Method for adding alloy behind oriented silicon steel converter

Through converter smelting, optimized addition and temperature control of ferrosilicon alloys, the problems of uneven alloy distribution and low production efficiency in traditional methods are solved, and efficient industrial production of oriented silicon steel is achieved.

CN118879971APending Publication Date: 2024-11-01BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410999066.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The traditional method of adding oriented silicon steel alloys has problems such as uneven alloy distribution, long feeding time and low production efficiency, which is difficult to meet the needs of large-scale industrial production.

Method used

By using converter smelting, ferrosilicon alloy addition, alloying treatment and temperature control methods, the amount and speed of alloy addition are adjusted in real time, the alloy is uniformly distributed in the molten steel, and sufficient stirring and reaction are carried out to form a stable alloy phase, and the Process flow to improve production efficiency.

Benefits of technology

It realizes uniform distribution and stable reaction of alloys, shortens the refining and processing time, improves production efficiency, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an optimized production method for adding ferro-silicon alloy behind a converter of oriented silicon steel, which optimizes the adding opportunity and the adding amount of the ferro-silicon alloy and optimizes the process flow through the links of converter smelting, ferro-silicon alloy adding, alloying treatment, temperature control and the like, is more convenient to operate, is suitable for large-scale industrial production and improves the production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for adding alloy after a converter furnace of oriented silicon steel. Background Art

[0002] Oriented silicon steel is an important magnetic material in the electric power industry. It plays an important role in power transformers, motors and other power equipment. Its magnetic properties and orientation have a direct impact on the performance of power equipment. In the manufacturing process of oriented silicon steel, the addition of alloys is one of the key steps. Ferrosilicon alloys, as a commonly used alloy additive, have an important influence on the performance of oriented silicon steel. However, the traditional alloy addition method has problems such as uneven alloy distribution, long feeding time, and low production efficiency. The present invention can solve the above problems well. Summary of the invention

[0003] The purpose of the present invention is to provide a method for adding alloys after a converter furnace of oriented silicon steel, which optimizes the timing and amount of adding ferrosilicon alloy through converter smelting, adding ferrosilicon alloy, alloying treatment and temperature control, optimizes the process flow, makes the operation more convenient, is suitable for large-scale industrial production, and improves production efficiency.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for adding alloy to a oriented silicon steel converter, comprising the following steps:

[0006] Converter smelting: According to the conventional converter smelting process, the raw materials are added into the converter for smelting to obtain molten steel;

[0007] Ferrosilicon alloy addition: After the converter, ferrosilicon alloy is added to the molten steel through the alloy collection hopper; during the addition process, the amount and speed of ferrosilicon alloy addition are adjusted in real time according to the temperature and composition of the molten steel to ensure that the alloy is evenly distributed in the molten steel;

[0008] Alloying treatment: After the addition of ferrosilicon alloy is completed, the molten steel is fully stirred and alloyed to allow the ferrosilicon alloy to fully react with other elements in the molten steel to form a stable alloy phase;

[0009] Temperature control: After alloying, the temperature of the molten steel is precisely controlled according to the composition of the molten steel and subsequent process requirements to provide the best temperature conditions for subsequent refining.

[0010] Further, the method specifically includes the following steps:

[0011] Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 772ppm and the temperature is 1633℃. The sliding plate double-stage slag process is adopted in the steel-making process.

[0012] Addition of ferrosilicon alloy: After the converter, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy is added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value;

[0013] Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 500Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase;

[0014] Temperature control: After alloying treatment, the temperature is measured at 1644°C, the argon flow rate is adjusted to 300Nl / min, and after stirring for 5 minutes, the temperature is measured at 1620°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

[0015] Further, the method specifically includes the following steps:

[0016] Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 665ppm and the temperature is 1638℃. The sliding plate double-stage slag process is adopted in the steel-making process.

[0017] Addition of ferrosilicon alloy: After the converter, slowly add 10.5 tons of high-purity ferrosilicon alloy to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is discharged, start adding the first batch of alloy. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the temperature of the molten steel or uneven distribution of silicon elements; when the molten steel is discharged to 2 / 5, add the second batch of alloy. At this time, the molten steel will undergo a period of stirring and reaction. The first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon can be added. Alloy, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloys have been completely melted and the steel tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy is added to adjust the silicon content in the molten steel to the target value; alloying treatment: after the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 510Nl / min, and the molten steel is stirred for 4 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase;

[0018] Temperature control: After alloying treatment, the temperature was measured at 1641°C, the argon flow rate was adjusted to 280Nl / min, and after stirring for 5.5 minutes, the temperature was measured at 1618°C, the argon was turned off, and the ladle was hoisted to RH refining for the next step of treatment.

[0019] Further, the method specifically includes the following steps:

[0020] Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 753ppm and the temperature is 1628℃. The sliding plate double-stage slag process is adopted in the steel-making process.

[0021] Addition of ferrosilicon alloy: After the converter, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy is added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value;

[0022] Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 450Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase;

[0023] Temperature control: After alloying treatment, the temperature is measured at 1625°C, the argon flow rate is adjusted to 290Nl / min, and after stirring for 3 minutes, the temperature is measured at 1622°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

[0024] Compared with the prior art, the beneficial technical effects of the present invention are:

[0025] The present invention optimizes the timing and amount of adding ferrosilicon alloy through converter smelting, ferrosilicon alloy addition, alloying treatment and temperature control, optimizes the process flow, makes the operation more convenient, is suitable for large-scale industrial production, and improves production efficiency. DETAILED DESCRIPTION

[0026] The present invention is further described below by way of examples.

[0027] Example 1

[0028] A method for adding alloy to a oriented silicon steel converter comprises the following steps:

[0029] Converter smelting: Qualified desulfurized molten iron is added into the converter, and self-produced low-impurity scrap steel is added. During the converter smelting process, active lime, light-burned dolomite, iron balls and other slag-forming materials are added. At the end point control, the oxygen is 772ppm and the temperature is 1633℃. The slide plate double-stage slag process is adopted in the steelmaking process.

[0030] Addition of ferrosilicon alloy: After the converter furnace, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy begins to be added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can not only ensure the continuous supply of silicon elements, but also avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value.

[0031] Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 500Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase.

[0032] Temperature control: After alloying treatment, the temperature is measured at 1644°C, the argon flow rate is adjusted to 300Nl / min, and after stirring for 5 minutes, the temperature is measured at 1620°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

[0033] Through the above operations, the RH refining process time was shortened. Without the optimization measures, RH refining took 60 minutes to complete; after the optimization, the RH refining time was shortened to 50 minutes, and the production efficiency was increased by about 16.7%.

[0034] Example 2

[0035] A method for adding alloy to a oriented silicon steel converter comprises the following steps:

[0036] Converter smelting: Qualified desulfurized molten iron is added into the converter, and self-produced low-impurity scrap steel is added. During the converter smelting process, active lime, light-burned dolomite, iron balls and other slag-forming materials are added. At the end point control, the oxygen is 665ppm and the temperature is 1638℃. The slide plate double-stage slag process is adopted in the steelmaking process.

[0037] Addition of ferrosilicon alloy: After the converter furnace, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy begins to be added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can not only ensure the continuous supply of silicon elements, but also avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value.

[0038] Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 510Nl / min, and the molten steel is stirred for 4 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase.

[0039] Temperature control: After alloying treatment, the temperature was measured at 1641°C, the argon flow rate was adjusted to 280Nl / min, and after stirring for 5.5 minutes, the temperature was measured at 1618°C, the argon was turned off, and the ladle was hoisted to RH refining for the next step of treatment.

[0040] Through the above operation, the RH refining treatment time was shortened. Without improving the ferrosilicon alloy addition method, RH refining required 60 minutes; after the improvement, the RH refining time was shortened to 53 minutes, and the production efficiency was increased by about 11.7%.

[0041] Example 3

[0042] A method for adding alloy to a oriented silicon steel converter comprises the following steps:

[0043] Converter smelting: Qualified desulfurized molten iron is added into the converter, and self-produced low-impurity scrap steel is added. During the converter smelting process, active lime, light-burned dolomite, iron balls and other slag-forming materials are added. At the end point control, the oxygen is 753ppm and the temperature is 1628℃. The slide plate double-stage slag process is adopted in the steelmaking process.

[0044] Addition of ferrosilicon alloy: After the converter furnace, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy begins to be added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can not only ensure the continuous supply of silicon elements, but also avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value.

[0045] Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 450Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase.

[0046] Temperature control: After alloying treatment, the temperature is measured at 1625°C, the argon flow rate is adjusted to 290Nl / min, and after stirring for 3 minutes, the temperature is measured at 1622°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

[0047] Through the above operation, the RH refining treatment time is shortened. Without improving the ferrosilicon alloy addition method, RH refining takes 60 minutes; after the improvement, the RH refining time is shortened to 52 minutes, and the production efficiency is increased by about 13.3%.

[0048] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for adding alloy to a oriented silicon steel converter, characterized in that: The following steps are involved: Converter smelting: According to the conventional converter smelting process, the raw materials are added into the converter for smelting to obtain molten steel; Ferrosilicon alloy addition: After the converter, ferrosilicon alloy is added to the molten steel through the alloy collection hopper; during the addition process, the amount and speed of ferrosilicon alloy addition are adjusted in real time according to the temperature and composition of the molten steel to ensure that the alloy is evenly distributed in the molten steel; Alloying treatment: After the addition of ferrosilicon alloy is completed, the molten steel is fully stirred and alloyed to allow the ferrosilicon alloy to fully react with other elements in the molten steel to form a stable alloy phase; Temperature control: After alloying, the temperature of the molten steel is precisely controlled according to the composition of the molten steel and subsequent process requirements to provide the best temperature conditions for subsequent refining.

2. The method for adding alloy to a oriented silicon steel converter according to claim 1, characterized in that: The specific steps include: Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 772ppm and the temperature is 1633℃. The sliding plate double-stage slag process is adopted in the steel-making process. Addition of ferrosilicon alloy: After the converter, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy is added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy is added, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value; Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 500Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase; Temperature control: After alloying treatment, the temperature is measured at 1644°C, the argon flow rate is adjusted to 300Nl / min, and after stirring for 5 minutes, the temperature is measured at 1620°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

3. The method for adding alloy after converter furnace of oriented silicon steel according to claim 1, characterized in that: The specific steps include: Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 665ppm and the temperature is 1638℃. The sliding plate double-stage slag process is adopted in the steel-making process. Addition of ferrosilicon alloy: After the converter, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy is added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy is added, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value; Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 510Nl / min, and the molten steel is stirred for 4 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase; Temperature control: After alloying treatment, the temperature was measured at 1641°C, the argon flow rate was adjusted to 280Nl / min, and after stirring for 5.5 minutes, the temperature was measured at 1618°C, the argon was turned off, and the ladle was hoisted to RH refining for the next step of treatment.

4. The method for adding alloy after converter furnace of oriented silicon steel according to claim 1, characterized in that: The specific steps include: Converter smelting: add qualified desulfurized molten iron into the converter, and add self-produced low-impurity scrap steel. Add active lime, light-burned dolomite, and iron ball slag-making materials into the converter during the converter smelting process. When the endpoint is controlled, the oxygen is 753ppm and the temperature is 1628℃. The sliding plate double-stage slag process is adopted in the steel-making process. Addition of ferrosilicon alloy: After the converter, 10.5 tons of high-purity ferrosilicon alloy is slowly added to 260 tons of molten steel through the alloy collection bucket in three times to ensure that the alloy is evenly distributed in the molten steel; when 1 / 5 of the molten steel is tapped, the first batch of alloy is added. The amount added should not be too much, and 3 tons can be added to avoid a sharp drop in the molten steel temperature or uneven distribution of silicon elements; when the molten steel is tapped to 2 / 5, the second batch of alloy is added. At this time, the molten steel will undergo a period of stirring and reaction, and the first batch of alloy is basically melted in the molten steel. At this time, 5 tons of ferrosilicon alloy can be added, which can ensure the continuous supply of silicon elements and avoid excessive impact on the molten steel; when the molten steel is tapped to 4 / 5, the third batch of alloy is added. At this time, the first two batches of alloy have been completely melted, and tapping is about to end. At this time, the remaining 2.5 tons of ferrosilicon alloy are added to adjust the silicon content in the molten steel to the target value; Alloying treatment: After the addition of ferrosilicon alloy is completed, the argon blowing flow rate at the bottom of the ladle is adjusted to 450Nl / min, and the molten steel is stirred for 3 minutes to allow the ferrosilicon alloy to fully react in the molten steel to form a stable alloy phase; Temperature control: After alloying treatment, the temperature is measured at 1625°C, the argon flow rate is adjusted to 290Nl / min, and after stirring for 3 minutes, the temperature is measured at 1622°C, the argon is turned off, and the ladle is hoisted to RH refining for the next step of treatment.

Citation Information

Patent Citations

  • Refining method for silicon-killed steel ANS process

    CN105861781A

  • Converter blowing end point temperature compensation method

    CN110042188A

  • RH variety steel silicon deoxidation process

    CN112553410A

  • Silicon-containing steel and smelting method thereof

    CN116200642A

  • Low-cost RH ultra-low carbon silicon steel smelting method

    CN117467822A