Application of straw carbon as carbon in IF steel casting powder production

By using straw charcoal and CaO-SiO2-Al2O3 slag system combination in IF steel protection slag, the problem of harmful gas emissions during combustion of existing carbon materials is solved, and the production of pollutants and higher combustion efficiency is achieved. Supports environmentally friendly and sustainable resource utilization.

CN118879983APending Publication Date: 2024-11-01NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410944081.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing carbon materials release a large amount of harmful gases and solid pollutants when burned in IF steel protective slag, and are non-renewable, affecting the efficiency of environmental and resource utilization.

Method used

Straw charcoal is used as the carbon material for protecting slag, and by combining it with the CaO-SiO2-Al2O3 slag system, an optimized protective slag structure is formed, reducing carbon dioxide emissions and improving combustion efficiency.

Benefits of technology

The low fixed carbon content and low sulfur and nitrogen content of straw charcoal reduce the production of pollutants such as SO2 and NOx, and its wide distribution of biomass resources will help sustainable agricultural development and replace fossil energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879983A_ABST
    Figure CN118879983A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of IF steel casting powder carbon matching materials, in particular to application of straw carbon as carbon matching in IF steel casting powder production, and the application of the straw carbon as the carbon matching material in the casting powder specifically comprises the following steps that S1, CaO, SiO2, Al2O3, Na2O, CaF2, MgO and the straw carbon are sequentially added into an agate crucible; and S2, grinding the added materials in the agate crucible, and uniformly mixing to obtain the casting powder. The straw carbon is adopted as a carbon blending material of the casting powder, compared with a traditional carbon blending material, combustion is more sufficient, generated pollutants such as CO2, SO2 and NOx are fewer, and in addition, due to the fact that the storage amount of the straw carbon is huge, development and utilization of the straw carbon are of great significance to fossil resources and agricultural sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon-matching materials for IF steel protection slag, and in particular to application of straw charcoal as carbon-matching material in the production of IF steel protection slag. Background Art

[0002] IF steel is ultra-low carbon interstitial-free steel, with a carbon content generally between 0.002% and 0.015%. Compared with traditional carbon steel, its carbon content is lower and has the advantages of better weldability, mechanical properties and toughness. As a steel for cold-rolled thin plates at high pressure rates, it is the most commonly used deep drawing steel in the home appliance and automotive fields. When IF steel is produced, the C and N interstitial atoms are first controlled to an extremely low content through vacuum degassing technology. Then, by adding elements such as Ti and Nb, the residual C and N in the steel are fixed, so that the steel plate has excellent stamping performance. Continuous casting is an important process in the production of IF steel. During its smelting process, there is often carbon increase in the ingot, which seriously affects the quality of the ingot and is directly related to the carbon matching behavior in the protective slag.

[0003] Shielding slag is an important functional material in the continuous casting process. It is mainly composed of base material, solvent and carbonaceous material. It plays the role of heat insulation, preventing steel liquid oxidation, lubricating ingot, controlling heat transfer in crystallizer and absorbing non-metallic inclusions. When shielding slag is added to the crystallizer, as the temperature rises, the carbon in the shielding slag gradually reacts and burns with the oxygen in the air to form carbon dioxide gas volatilization, and the content gradually decreases. Its role in controlling the melting rate weakens. The temperature range and time for the carbonaceous material to play an isolating role are the combustion temperature range and combustion time of the carbon in the shielding slag. When the carbon is burned, the role of carbon isolating the molten shielding slag also ends. As one of the raw materials that must be added to the shielding slag, the carbonaceous material plays a role in regulating the melting rate of the shielding slag and plays a role as a skeleton. By controlling the thickness of the liquid slag layer, the melting structure model of the shielding slag can be regulated, thereby affecting the insulation, lubrication and heat transfer properties of the shielding slag. The above-mentioned performance regulation role is directly determined by the physicochemical properties of the carbonaceous material in the shielding slag (type, addition amount, specific surface area, particle size and different carbonaceous material matching methods).

[0004] The current carbonaceous materials (graphite, carbon black and coke, etc.) have high contents of S, N and ash, and release a large amount of CO, SO2 and NO during heating. x , dioxins, dust and other gaseous and solid pollutants, which seriously endanger the ecological environment and human life and health. Secondly, the existing carbonaceous materials are a kind of non-renewable fossil energy. Due to the non-renewability of fossil energy and the huge consumption of it by humans, fossil energy is gradually becoming exhausted. In order to protect the environment and efficiently utilize natural resources, a renewable and environmentally friendly carbonaceous material must be developed. Summary of the invention

[0005] The object of the present invention is to provide an application of straw charcoal as a carbon blend in the production of IF steel protection slag to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The invention discloses an application of straw charcoal as carbon blend in the production of protective slag for IF steel.

[0008] Preferably, the IF steel protective slag is composed of a CaO-SiO2-Al2O3 slag system and straw charcoal, and the components of the CaO-SiO2-Al2O3 slag system include: CaO (25%~35%), SiO2 (25%~35%), Al2O3 (5%~12%), Na2O (10%~15%), CaF2 (10%~15%) and MgO (2%~5%).

[0009] Preferably, the ratio of CaO to SiO2 in the protective slag is 1:1.

[0010] Preferably, the straw charcoal is used as a carbon-matching material in IF steel protection slag by the following method:

[0011] S1: Add CaO, SiO2, Al2O3, Na2O, CaF2, MgO and straw charcoal into an agate crucible in sequence;

[0012] S2: Grind the added materials in an agate crucible and mix them evenly to obtain protective slag.

[0013] Preferably, the content of the straw charcoal as a carbon-bearing material in the protective slag is 6-10%.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention uses straw charcoal as a carbon-matching material for protective slag. Compared with traditional carbon-matching materials, straw charcoal has a lower fixed carbon content. After being added to protective slag, the emission of gases such as carbon dioxide can be reduced. Straw charcoal has a high volatile content and is flammable. It can be fully burned when added to protective slag to avoid the formation of a carbon-rich layer. At the same time, the sulfur and nitrogen content in straw charcoal is lower than that in flake graphite, and the SO2 and NO generated during use are x Fewer pollutants.

[0016] 2. Compared with woody biomass charcoal, herbaceous biomass charcoal, fruit biomass charcoal and bark biomass charcoal, the straw charcoal used in the present invention is the most widely distributed biomass resource and the most important crop by-product. The development and utilization of straw charcoal is of great significance to both fossil resources and agricultural sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 TG-DSC curve schematic diagram of flake graphite in Example 1 of the present invention;

[0018] Figure 2 TG-DSC curve diagram of straw charcoal in Example 2 of the present invention;

[0019] Figure 3 This is a schematic diagram of the TG-DSC curve of the protective slag using flake graphite as the carbon-matching material in Example 3 of the present invention;

[0020] Figure 4 This is a schematic diagram of the TG-DSC curve of the protective slag using straw charcoal as the carbon-matching material in Example 4 of the present invention;

[0021] Figure 5 A curve diagram showing the amount of carbon dioxide produced by burning protective slag using straw charcoal and flake graphite as carbon-matching materials in Example 5 of the present invention;

[0022] Figure 6 This is a curve diagram showing the amount of carbon monoxide produced by the combustion of protective slag using straw charcoal and flake graphite as carbon-matching materials in Example 5 of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] See also Figures 1 to 6 , the present invention provides:

[0025] Application of straw charcoal as carbon in the production of IF steel protective slag,

[0026] Selecting straw charcoal as the carbon-matching material for the CaO-SiO2-Al2O3 slag system can effectively improve the quality of the protective slag and reduce harmful gas emissions, which is of great significance to the sustainable development of fossil energy and agriculture.

[0027] Example 1

[0028] See also Figure 1 The specific surface area of ​​flake graphite is about 55.62m 2 / g, it has complete crystallization, thin flakes with good toughness, excellent physical and chemical properties, and has good thermal conductivity, electrical conductivity, thermal shock resistance, corrosion resistance and other characteristics. Flake graphite has a variety of specifications. The carbonaceous material selected in the present invention is flake graphite 1200 mesh. Take about 20 mg of flake graphite, put it into the HCT-3 comprehensive thermal analyzer, heat it from 20°C to 1400°C at a rate of 10°C / min, and observe its combustion in air atmosphere. Figure 1 It can be seen that the combustion temperature range of flake graphite is 570℃-760℃, and flake graphite can be completely burned in air.

[0029] Example 2

[0030] See also Figure 2 The specific surface area of ​​straw charcoal is about 1156m 2 / g, take about 20mg of straw charcoal, put it into the HCT-3 comprehensive thermal analyzer, heat it from 20℃ to 1400℃ at a rate of 10℃ / min, and observe its combustion in air atmosphere. Figure 2 It can be seen that the combustion temperature range of straw charcoal is 350℃-650℃, and straw charcoal can be completely burned under air.

[0031] Example 3

[0032] See also Figure 3 First, add 6% flake graphite into the protective slag, where the protective slag is a CaO-SiO2-Al2O3 slag system, and the proportions of each component added in the flake graphite carbon protective slag are: CaO is 27.5%; SiO2 is 27.5%; Al2O3 is 12%; Na2O is 14.2%; CaF2 is 10.8%; MgO is 2%; flake graphite 1200 mesh is 6%. Each component is added in turn, and the sample is ground in an agate crucible to mix the components evenly. Then, about 20 mg of the sample is taken and placed in the HCT-3 comprehensive thermal analyzer. The temperature is raised from 20°C to 1400°C at a rate of 10°C / min to observe the combustion of the flake graphite carbon protective slag in an air atmosphere. Figure 3 It can be seen that the combustion temperature range is 600℃-800℃, and the weight loss during the combustion process is 36.84%.

[0033] Example 4

[0034] See also Figure 4The amount of carbonaceous material added to the protective slag is generally adjusted between 2% and 15% to match the continuous casting conditions and the type of steel. In the present invention, 6% straw charcoal is added to the protective slag, wherein the protective slag is a CaO-SiO2-Al2O3 slag system, and the addition ratio of each component of the straw charcoal-carbon protective slag is: CaO is 27.5%; SiO2 is 27.5%; Al2O3 is 12%; Na2O is 14.2%; CaF2 is 10.8%; MgO is 2%; straw charcoal is 6%, and each component is added in turn. The sample is ground in an agate crucible to mix the components evenly, and then about 20 mg of the sample is taken and placed in an HCT-3 comprehensive thermal analyzer. The temperature is raised from 20°C to 1400°C at a rate of 10°C / min to observe the combustion of the straw charcoal-carbon protective slag in an air atmosphere. Figure 4 It can be seen that the combustion temperature range is 570℃-820℃, and the weight loss during the combustion process is 42.33%.

[0035] pass Figure 3 It can be seen that the weight loss of the flake graphite carbon protection slag during combustion is 36.84%. Figure 4 It can be seen that the weight loss of the straw charcoal and carbon protection slag in the combustion process of the present invention is 42.23%. Through the combustion curves of the two carbonaceous materials and the combustion curves of the two carbon protection slags, it can be concluded that the straw charcoal is easier to burn completely in the protection slag, and is a better carbon material for avoiding carbon increase of ultra-low carbon steel and reducing smoke emissions.

[0036] Example 5

[0037] The properties of straw carbon and flake graphite are shown in Table 1

[0038] Table 1: Composition and properties of straw charcoal and flake graphite

[0039] Straw charcoal Flake Graphite Volatile matter / % 13.47 5.48 Ash / % 5.13 1.41 Fixed carbon content / % 80.51 94.47 <![CDATA[Calorific value / MJ·kg -1 > 33.79 36.4 <![CDATA[Specific surface area / m 2 ·g -1 > 1155.73 55.62 Carbon content / % 44.56 72.84 Hydrogen content / % 4.11 2.92 Oxygen content / % 35.25 14.38 Nitrogen content / % 0.62 1.02 Sulfur content / % 0.13 0.35

[0040] It can be seen from Table 1 above that flake graphite, as a commonly used carbon-matching material for protective slag, has higher fixed carbon content and sulfur content than straw charcoal. When used as a carbon-matching material for protective slag, the harmful gases such as carbon dioxide and carbon monoxide produced by flake graphite are much higher than those of straw charcoal.

[0041] See also Figure 5 and Figure 6First, flake graphite and straw charcoal were used as two kinds of protective slags with carbon content of 10%, and the protective slag was CaO-SiO2-Al2O3 slag system. The proportion of each component of the protective slag was: CaO 25.5%; SiO2 25.5%; Al2O3 12%; Na2O 14.2%; CaF2 10.8%; MgO 2%; each component was added in turn, and the sample was ground using an agate crucible to mix the components evenly. Then, about 20 mg of the sample was taken and placed in a synchronous thermal analyzer. The temperature was raised from 20℃ to 1400℃ at a rate of 10℃ / min. The amount of carbon dioxide and carbon monoxide generated by the two protective slags during the heating process was analyzed by a gas mass spectrometer. It can be found that the protective slag with straw charcoal as the carbon material produced less carbon dioxide and carbon monoxide than the protective slag prepared with flake graphite as the carbon material. Therefore, straw charcoal has an important positive significance for environmental protection when used as a carbon material for protective slag.

[0042] The straw charcoal described in the present invention belongs to a kind of biomass charcoal. Straw charcoal is a carbon material with characteristic elements similar to graphite, carbon black, etc. produced by thermal decomposition under the conditions of lack of oxygen, oxygen-free or continuous supply of inert gas. It contains a large amount of carbon and plant nutrients, has a rich pore structure, a large specific surface area and contains more oxygen-containing active groups on the surface. It is a multifunctional material. Table 2 below is a comparison chart of some components of straw charcoal and straw.

[0043] Table 2: Comparison of the composition of straw and straw charcoal

[0044] sample Fixed carbon content / % Volatile matter / % Calorific value / MJ·kg-1 Straw 17.27 19.70 33.79 Straw charcoal 80.51 5.13 18.80

[0045] Compared with organic matter such as straw, biochar such as straw has a higher fixed carbon content and lower volatile matter. It has carbon materials with characteristic elements such as graphite and carbon black. It will not burn directly like organic matter as a protective slag additive, and has an excellent melting effect. In addition, organic materials such as straw decompose rapidly and increase the emission of greenhouse gases such as N2O. The biochar converted from biomass such as straw is stable and difficult to decompose. It can effectively "lock" the carbon pool and slow down its decomposition rate back to the atmosphere, which is of great help to the environment.

[0046] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. Application of straw charcoal as carbon in the production of IF steel protective slag.

2. The use of straw charcoal as carbon blend in the production of IF steel protection slag according to claim 1, characterized in that: The IF steel protective slag is composed of a CaO-SiO2-Al2O3 slag system and straw charcoal. The components of the CaO-SiO2-Al2O3 slag system include: CaO, SiO2, Al2O3, Na2O, CaF2 and MgO.

3. The use of straw charcoal as carbon blend in the production of IF steel protection slag according to claim 2, characterized in that: The ratio of CaO to SiO2 in the protective slag is 1:

1.

4. The use of straw charcoal as carbon blend in the production of IF steel protection slag according to claim 2 or 3, characterized in that: Use the following method: S1: Add CaO, SiO2, Al2O3, Na2O, CaF2, MgO and straw charcoal into an agate crucible in sequence; S2: Grind the added materials in an agate crucible and mix them evenly to obtain protective slag.

5. The use of straw charcoal as carbon blend in the production of IF steel protection slag according to claim 4, characterized in that: The content of the straw charcoal as a carbon-matching material in the protective slag is 6-10%.

Citation Information

Cited By

  • Nano graphite powder as well as preparation method and application thereof

    CN120117601A

  • Casting powder in ultra-low carbon steel production and application thereof

    CN121624377A