ≤0.005%;
[0114] Step three, adding lime, fluorite and calcium aluminosilicate ternary synthetic slag, the main components of calcium aluminosilicate ternary synthetic slag are CaO 50-55%, Al2O3 20-25%, SiO2 15-20%, MgO 3-5% and other inevitable components, among which 2CaO·Al2O3·SiO2 phase accounts for ≥80%, and then transported to LF for refining and heating.
[0115] By designing the converter deep dephosphorization process, the P content in the molten steel can be removed to an extremely low level. If it cannot be removed, dephosphorization will continue during the steelmaking process to ensure that the P content meets the standard.
[0116] After ensuring that the phosphorus content meets the standard, in order to further develop high-purity steel to prepare high-conductivity copper-clad steel wire, the prior art proposes a variety of preparation methods, including physical methods, chemical methods, or physical and chemical methods.
[0118] However, these preparation methods all have some problems that make it impossible to obtain copper-clad steel with high conductivity, such as the tensile strength of the wire rod obtained is relatively high and the control level of harmful impurity elements is poor; the content of impurity elements S, O, and N is difficult to control, and the high-basicity slag causes the high-melting-point brittle inclusions in the steel to exceed the standard; the content of impurity elements P, S, Alt, Si, and N is difficult to control, and the amount of Al2O3 inclusions in the molten steel is relatively large; the residual Al and Ti content in the molten steel is high, and the content of impurity elements such as P, S, Mn, and N is also relatively high overall; the content of Al, Mn, and P is relatively high, and the amount of Al2O3 inclusions is relatively large; the content of impurity elements C, Si, Mn, P, and S is relatively high, and the grains are coarse.
[0119] Therefore, the present application further provides a method for preparing a wire rod for high conductivity copper-clad steel wire. Figure 1 As shown, the content of each element (P, S, Cr, Cu, Mo, C, Al, Si, Mn) is reduced as much as possible to make the steel purer and improve the conductivity under the control of the rolling process.
[0120] The specific steps include:
[0121] Step S1: Production preparation, a number of ladles are numbered from short to long according to their ages, and ladles numbered 1-20 are selected for desulfurization treatment; after the ladle is charged with iron into the converter each time, the ladle is hoisted into the cleaning position, and after turning over, the residue in the ladle is cleaned with a high-pressure air gun, and the nodules at the ladle mouth are cleaned with a bag unpacker;
[0122] The tapping holes used in the converter are numbered in sequence according to the order of use, and the tapping holes numbered 3-20 are selected;
[0123] Before the converter smelts copper-clad steel, ensure that the converter completes the smelting of at least two batches of ultra-low phosphorus and ultra-low sulfur steel grades (steel grades with P≤0.012%, S≤0.005%), and after the smelting is completed, the slag is drained cleanly, and the steel and slag at the steel outlet are cleaned, and no slag splashing furnace protection operation is performed;
[0124] Before the converter is used to smelt copper-clad steel, the molten steel from a furnace of boiling steel is used to clean and heat the vacuum chamber. After continuous circulation for 10-20 minutes, the copper-clad steel molten steel is transported to the vacuum chamber for the next step of treatment.
[0125] LF refining bag covers, RH vacuum tank covers, and VD / VOD vacuum tank covers are all cleaned;
[0126] Prepare unused carbon-free ladle, C content ≤ 1.5%, baking time ≥ 30 hours, temperature ≥ 1250℃;
[0127] Prepare low-carbon refractory materials and protective slag for continuous casting process; the prepared low-carbon refractory materials include RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom trough, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three major parts of continuous casting, among which the C content of RH vacuum furnace immersion tube and refractory materials in contact with molten steel in the bottom trough is ≤1%, the C content of refractory materials in the working layer of the continuous casting tundish is ≤1%, and the C content of refractory materials for the three major parts of continuous casting is ≤10%; the C content of protective slag is ≤2%.
[0128] Step S2: Pretreatment of molten iron, deep desulfurization of the molten iron, the sulfur element in the molten iron forms desulfurization slag; in this step, the main purpose of molten iron pretreatment is to remove the sulfur element in the molten iron to an extremely low level, and the S element can be removed by simply scraping off the formed desulfurization slag. In actual operation, the elements in the molten iron entering the KR station include C 4.2-4.5%, Si 0.20-0.65%, Mn≤0.30%, P≤0.10%, S≤0.050%, as well as Fe and other inevitable components, the temperature is ≥1350℃, the KR enters the station to the processing position, first scrapes off the blast furnace slag, and the slag scraping rate is ≥97%. The S content of the molten iron after desulfurization is ≤0.001%, and the slag after desulfurization is scraped off.
[0130] The slag removal rate is ≥96%, and the temperature is ≥1320℃.
[0131] Step S3: converter smelting, using the converter double slag method combined with the steel slag washing method; based on the molten iron from which the desulfurization slag is removed in step S2, it is added into the converter and high-quality scrap steel is added for smelting; the alloy elements of high-quality scrap steel or clean scrap steel need to be controlled at a lower level to facilitate the removal of P, Al, Ti, and Cr content in the molten steel during smelting, while reducing the content of Mo and other elements that are not easily oxidized to avoid their inability to be oxidized and removed during converter smelting.
[0132] Preferably, in the high-quality scrap steel provided in the present application, the P content is ≤0.02%, S≤0.005%, Al≤0.05%, Ti≤0.005%, Cr≤0.05%, Mo≤0.02%, V≤0.035%, Sn≤0.03%, As≤0.015%, and the rest is Fe and other inevitable components.
[0133] When the blow is stopped in the primary stage of converter smelting, the slag basicity is 1.8-2.5, the T.Fe content in the slag is 25-35%, the temperature is 1380-1420℃, and the slag is 70-80%; then continue slag making and blowing, and at the end of blowing, the slag basicity is 3.5-5.5, the T.Fe content is 20-30%, and 60-70% of the slag is first poured; continue to tap steel, use a slide plate to block the slag, close the tapping hole slide plate before tapping the steel, and open the slide plate to tap steel after the molten steel is completely immersed in the top of the slide plate for more than 30cm. The above operation can reduce the carbon content, TO content and phosphorus content of the tapped steel to extremely low levels. Through the design of smelting process flow, equipment selection, process scheme design, etc., the control target can be achieved, that is, the carbon content of the converter tapped steel is 0.025-0.055%, the oxygen content is 0.045-0.085%, P≤0.01%, and the tapping temperature is ≥1620℃.
[0134] In the converter smelting process, low-sulfur scrap steel and slag-making materials such as lime are combined to prevent sulfur increase in molten steel and obtain ultra-low S molten steel.
[0135] Regarding the special treatment of phosphorus in this step, the first innovation of the present application is to provide a low-phosphorus converter smelting method for improving the conductivity of wire rods for copper-clad steel wire, which can be implemented according to the above method.
[0136] The second is carbon element. While removing P in the converter, oxygen blowing decarburization is also carried out to reduce the C content to about 0.02-0.05% water, and then the steel is tapped. After the LF refining treatment in step S4, deep decarburization treatment is performed under RH / VD / VOD vacuum to obtain ultra-low carbon molten steel.
[0137] Next is the TO content. The slag is modified during the converter tapping and the LF refining process of step S4 to control the oxygen content and temperature of the molten steel slag. Then, C is used for deoxidation under RH / VD / VOD vacuum. After most of the oxygen is removed, an appropriate amount of aluminum-containing alloy is added. The amount added is controlled to remove the oxygen content of the molten steel while preventing the Al content in the molten steel from being too high.
[0138] The last element is Ti, which is oxidized by the oxidizing property of the converter. Titanium oxide enters the slag, and then the slag is controlled during the steelmaking process to avoid bringing Ti into the molten steel.
[0139] Step S4: LF refining, based on the molten steel obtained by the converter smelting in step S3 after the steel slag is washed and dephosphorized, the lime, fluorite and calcium aluminosilicate ternary synthetic slag are melted in the LF refining process, and 0.5-1.0kg / t low-carbon steel slag surface deoxidizer is added in the slagging process; wherein the main components of the low-carbon steel slag surface deoxidizer are Al 25-35%, CaO 40-50%, Al2O310-15%, SiO2≤5% and other inevitable components, and the oxygen content in the molten steel is controlled to be in the range of 0.040-0.065%, and the molten steel is heated to at least 1620°C.
[0141] Transport to vacuum treatment.
[0142] After the oxygen content is well controlled, the bubbles formed on the surface and inside of the billet during the subsequent step S6 of continuous casting of the billet can be reduced, thereby improving the surface and internal quality of the billet.
[0143] Step S5: vacuum refining, vacuum refining methods include RH vacuum treatment, VD / VOD vacuum treatment. When performing vacuum treatment, set the vacuum chamber working pressure ≤ 100Pa, after decarburization for 15 minutes, add metal aluminum for deoxidation, wherein the amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel , M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of decarburization in the vacuum chamber, %; m O RH is the target oxygen content of molten steel, %; M steel is the weight of molten steel, kg; a is the oxygen supply coefficient to the molten steel considering slag, vacuum tank and ladle wall cold slag, 1.35-1.55.
[0144] The deoxidizer used in vacuum refining in this step needs to be strictly controlled for its related deoxidizing elements because there is a large amount of oxygen in the molten steel after the vacuum deep decarburization. In order to obtain high-conductivity copper-clad steel, all kinds of elements in the steel must be strictly controlled. At the same time, the strong deoxidizing elements such as Al, Ca, and Mg must be controlled to be extremely low in their own content (the total oxygen in the molten steel is still maintained within 50ppm after the deoxidation, and it is not advisable to remove it to below 15ppm, because removing the oxygen content too low will lead to more inclusions produced by the deoxidizing elements) and reducing the content of Si and Mn, which are commonly used deoxidizing alloy elements (removing the oxygen content in the molten steel to below 50ppm), to remove the oxygen content in the molten steel.
[0145] Specifically, for RH vacuum treatment, the ladle is placed in the treatment position, and vacuum is quickly evacuated for deep decarburization. After the C in the molten steel is ≤0.0015%, a deoxidizer is added for deoxidation (the deoxidizer uses metallic aluminum for deoxidation), and then the net circulation is at least 8 minutes, the air is broken and the steel is tapped, and it is left to stand for at least 10 minutes before being transported to the continuous casting.
[0146] For VD / VOD vacuum treatment, the ladle is placed in the treatment position, the bottom blowing argon is turned on, and the vacuum ladle cover is sealed and vacuuming is started. The bottom blowing argon flow rate is set to 400-600NL / min. After C in the molten steel is ≤0.0015%, metallic aluminum is added to the ladle for deoxidation, and then the bottom blowing pressure is reduced to 30-80NL / min. Stir for 5-10 minutes, break the air, tap the steel, soft blow for at least 15 minutes, and then transport it to continuous casting.
[0147] Step S6: continuous casting of large square billets, set the continuous casting speed to 0.5-0.8m / min, use ultra-low carbon steel protective slag, the water volume of the crystallizer is 2900-3100NL / min, the inlet and outlet water temperature difference is ≤10℃, the secondary cooling water volume is 0.38-0.42NL / kg; the pressure is distributed to 5-12 pairs of rollers, and the pressure reduction is set to 0.5-1.0mm, 2.0-2.5mm, 3.0-3.5mm, 4.0-4.5mm, 4.0-4.5mm, 2.0-3.0mm, 2.0-3.0mm, and 1.0-1.5mm respectively. The continuous casting section is 300mm×390mm, the tundish superheat control range is 25-45℃, the pouring tonnage is ≥20 tons, the molten steel weight is ≥35 tons during normal pouring, the tundish tonnage is ≥30 tons during continuous casting and ladle changing, the crystallizer is set with electromagnetic stirring current of 300-500A, frequency of 1.5-4.5HZ, strong cooling process is adopted, and the reduction is 18-22mm.
[0148] The continuous casting operation in this step adopts a high superheat strong cooling process. Because the molten steel contains a certain amount of oxygen, a small amount of small bubbles will be formed in the ingot during the continuous casting cooling process. The aforementioned steps S3-S5 have achieved the control of the oxygen content, and the high superheat intensity strong cooling process in this step can further promote the overflow of bubbles and ensure the ingot shape. Combined with the process of precise distribution of large pressure reduction, it can reduce the cooling of molten steel and the cooling of wire rods during rolling to precipitate oxide inclusions, control the pores and center quality of the ingot, and obtain ingots with low defect rates.
[0149] Step S7: blanking and grinding. Before blanking, the surface of the ingot is dephosphorized and cleaned before being sent to a heating furnace for the first heating. The heating furnace time is set to 150-180 minutes, the heating furnace temperature is set to 1150-1200°C, and the blanking temperature is 1120-1150°C. After the first heating is completed, the blank is opened to obtain a 140mm×140mm billet. After blanking, magnetic particle inspection is performed, and local grinding is performed according to the inspection results. The grinding depth is ≥0.5mm. After ensuring that there are no obvious defects on the surface, it is sent to a heating furnace for a second heating to obtain a small square billet for preparing wire rods, thereby improving the surface quality of the intermediate billet and preventing foreign matter such as oxide scale from being pressed in during the subsequent rolling process to affect the surface quality.
[0150] Step S8: high-speed wire rolling, set the rolling temperature to 980-1000°C, the spinning temperature to 880-920°C, here, the spinning temperature of the spinning machine is set above the phase change temperature, but not too high. In order to avoid the steel strength being too high, the difference between the spinning temperature and the phase change temperature should be reduced. Controlled cooling is performed on the Stelmor cooling line, the Stelmor cooling line fan switch and air volume, and the number of insulation cover switches are preset, slow cooling is performed, and the strength of the wire rod is controlled; specifically, during high-speed wire rolling, controlled cooling is performed on the Stelmor cooling line, all fans on the Stelmor cooling line are turned off, the roller operation entrance speed is controlled at 12-18m / min, the maximum speed is controlled at 24-30m / min, the first section insulation cover is fully opened, the second section is opened 50% insulation cover is opened, the third to sixth sections insulation cover are fully closed, and each insulation cover from the seventh section and thereafter is fully opened, because the phase change of the steel has ended at this time, in order to ensure that the wire rod is not coiled, the wire rod should be properly accelerated to cool after the phase change. Obtain low-strength and high-quality copper-clad steel wire rod.
[0151] Step S9: Packing and transportation: the baling wire and the wire rod are separated by soft wear-resistant materials, and wide baling tape is used, with a set width of 3-5 cm and a binding pressure of 20-40 MPa.
[0152] After the process design optimization of the aforementioned steps S1-S5, the content of all alloying elements and impurity elements can be stably controlled at a low level, thereby improving the electrical conductivity of the wire rod and reducing the tensile strength, which is beneficial to the drawing of the wire rod. The optimization and improvement of the smelting process first controls the content of conventional alloying elements such as Al, Si, Mn, and Ti, while greatly reducing the content of impurity elements such as C, P, S, O, and N. Further, by controlling the types and components of molten iron, scrap steel, and deoxidizers, harmful elements such as Cr, Mo, V, Sn, and As are reduced, and comprehensive control of impurity elements is achieved. The number of inclusions is strictly controlled, which can significantly improve the electrical conductivity of copper-clad steel; at the same time, the size of the inclusions is controlled, so that the drawing performance is also significantly improved.
[0153] In the continuous casting process of step S6, the quality of the billet is controlled by a high superheat strong cooling process combined with a continuous casting large reduction process to obtain a low defect rate cast billet. In the billet rolling process of step S7, the intermediate billet is provided with good surface quality by surface flaw detection, grinding and other measures; in the finishing rolling and controlled cooling stage of step S8, a slow cooling process is adopted to obtain a low-strength wire rod and promote the drawing performance of the wire rod. A copper-clad steel wire rod with high conductivity and excellent drawing performance is obtained comprehensively.
[0154] The high-conductivity copper-clad steel wire wire produced by the above-mentioned preparation method has the following chemical components in terms of mass percentage:
[0156] C≤0.0020%, Si≤0.008%, Mn≤0.05%, Alt≤0.0035%, P≤0.006%, S≤0.0025%, TO≤0.0055%, N≤0.0020%, H≤0.00015%, Ti≤0.0007%, Cr≤0.01%, Mo≤0.005%, V≤0.006%, Sn≤0.01%, As≤0.008%, and the rest are Fe and other inevitable impurity components.
[0157] The above is a specific explanation of a low-phosphorus converter smelting method and a preparation method for improving the conductivity of wire rods for copper-clad steel wire provided in this application. Next, several embodiments of preparing and producing finished wire rods by implementing the above-mentioned preparation method are introduced respectively. The embodiments are mainly provided in the form of specific parameters throughout the preparation method.
[0158] Embodiment 1-6:
[0159] After production preparation, the molten iron is pretreated and deep desulfurized. The sulfur element in the molten iron forms desulfurization slag. The S element can be removed by simply scraping off the desulfurization slag. The specific values of the slag scraping rate, the S content of the molten iron after desulfurization, and the tapping temperature are shown in Table 1.
[0160] Table 1
[0161]
[0162] Based on step S2, the molten iron from which the desulfurization slag is removed is added into a converter and high-quality scrap steel is added for smelting; wherein, the content of each element selected in the high-quality scrap steel is P ≤ 0.02%, S ≤ 0.005%, Al ≤ 0.05%, Ti ≤ 0.005%, Cr ≤ 0.05%, Mo ≤ 0.02%, V ≤ 0.035%, Sn ≤ 0.03%, As ≤ 0.015%, and the rest is Fe and other inevitable components.
[0163] The converter double slag method combined with the slag washing method is used. Table 2 shows the slag basicity, T.Fe content in the slag, temperature and slag pouring rate when the blowing is stopped in the primary stage of converter smelting.
[0164] Table 2
[0165] Serial number Slag basicity T.Fe content, % Temperature, °C Slag discharge rate, % Example 1 1.9 27.6 1393 76 Example 2 2.3 25.0 1420 70 Example 3 1.8 33.3 1388 80 Example 4 2.0 29.2 1400 77 Example 5 2.2 35.0 1380 75 Example 6 2.5 31.8 1407 73
[0166] Then continue slag making and blowing. Table 3 shows the slag basicity, T.Fe content and slag dumping rate at the end of blowing.
[0167] Table 3
[0168] Serial number Slag basicity T.Fe content, % Slag discharge rate, % Steel tapping temperature, ℃ Example 1 4.9 20.0 67 1625 Example 2 5.5 28.5 65 1628 Example 3 3.8 25.8 70 1620 Example 4 4.0 23.3 63 1637 Example 5 3.5 30.0 60 1643 Example 6 5.2 28.7 68 1630
[0169] Continue to start tapping steel, use the slide plate to block the slag, close the tapping hole slide plate before tapping and shaking the furnace, and open the slide plate to tap steel after the molten steel is completely submerged above the top of the slide plate by more than 30 cm.
[0170] When the converter is smelting steel, if the steel tapping P in Example 1-Example 6 is ≤0.0060%, 4.5kg / t of lime, 1.1kg / t of fluorite, and 7.5kg / t of calcium aluminosilicate ternary synthetic slag are added to the ladle to make slag when the converter taps 65-75%, and the ladle bottom blowing flow rate during the steel tapping process is 700NL / min.
[0171] If the steel tapping P in Example 1-Example 6 is greater than 0.0060%, then 3.6 kg / t of fine lime is added to the ladle slag when 10% of the converter steel is tapped, with a particle size of 1-5 mm accounting for 93% and a CaO content of 96.5%; 1.6 kg / t of iron oxide powder is added, with a particle size of 3-10 mm accounting for 92%, and Fe oxide accounting for 85%; during the steel tapping process, the ladle bottom blowing flow rate is 700 NL / min, which is set to 900 NL / min after the steel tapping is completed. After stirring for 3.5 minutes, the bottom blowing of argon is stopped and slag removal is started, with a slag removal rate of 95% and a P content in the molten steel ≤0.005%; calcium aluminosilicate ternary synthetic slag is added, and the 2CaO·Al2O3·SiO2 phase accounts for 88% of the calcium aluminosilicate ternary synthetic slag.
[0172] Step S4 is LF refining. During the LF refining and slagging process of the molten steel transported from the converter and dephosphorized, the content of the deoxidizer on the surface of the low carbon steel slag added in Examples 1 to 6, the content of oxygen in the RH incoming molten steel, and the temperature of the molten steel after heating are shown in Table 4.
[0173] Table 4
[0174] Serial number Deoxidation dosage of low carbon steel slag surface, kg / t RH inlet oxygen content, % Temperature of molten steel after heating, % Example 1 0.6 0.055 1630 Example 2 0.9 0.060 1625 Example 3 0.5 0.047 1627 Example 4 1.0 0.065 1620 Example 5 0.8 0.040 1633 Example 6 0.7 0.053 1621
[0175] Next, the vacuum refining stage is entered. In Examples 1 to 6, RH vacuum treatment is preferred. When performing RH vacuum treatment, the parameters set are shown in Table 5, including the vacuum chamber working pressure, the amount of metal aluminum added, and the carbon content in the molten steel after vacuum deep decarburization treatment, etc., and finally the target oxygen content of RH steelmaking molten steel is achieved to be below 0.0035%.
[0176] Table 5
[0177]
[0178] In the bloom continuous casting process, the parameters set are shown in Table 6:
[0179] Table 6
[0180]
[0181] After the continuous casting process is completed, Table 7 shows the relevant technical parameters of billet grinding and high-speed wire rolling:
[0182] Table 7
[0183]
[0184] The properties of the wire rod obtained by the above preparation method are shown in Table 8:
[0185] Table 8
[0186]
[0187] It can be seen from the above embodiments that the wire rod prepared by the present application has a conductivity of ≥17.0%. When used to make copper-clad steel wire, the thickness of the surface copper plating layer can be reduced, the production cost of downstream enterprises can be reduced, the size of inclusions in the wire rod is reduced, the number of large-sized inclusions is small, the number of brittle inclusions is small, and the size is small. It is not easy to break the wire during the subsequent wire rod deep processing and drawing process, which significantly reduces the wire breakage rate during the wire rod deep processing process; compared with the traditional method, the low-strength wire rod rolling process produces a wire rod with a tensile strength of 1.5447 W / m.
[0188] ≤260MPa, it is easy to draw during deep processing, and the surface and internal defects of the wire rod are reduced through large pressing, blanking and grinding, further improving the drawing performance of the wire rod.
[0189] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.
[0190] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.
[0191] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.
[0192] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire wire rod, characterized in that: When the converter is used for smelting, the carbon content of the converter steel is 0.025-0.055%, the oxygen content is 0.050-0.085%, P≤0.012%, and the tapping temperature is ≥1620℃; If the P of the tapped steel is ≤ 0.060%, then lime, fluorite and calcium aluminosilicate ternary synthetic slag are directly added to the ladle; If the P of the steel is greater than 0.0060%, dephosphorization treatment will continue during the steel-making process. After the slag is cleaned, lime, fluorite and calcium aluminosilicate ternary synthetic slag will be added.
2. The low-phosphorus converter smelting method for improving the electrical conductivity of copper-clad steel wire according to claim 1, characterized in that: If P of converter steel is ≤0.0060%, add 4.0-5.0kg / t of lime, 0.8-1.3kg / t of fluorite and 6.0-8.0kg / t of calcium aluminosilicate ternary synthetic slag into the ladle for slagging when 65-75% of converter steel is tapped. The bottom blowing flow rate of the ladle during the tapping process is 600-800NL / min. After tapping, the steel is transported to LF for heating.
3. The low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire according to claim 1, characterized in that: If the P of the converter steel is greater than 0.0060%, dephosphorization treatment is performed during the steel tapping process. The specific steps are: Step 1: When 10% of the steel is tapped from the converter, fine lime and iron oxide powder are added to the ladle slag; Among them, the amount of fine lime added is 3.0-4.0kg / t, the particle size of 1-5mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 10mm, the CaO content is ≥95%, and other unavoidable impurities; the amount of iron oxide powder added is 1.0-2.0kg / t, the particle size of 3-10mm accounts for ≥90%, the slag ratio of other particle sizes is <10%, the maximum does not exceed 15mm, and the Fe oxide accounts for ≥80%; Step 2: During the steel tapping process, the ladle bottom blowing flow rate is 600-800NL / min, and after the steel tapping is completed, it is set to 800-1000NL / min. After stirring for 3-5 minutes, the bottom blowing of argon is stopped, and slag removal is started. The slag removal rate is ≥90%, and the P content of the molten steel is ≤0.005%; Step three, adding lime, fluorite and calcium aluminosilicate ternary synthetic slag, the main components of calcium aluminosilicate ternary synthetic slag are CaO 50-55%, Al2O3 20-25%, SiO2 15-20%, MgO 3-5% and other inevitable components, among which 2CaO·Al2O3·SiO2 phase accounts for ≥80%, and then transported to LF for refining and heating.
4. A method for preparing a wire rod for high conductivity copper-clad steel wire, characterized in that: The specific steps include: Step S1: Production preparation, a number of ladles are numbered from short to long according to their ages, and ladles numbered 1-20 are selected for desulfurization treatment; The tapping holes used in the converter are numbered in sequence according to the order of use, and the tapping holes numbered 3-20 are selected; before the converter smelts copper-clad steel, ensure that the converter completes the smelting of at least two batches of ultra-low phosphorus and ultra-low sulfur steel grades, and after the smelting is completed, the slag is removed cleanly, and no slag splashing furnace protection operation is performed; Before copper-clad steel is smelted in the converter, a furnace of boiling molten steel is used to clean and heat the vacuum chamber, and the cycle treatment is continued for 10-20 minutes; LF refining bag covers, RH vacuum tank covers, and VD / VOD vacuum tank covers are all cleaned; Prepare unused carbon-free ladles; Prepare low carbon refractory and mold slag for continuous casting process; Step S2: pre-treating the molten iron, performing deep desulfurization treatment on the molten iron, and forming desulfurization slag with sulfur elements in the molten iron; Step S3: adopting the low-phosphorus converter smelting method for improving the conductivity of copper-clad steel wire wire rod according to claims 1-3, adding the molten iron from which the desulfurization slag is removed in step S2 into the converter and adding high-quality scrap steel for smelting; Step S4: LF refining, LF refining is powered on and heated quickly to raise the temperature of the molten steel transported from the converter to greater than or equal to 1620°C; Step S5: Vacuum refining, set the vacuum chamber working pressure ≤ 100Pa, decarburize for 15 minutes, add metal aluminum for deoxidation, Among them, the amount of metal aluminum added is M Al =9 / 8(a·M O -m O )M steel , M Al is the amount of metal aluminum added, kg; M O The oxygen content at the end of decarburization in the vacuum chamber, %; m O RH is the target oxygen content of molten steel, %; M steel is the weight of molten steel, kg; a is the oxygen supply coefficient to molten steel considering slag, vacuum tank and ladle wall cold slag, 1.35-1.55; After decarburization and deoxidation, the steel is discharged and transported to continuous casting; Step S6: continuous casting of large square billets, setting the continuous casting section to 300 mm×390 mm, and adopting a strong cooling process; Step S7: Opening and grinding, setting the heating furnace temperature and the opening temperature, dephosphorizing the surface of the ingot before opening, cleaning it and sending it to the heating furnace for the first heating. After the first heating is completed, the ingot is opened to obtain the ingot, and the ingot is subjected to magnetic particle inspection. According to the inspection results, local grinding is performed to ensure that there are no obvious defects on the surface, and then the ingot is sent to the heating furnace for the second heating to obtain a small square billet for preparing wire rod; Step S8: high-speed wire rolling, setting the rolling start temperature and the wire laying temperature, performing controlled cooling on the Stelmor cooling line, presetting the Stelmor cooling line fan switch and air volume, and the number of insulation cover switches, performing slow cooling, and controlling the wire rod strength; Step S9: Packing and transportation: the baling wire and the wire rod are separated by soft wear-resistant materials, and wide baling tape is used, with a set width of 3-5 cm and a binding pressure of 20-40 MPa.
5. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S1, after the ladle is charged with iron into the converter each time, the ladle is hoisted into the cleaning position, turned over, and the residue in the ladle is cleaned with a high-pressure air gun, and the nodules at the ladle mouth are cleaned with a bag unpacker; Before the converter smelting copper clad steel operation, tap 2-3 furnaces continuously and clean the steel and slag at the tapping port; The converter continuously smelts at least two batches of steel with P≤0.012% and S≤0.005%. After the converter smelting is completed, all the excess steel and slag shall be completely removed; The prepared unused carbon-free ladle has a C content of ≤1.5%, a baking time of ≥30 hours, and a temperature of ≥1250°C; The prepared low-carbon refractory materials include RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting. Among them, the C content of RH vacuum furnace immersion tube, refractory materials in contact with molten steel in the bottom tank, refractory materials in the working layer of the continuous casting tundish, and refractory materials for three large parts of continuous casting is ≤10%; The C content of the mold slag is ≤2%.
6. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S2, during the pretreatment of molten iron, the elements in the incoming molten iron include C 4.2-4.5%, Si 0.20-0.65%, Mn≤0.30%, P≤0.10%, S≤0.050%, and Fe and other inevitable components, and the temperature is ≥1350°C; When entering the station and reaching the processing position, first remove the blast furnace slag, and the slag removal rate should be ≥97%; The S content of molten iron after desulfurization is ≤0.001%, the slag is scraped off after desulfurization, the slag scraping rate is ≥96%, and the temperature is ≥1320℃.
7. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S3, the converter double slag method is combined with the steel slag washing method during converter smelting; In the added high-quality scrap steel, the content of P is ≤0.02%, S ≤0.005%, Al ≤0.05%, Ti ≤0.005%, Cr ≤0.05%, Mo ≤0.02%, V ≤0.035%, Sn ≤0.03%, As ≤0.015%, and the rest is Fe and other inevitable components.
8. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S3, when the blowing is stopped at the primary stage of converter smelting, the slag basicity is 1.8-2.5, the T.Fe content in the slag is 25-35%, the temperature is 1380-1420°C, and 70-80% of the slag is poured; then slag making and blowing are continued, and at the end of blowing, the slag basicity is 3.5-5.5, the T.Fe content is 20-30%, and 60-70% of the slag is poured first; steel tapping is continued, and the slide plate is used to block the slag, and the steel tapping hole slide plate is closed before the steel tapping and shaking furnace is shaken, and the slide plate is opened for steel tapping after the molten steel is completely immersed in the top of the slide plate for more than 30 cm.
9. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S4, based on the molten steel obtained by converter smelting in step S3 after slag dephosphorization, the ternary synthetic slag of lime, fluorite and calcium aluminosilicate is melted in the LF refining process, and 0.5-1.0 kg / t low carbon steel slag surface deoxidizer is added in the slagging process; Among them, the main components of low carbon steel slag surface deoxidizer are Al 25-35%, CaO 40-50%, Al2O310-15%, SiO2≤5% and other inevitable components. The oxygen content in the molten steel is controlled to be in the range of 0.040-0.065%. At the same time, the molten steel is heated to at least 1620℃ and transported to RH vacuum treatment and VD / VOD vacuum treatment.
10. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S5, the vacuum refining method includes RH vacuum treatment and VD / VOD vacuum treatment.
11. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 10, characterized in that: During RH vacuum treatment, the ladle is placed in the treatment position, and vacuum is quickly evacuated for deep decarburization. After C in the molten steel is ≤0.0015%, deoxidizer is added for deoxidation, and then the net circulation is at least 8 minutes, the steel is broken out of the air, and it is left to stand for at least 10 minutes before being transported to the continuous casting; Among them, the deoxidizer uses metal aluminum for deoxidation.
12. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 10, characterized in that: During VD / VOD vacuum treatment, the ladle is placed in the treatment position, the bottom blowing argon is turned on, and the vacuum ladle cover is sealed and vacuuming is started. The bottom blowing argon flow rate is set to 400-600NL / min. After C in the molten steel is ≤0.0015%, metallic aluminum is added to the ladle for deoxidation, and then the bottom blowing pressure is reduced to 30-80NL / min, stirred for 5-10 minutes, broken, and steel is discharged. Soft blowing is carried out for at least 15 minutes before being transported to continuous casting.
13. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S6, during continuous casting of large square billets, the tundish superheat control range is 25-45°C, the pouring tonnage is ≥20 tons, the molten steel weight is ≥35 tons during normal pouring, and the tundish tonnage is ≥30 tons during continuous casting and ladle replacement.
14. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S6, during the continuous casting of the large square billet, the crystallizer is set with an electromagnetic stirring current of 300-500A, a frequency of 1.5-4.5Hz, a crystallizer water volume of 2900-3100NL / min, an inlet and outlet water temperature difference of ≤10°C, and a secondary cooling water volume of 0.38-0.42NL / kg.
15. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S6, during the continuous casting of the large square billet, the continuous casting speed is set to 0.5-0.8 m / min, and ultra-low carbon steel protective slag is used.
16. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S6, during the continuous casting of the large square billet, a strong cooling process is adopted with a reduction amount of 18-22 mm.
17. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 16, characterized in that: The pressure is distributed among 5-12 pairs of rollers, and the pressure amounts are set to 0.5-1.0mm, 2.0-2.5mm, 3.0-3.5mm, 4.0-4.5mm, 4.0-4.5mm, 2.0-3.0mm, 2.0-3.0mm, and 1.0-1.5mm respectively.
18. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S7, the surface of the ingot is dephosphorized before opening, and the ingot is sent to the heating furnace after cleaning. The heating furnace time is set to 150-180 minutes. The ingot is opened to obtain a 140mm×140mm ingot. The ingot is sent to the heating furnace after magnetic particle inspection and automatic grinding.
19. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 18, characterized in that: In step S7, the heating furnace temperature is set to 1150-1200° C., the blanking temperature is set to 1120-1150° C., and the grinding depth is ≥0.5 mm.
20. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S8, during high-speed wire rolling, the starting rolling temperature is set at 980-1000°C and the wire laying temperature is set at 880-920°C.
21. The method for preparing a wire rod for high conductivity copper clad steel wire according to claim 4, characterized in that: In step S8, controlled cooling is performed on the Stelmor controlled cooling line during high-speed wire rolling, all fans on the Stelmor controlled cooling line are turned off, the roller table entrance speed is controlled at 12-18m / min, the maximum speed is controlled at 24-30m / min, the first section insulation cover is fully opened, the second section insulation cover is 50% opened, the third to sixth sections insulation covers are fully closed, and the insulation covers from the seventh section and thereafter are fully opened.
22. The wire rod produced by the preparation method according to any one of claims 4 to 21, characterized in that: The chemical composition of the wire rod includes, by mass percentage: C≤0.0020%, Si≤0.008%, Mn≤0.05%, Alt≤0.0035%, P≤0.006%, S≤0.0025%, TO≤0.0055%, N≤0.0020%, H≤0.00015%, Ti≤0.0007%, Cr≤0.01%, Mo≤0.005%, V≤0.006%, Sn≤0.01%, As≤0.008%, and the rest is Fe and other inevitable impurity components; The maximum inclusion size in the wire rod is ≤10 μm, the brittle inclusion is ≤5 μm, and the tensile strength of the wire rod is ≤260 MPa.
23. The wire rod produced by the preparation method according to claim 22, characterized in that: The produced wire rod has a wire breakage rate of ≤0.12 times / ton and a conductivity of ≥17.0%.