Smelting method of low-density steel

By controlling the heating rate and vacuum degree in the smelting furnace, combined with the treatment of carbon powder and manganese metal, the problem of high Class B inclusion content in low-density steel is solved, and the cleanliness and smelting efficiency of the molten steel is improved.

CN118879985APending Publication Date: 2024-11-01NINGBO IRON & STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028159.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

How to control the content of Class B inclusions in low-density steel to ensure its cleanliness.

Method used

Scrap steel is melted in a smelting furnace, the heating rate and vacuum degree are controlled, and the oxide and nitrogen content in the steel liquid is reduced through multi-step pretreatment and alloying process, and the formation of Class B inclusions is reduced. The specific steps include adjusting the heating rate and vacuum degree within different temperature ranges, and using carbon powder and manganese metal to deoxygenate and nitrogen removal treatment to ensure the cleanliness of the steel liquid.

Benefits of technology

It effectively reduces the content of Class B inclusions in low-density steel, improves the cleanliness and smelting efficiency of steel, reduces the precipitation of oxides and nitrogen, and avoids liquid steel splashing and excessively rapid scrap melting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879985A_ABST
    Figure CN118879985A_ABST
Patent Text Reader

Abstract

The invention provides a smelting method of low-density steel, and relates to the technical field of ferrous metallurgy, the smelting method of the low-density steel comprises the following steps: S1, smelting waste steel in a smelting furnace to obtain smelted molten steel; s2, the temperature of the molten steel is increased to 1540-1550 DEG C, meanwhile, the vacuum degree in the furnace is not higher than 50 Pa, and pretreated molten steel is obtained; wherein the heating rate is 1-5 DEG C / min; s3, alloying the pretreated smelted molten steel to obtain alloyed molten steel; and S4, the alloyed molten steel is poured, and the low-density steel is obtained. According to the method, by controlling the heating rate and the vacuum degree in the furnace in the heating process in the step S1, the content of B-type inclusions in the low-density steel can be reduced, and therefore it is guaranteed that the low-density steel has high cleanliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a method for smelting low-density steel. Background Art

[0002] Relevant surveys show that about 23% of carbon dioxide emissions come from automobile transportation; in addition, transportation is the largest end user of oil and other liquid fuel consumption, accounting for more than 50%. Therefore, reducing carbon dioxide emissions and fuel consumption is a challenge facing the automotive industry. One of the most important ways to achieve the above goals is to reduce the weight of the vehicle body structure. Taking a Class A car as an example, its body-in-white weight is about 350kg. If the body structure weight is reduced by 10%, it can save 6-8% of fuel and reduce exhaust emissions by 5-6%. Therefore, lightweighting is the future development path of the automotive industry. Lightweighting of automobiles can be achieved in the following two ways: (1) Improving the strength of steel plates, thereby reducing the size of automotive parts. (2) Reducing the density of steel plates.

[0003] The main method to reduce the density of steel materials is to add low-density elements, such as Al and Mn, to the composition of steel. The Al element has a significant effect on the density of steel. For every 1% of Al added to steel, the density of steel decreases by about 1.3%; the addition of Mn also has a certain weight reduction effect. For every 1% of Mn added to steel, the density of steel decreases by about 0.1%; Among them, the mechanism of Al element reducing the density of steel can be divided into two aspects: on the one hand, the alloy element Al element solid solution in the matrix expands the lattice constant of steel and increases the unit cell volume; on the other hand, the atomic mass of Al element is relatively low.

[0004] However, Al, as an active metal, has a strong affinity with O, N, etc. The Al content in conventional density steel products is generally below 0.035%. During the smelting process, the Al element in this content range has the effect of deoxidation and nitrogen fixation, thereby improving the mechanical properties of the steel product. The Al content in low-density steel is relatively high, about 3%. When the Al content in the steel is high, a large amount of Class B inclusions are more likely to form in the steel, which deteriorates the cleanliness of the steel. Therefore, how to control the content of Class B inclusions in low-density steel (the Al content is about 3%), thereby ensuring that the low-density steel has a high cleanliness, is a problem that needs to be solved urgently. Summary of the invention

[0005] The problem solved by the invention is: how to control the content of B-type inclusions in low-density steel, so as to ensure that the low-density steel has a higher cleanliness.

[0006] In order to solve the above problems, the present invention provides a smelting method of low-density steel. The components of the low-density steel include, by weight percentage: C: 0.48-0.52%, Si: 0-0.05%, Mn: 4.90-5.10%, P: 0-0.020%, S: 0-0.020%, Al: 2.90-3.10%, and the balance is Fe and unavoidable impurities;

[0007] The smelting method of the low-density steel comprises:

[0008] Step S1, smelting scrap steel in a smelting furnace to obtain molten steel;

[0009] Step S2, heating the molten steel to 1540-1550°C, while making the vacuum degree in the furnace no higher than 50Pa, to obtain pre-treated molten steel; wherein the heating rate is 1-5°C / min;

[0010] Step S3, alloying the pre-treated molten steel to obtain alloyed molten steel;

[0011] Step S4, pouring the alloyed molten steel to obtain low-density steel;

[0012] Wherein, the step S1 comprises:

[0013] Step S11, adding the scrap steel into the smelting furnace, raising the temperature inside the smelting furnace to a first temperature, and performing heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 300-400° C.;

[0014] Step S12, raising the temperature in the smelting furnace to a second temperature, and performing heat preservation treatment until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1480-1535° C.;

[0015] Wherein, the heating rate and the vacuum degree in the furnace during the heating process of the step S1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 30-40°C / min, and P≤500Pa; when T is 300-400°C, V is 5-10°C / min, and P≤200Pa; when 400°C<T<1400°C, V is 30-40°C / min, and P≤100Pa; when 1400°C≤T<1480°C, V is 15-20°C / min, and P≤100Pa; when 1480°C≤T≤1535°C, V is 5-10°C / min, and P≤200Pa.

[0016] Optionally, in step S11, the insulation treatment time is 10-20 minutes.

[0017] Optionally, step S3 includes:

[0018] Step S31, controlling the temperature of the pre-treated molten steel to 1540-1550°C, controlling the vacuum degree in the furnace to 15-50Pa, adding carbon powder and performing heat preservation treatment to obtain the first intermediate molten steel;

[0019] Step S32, adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel;

[0020] Step S33, adding aluminum powder to the second intermediate molten steel, and homogenizing it to obtain a third intermediate molten steel;

[0021] Step S34, filling the smelting furnace with inert gas, controlling the temperature of the third intermediate smelting molten steel to 1495-1510° C., adding metallic manganese, controlling the temperature of the molten steel to 1460-1480° C., and performing homogenization treatment to obtain alloyed molten steel.

[0022] Optionally, in step S31, the insulation treatment time is 5-10 minutes.

[0023] Optionally, in step S31, the amount of carbon powder added is 1.29-1.62 kg / ton of molten steel.

[0024] Optionally, in step S32, the amount of carbon powder added is 4.86-5.16 kg / ton of molten steel.

[0025] Optionally, in step S33, the amount of aluminum powder added is 30.79-32.88 kg / ton of molten steel.

[0026] Optionally, in step S33, the homogenization treatment time is 3-5 minutes.

[0027] Optionally, in step S34, the amount of metallic manganese added is 50.96-51.86 kg / ton of molten steel.

[0028] Optionally, in step S34, the homogenization treatment time is 3-5 minutes.

[0029] Compared with the prior art, in the process of smelting scrap steel in the smelting furnace, the present invention starts to heat the scrap steel while ensuring that the vacuum degree in the furnace is not higher than 500Pa, and controls the heating rate to be 30-40°C / min, so that the scrap steel is quickly heated to bake the refractory material, which can reduce the smelting time and improve the smelting efficiency; in the process of heating, when T is 300-400°C, the vacuum degree in the furnace is further reduced (P≤200Pa), and the heating rate is reduced (V is 5-10°C / min), so that the refractory material and scrap steel in the smelting furnace are quickly dried, and water and iron are prevented from reacting to form iron oxides at a subsequent higher temperature, thereby further reducing the oxide content in the molten steel, which is beneficial to reducing the content of Class B inclusions in low-density steel; when 400°C<T<1400°C, the vacuum degree in the furnace is further reduced (P≤100Pa), and the heating rate is increased (V is 30- 40℃ / min), which can reduce the smelting time and improve the smelting efficiency; when 1400℃≤T<1480℃, the scrap steel in the lower part of the smelting furnace has begun to melt gradually and slowly. At this time, the heating rate is reduced to 15-20℃ / min, and the vacuum degree in the furnace is P≤100Pa, so that the gas partial pressure in the smelting furnace is low, which prompts O in the molten steel to react with C in the molten steel to produce CO bubbles. The CO bubbles can carry N to precipitate, thereby removing O and N in the molten steel, which is beneficial to further reduce the content of Class B inclusions in low-density steel; when 1480℃≤T≤1535℃, the scrap steel enters the rapid melting stage, the heating rate is reduced to 5-10℃ / min, and the vacuum degree in the furnace is P≤200Pa, so that O and N in the molten steel are slowly precipitated, and the scrap steel can be prevented from melting too quickly due to too fast heating rate and too high vacuum, thereby avoiding the splashing of molten steel. In the present invention, after the scrap steel is completely melted, the heating rate is controlled to be 1-5°C / min, and the vacuum degree in the furnace is not higher than 50Pa, which is conducive to further removing O and N elements in the molten steel and further ensuring that the low-density steel has a lower content of class B inclusions. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of a process for smelting low-density steel in an embodiment of the present invention;

[0031] Figure 2 This is a metallographic structure picture of the low-density steel prepared in Example 1;

[0032] Figure 3 This is a metallographic structure picture of the low-density steel prepared in Example 2;

[0033] Figure 4 This is a metallographic structure picture of the low-density steel prepared in Example 3;

[0034] Figure 5 This is a metallographic structure picture of the low-density steel prepared in Comparative Example 1;

[0035] Figure 6 This is a metallographic structure picture of the low-density steel prepared in Comparative Example 2. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0037] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0038] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0039] In addition, it should be noted that Kg / ton of molten steel in the present invention refers to the amount of a substance added per ton of molten steel. The vacuum degree in the furnace refers to the vacuum degree in the smelting furnace. Class B inclusions refer to alumina inclusions.

[0040] like Figure 1As shown, a smelting method of low-density steel provided by an embodiment of the present invention, wherein the components of the low-density steel include, by weight percentage: C: 0.48-0.52%, Si: 0-0.05%, Mn: 4.90-5.10%, P: 0-0.020%, S: 0-0.020%, Al: 2.90-3.10%, and the balance is Fe and unavoidable impurities;

[0041] The smelting method of the low-density steel comprises:

[0042] Step S1, smelting scrap steel in a smelting furnace to obtain molten steel;

[0043] Step S2, heating the molten steel to 1540-1550°C, while making the vacuum degree in the furnace no higher than 50Pa, to obtain pre-treated molten steel; wherein the heating rate is 1-5°C / min;

[0044] Step S3, alloying the pre-treated molten steel to obtain alloyed molten steel;

[0045] Step S4, pouring the alloyed molten steel to obtain low-density steel;

[0046] Wherein, the step S1 comprises:

[0047] Step S11, adding the scrap steel into the smelting furnace, raising the temperature inside the smelting furnace to a first temperature, and performing heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 300-400° C.;

[0048] Step S12, raising the temperature in the smelting furnace to a second temperature, and performing heat preservation treatment until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1480-1535° C.;

[0049] Wherein, the heating rate and the vacuum degree in the furnace during the heating process of the step S1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 30-40°C / min, and P≤500Pa; when T is 300-400°C, V is 5-10°C / min, and P≤200Pa; when 400°C<T<1400°C, V is 30-40°C / min, and P≤100Pa; when 1400°C≤T<1480°C, V is 15-20°C / min, and P≤100Pa; when 1480°C≤T≤1535°C, V is 5-10°C / min, and P≤200Pa.

[0050] In the process of smelting scrap steel in a smelting furnace according to the embodiment of the present invention, while ensuring that the vacuum degree in the furnace is not higher than 500Pa, the scrap steel is started to be heated, and the heating rate is controlled to be 30-40°C / min, so that the scrap steel is quickly heated to bake the refractory material, which can reduce the smelting time and improve the smelting efficiency; in the process of heating, when T is 300-400°C, the vacuum degree in the furnace is further reduced (P≤200Pa), and the heating rate is reduced (V is 5-10°C / min), so as to promote the rapid drying of the refractory material and the scrap steel in the smelting furnace, and avoid the reaction of water and iron at a higher temperature to generate iron oxides, thereby further reducing the oxide content in the molten steel, which is beneficial to reducing the content of Class B inclusions in low-density steel; when 400°C<T<1400°C, the vacuum degree in the furnace is further reduced (P≤100Pa), and the heating rate is increased (V is 30-40°C / min), so as to reduce the content of Class B inclusions in low-density steel. / min), which can reduce the smelting time and improve the smelting efficiency; when 1400℃≤T<1480℃, the scrap steel in the lower part of the smelting furnace has begun to melt gradually and slowly. At this time, the heating rate is reduced to 15-20℃ / min, and the vacuum degree in the furnace is P≤100Pa, so that the gas partial pressure in the smelting furnace is low, which prompts O in the molten steel to react with C in the molten steel to produce CO bubbles. The CO bubbles can carry N to precipitate, thereby removing O and N in the molten steel, which is beneficial to further reduce the content of Class B inclusions in low-density steel; when 1480℃≤T≤1535℃, the scrap steel enters the rapid melting stage, the heating rate is reduced to 5-10℃ / min, and the vacuum degree in the furnace is P≤200Pa, so that O and N in the molten steel are slowly precipitated, and the scrap steel can be prevented from melting too quickly due to too fast heating rate and too high vacuum, thereby avoiding the splashing of molten steel. In the embodiment of the present invention, after the scrap steel is completely melted, the heating rate is controlled to be 1-5°C / min, and the vacuum degree in the furnace is not higher than 50Pa, which is conducive to further removing O and N elements in the molten steel and further ensuring that the low-density steel has a lower content of class B inclusions.

[0051] In some embodiments of the present invention, in step S11, the insulation treatment time is 10-20 minutes, thereby ensuring that the moisture in the refractory material and scrap steel in the smelting furnace is fully removed.

[0052] In some embodiments of the present invention, step S3 includes:

[0053] Step S31, controlling the temperature of the pre-treated molten steel to 1540-1550°C, controlling the vacuum degree in the furnace to 15-50Pa, adding carbon powder and performing heat preservation treatment to obtain the first intermediate molten steel;

[0054] Step S32, adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel;

[0055] Step S33, adding aluminum powder to the second intermediate molten steel, and homogenizing it to obtain a third intermediate molten steel;

[0056] Step S34, filling the smelting furnace with inert gas, controlling the temperature of the third intermediate smelting molten steel to 1495-1510° C., adding metallic manganese, controlling the temperature of the molten steel to 1460-1480° C., and performing homogenization treatment to obtain alloyed molten steel.

[0057] In this embodiment, first, the temperature of the pre-treatment molten steel is controlled to 1540-1550° C., and the vacuum degree in the furnace is controlled to 15-50 Pa, so as to ensure that all the scrap steel can be melted and the molten steel has good fluidity, which is convenient for subsequent alloying; then, a small amount of carbon powder should be added to the pre-treatment molten steel, and the carbon powder is used to reduce the oxides in the molten steel, and further remove the O element in the molten steel. The CO bubbles generated in this process can carry N to precipitate; because the Mn element is volatile at high temperature, before adding metallic manganese, the temperature of the molten steel is reduced to 1495-1510° C., and inert gas is filled to reduce the volatilization of the Mn element, and the temperature of the molten steel is close to the liquidus, so as to ensure that the subsequent casting is carried out in a low superheat and protective atmosphere, thereby achieving the purpose of rapid solidification and further reducing the oxidation of the steel.

[0058] In some embodiments of the present invention, in step S31, the insulation treatment time is 5-10 minutes.

[0059] In some embodiments of the present invention, in step S31, the amount of carbon powder added is 1.29-1.62 kg / ton of molten steel.

[0060] In some embodiments of the present invention, in step S32, the amount of carbon powder added is 4.86-5.16 kg / ton of molten steel.

[0061] In some embodiments of the present invention, in step S33, the amount of aluminum powder added is 30.79-32.88 kg / ton of molten steel, and the homogenization treatment time is 3-5 min.

[0062] In some embodiments of the present invention, in step S34, the amount of metallic manganese added is 50.96-51.86 kg / ton of molten steel, and the homogenization treatment time is 3-5 min.

[0063] The present invention is further described below in conjunction with specific embodiments.

[0064] Example 1

[0065] A1. Smelting scrap steel in a smelting furnace to obtain molten steel; wherein the step A1 comprises:

[0066] A11, adding the scrap steel into the smelting furnace, raising the temperature inside the smelting furnace to a first temperature, and performing heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 300° C.;

[0067] A12, raising the temperature in the smelting furnace to a second temperature, and performing heat preservation treatment until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1523° C.;

[0068] The heating rate and the vacuum degree in the furnace during the heating process of step A1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 35°C / min, and P is 500Pa; when T is 300-400°C, V is 6°C / min, and P is 200Pa; when 400°C<T<1400°C, V is 35°C / min, and P is 89Pa; when 1400°C≤T<1480°C, V is 18°C / min, and P is 89Pa; when 1480°C≤T≤1523°C, V is 8°C / min, and P is 176Pa.

[0069] A2. The molten steel is heated to 1550° C. and the vacuum degree in the furnace is set to 47 Pa to obtain pretreated molten steel; wherein the heating rate is 3° C. / min.

[0070] A3. Control the temperature of the pre-treated molten steel to 1543° C., control the vacuum degree in the furnace to 50 Pa, add carbon powder and perform insulation treatment to obtain the first intermediate molten steel; wherein the insulation treatment time is 8 min, and the amount of carbon powder added is 1.29 kg / ton of molten steel.

[0071] A4. Adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel; wherein the amount of the carbon powder added is 5.16 kg / ton of molten steel.

[0072] A5. Add aluminum powder to the second intermediate molten steel and perform homogenization treatment to obtain a third intermediate molten steel; wherein the amount of aluminum powder added is 32.88 kg / ton of molten steel, and the homogenization treatment time is 5 min.

[0073] A6. Inert gas is charged into the smelting furnace, the temperature of the third intermediate molten steel is controlled to 1500° C., metallic manganese is added, homogenization treatment is performed, and the temperature of the molten steel is controlled to 1475° C. to obtain alloyed molten steel; wherein the amount of metallic manganese added is 51.58 kg / ton of molten steel, and the homogenization treatment time is 3 min.

[0074] A7. The alloyed molten steel is poured to obtain low-density steel; the components of the low-density steel include, by weight percentage: C: 0.50%, Si: 0.005%, Mn: 5.02%, P: 0.005%, S: 0.003%, Al: 3.06%, and the balance is Fe and unavoidable impurities.

[0075] Example 2

[0076] A1. Smelting scrap steel in a smelting furnace to obtain molten steel; wherein the step A1 comprises:

[0077] A11. Add the scrap steel into the smelting furnace, raise the temperature in the smelting furnace to a first temperature, and perform heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 343° C.;

[0078] A12, raising the temperature in the smelting furnace to a second temperature, and maintaining the temperature until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1519° C.;

[0079] The heating rate and the vacuum degree in the furnace during the heating process of step A1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 40°C / min, and P is 414Pa; when T is 300-400°C, V is 8°C / min, and P is 193Pa; when 400°C<T<1400°C, V is 40°C / min, and P is 100Pa; when 1400°C≤T<1480°C, V is 20°C / min, and P is 100Pa; when 1480°C≤T≤1519°C, V is 10°C / min, and P is 183Pa.

[0080] A2. The molten steel is heated to 1540° C. and the vacuum degree in the furnace is set to 50 Pa to obtain pretreated molten steel; wherein the heating rate is 5° C. / min.

[0081] A3. Control the temperature of the pre-treated molten steel to 1550° C., control the vacuum degree in the furnace to 15 Pa, add carbon powder and perform heat preservation treatment to obtain the first intermediate molten steel; wherein the heat preservation treatment time is 8 min, and the amount of carbon powder added is 1.40 kg / ton of molten steel.

[0082] A4. Adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel; wherein the amount of the carbon powder added is 4.97 kg / ton of molten steel.

[0083] A5. Add aluminum powder to the second intermediate molten steel and perform homogenization treatment to obtain a third intermediate molten steel; wherein the amount of aluminum powder added is 31.85 kg / ton of molten steel, and the homogenization treatment time is 5 min.

[0084] A6. Inert gas is charged into the smelting furnace, the temperature of the third intermediate molten steel is controlled to 1510° C., metallic manganese is added, homogenization treatment is performed, and the temperature of the molten steel is controlled to 1480° C. to obtain alloyed molten steel; wherein the amount of metallic manganese added is 50.96 kg / ton of molten steel, and the homogenization treatment time is 5 min.

[0085] A7. The alloyed molten steel is poured to obtain low-density steel; the components of the low-density steel include, by weight percentage: C: 0.49%, Si: 0.005%, Mn: 4.98%, P: 0.005%, S: 0.003%, Al: 3.01%, and the balance is Fe and unavoidable impurities.

[0086] Example 3

[0087] A1. Smelting scrap steel in a smelting furnace to obtain molten steel; wherein the step A1 comprises:

[0088] A11. Add the scrap steel into the smelting furnace, raise the temperature in the smelting furnace to a first temperature, and perform heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 315° C.;

[0089] A12, raising the temperature in the smelting furnace to a second temperature, and maintaining the temperature until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1535° C.;

[0090] The heating rate and the vacuum degree in the furnace during the heating process of step A1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 30°C / min, and P is 453Pa; when T is 300-400°C, V is 6°C / min, and P is 190Pa; when 400°C<T<1400°C, V is 30°C / min, and P is 96Pa; when 1400°C≤T<1480°C, V is 15°C / min, and P is 96Pa; when 1480°C≤T≤1535°C, V is 5°C / min, and P is 200Pa.

[0091] A2. The molten steel is heated to 1545° C. and the vacuum degree in the furnace is set to 35 Pa to obtain pretreated molten steel; wherein the heating rate is 3° C. / min.

[0092] A3. Control the temperature of the pre-treated molten steel to 1540° C., control the vacuum degree in the furnace to 15 Pa, add carbon powder and perform heat preservation treatment to obtain the first intermediate molten steel; wherein the heat preservation treatment time is 5 min, and the amount of carbon powder added is 1.62 kg / ton of molten steel.

[0093] A4. Adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel; wherein the amount of the carbon powder added is 4.86 kg / ton of molten steel.

[0094] A5. Add aluminum powder to the second intermediate molten steel and perform homogenization treatment to obtain a third intermediate molten steel; wherein the amount of aluminum powder added is 30.79 kg / ton of molten steel, and the homogenization treatment time is 3 min.

[0095] A6. Inert gas is charged into the smelting furnace, the temperature of the third intermediate molten steel is controlled to 1495° C., metallic manganese is added, homogenization treatment is performed, and the temperature of the molten steel is controlled to 1470° C. to obtain alloyed molten steel; wherein the amount of metallic manganese added is 51.86 kg / ton of molten steel, and the homogenization treatment time is 3 min.

[0096] A7. The alloyed molten steel is poured to obtain low-density steel; the components of the low-density steel include, by weight percentage: C: 0.51%, Si: 0.005%, Mn: 5.03%, P: 0.005%, S: 0.003%, Al: 2.98%, and the balance is Fe and unavoidable impurities.

[0097] Comparative Example 1

[0098] The difference from Example 1 is that during the heating process of step A1, when T is 1400-1480°C, V is 10°C / min and P is 300Pa.

[0099] Comparative Example 2

[0100] The difference from Example 1 is that step A2 is: heating the molten steel to 1540°C, while making the vacuum degree in the furnace 100Pa, to obtain pretreated molten steel; wherein the heating rate is 10°C / min.

[0101] Experimental example

[0102] The metallographic impurities of the low-density steel obtained in Examples 1-3 and Comparative Examples 1-2 were characterized. Figure 2-6 ,from Figure 2-4 It can be seen that the metallographic inclusion ratings of the low-density steels prepared in Examples 1-3 are BT0.5, BT0.5 and BT0.5 respectively. Figure 5-6It can be seen that the metallographic inclusion ratings in the low-density steels prepared in Comparative Examples 1-2 are BT1.5 and BT1.0, respectively. It can be seen that compared with Comparative Examples 1-2, the Class B inclusion rating in the low-density steels prepared in Examples 1-3 is lower, that is, the Class B inclusions in the low-density steels prepared in Examples 1-3 are lower in content and smaller in size.

[0103] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for smelting low-density steel, characterized in that: The components of the low-density steel include, by weight percentage: C: 0.48-0.52%, Si: 0-0.05%, Mn: 4.90-5.10%, P: 0-0.020%, S: 0-0.020%, Al: 2.90-3.10%, and the balance is Fe and unavoidable impurities; The smelting method of the low-density steel comprises: Step S1, smelting scrap steel in a smelting furnace to obtain molten steel; Step S2, heating the molten steel to 1540-1550°C, while making the vacuum degree in the furnace no higher than 50Pa, to obtain pre-treated molten steel; wherein the heating rate is 1-5°C / min; Step S3, alloying the pre-treated molten steel to obtain alloyed molten steel; Step S4, pouring the alloyed molten steel to obtain low-density steel; Wherein, the step S1 comprises: Step S11, adding the scrap steel into the smelting furnace, raising the temperature inside the smelting furnace to a first temperature, and performing heat preservation treatment to obtain preheated scrap steel; wherein the first temperature is 300-400° C.; Step S12, raising the temperature in the smelting furnace to a second temperature, and performing heat preservation treatment until the preheated scrap steel is completely melted to obtain molten steel; wherein the second temperature is 1480-1535° C.; Wherein, the heating rate and the vacuum degree in the furnace during the heating process of the step S1 are controlled as follows: the furnace temperature of the smelting furnace is T, the heating rate is V, and the vacuum degree in the furnace is P; when T is less than 300°C, V is 30-40°C / min, and P≤500Pa; when T is 300-400°C, V is 5-10°C / min, and P≤200Pa; when 400°C<T<1400°C, V is 30-40°C / min, and P≤100Pa; when 1400°C≤T<1480°C, V is 15-20°C / min, and P≤100Pa; when 1480°C≤T≤1535°C, V is 5-10°C / min, and P≤200Pa.

2. The method for smelting low-density steel according to claim 1, characterized in that: In the step S11, the heat preservation treatment time is 10-20 minutes.

3. The method for smelting low-density steel according to claim 1, characterized in that: The step S3 comprises: Step S31, controlling the temperature of the pre-treated molten steel to 1540-1550°C, controlling the vacuum degree in the furnace to 15-50Pa, adding carbon powder and performing heat preservation treatment to obtain the first intermediate molten steel; Step S32, adding carbon powder to the first intermediate molten steel again to obtain a second intermediate molten steel; Step S33, adding aluminum powder to the second intermediate molten steel, and homogenizing it to obtain a third intermediate molten steel; Step S34, filling the smelting furnace with inert gas, controlling the temperature of the third intermediate smelting molten steel to 1495-1510° C., adding metallic manganese, controlling the temperature of the molten steel to 1460-1480° C., and performing homogenization treatment to obtain alloyed molten steel.

4. The method for smelting low-density steel according to claim 3, characterized in that: In step S31, the insulation treatment time is 5-10 minutes.

5. The method for smelting low-density steel according to claim 3, characterized in that: In the step S31, the amount of carbon powder added is 1.29-1.62 kg / ton of molten steel.

6. The method for smelting low-density steel according to claim 3, characterized in that: In the step S32, the amount of carbon powder added is 4.86-5.16 kg / ton of molten steel.

7. The method for smelting low-density steel according to claim 3, characterized in that: In step S33, the amount of aluminum powder added is 30.79-32.88 kg / ton of molten steel.

8. The method for smelting low-density steel according to claim 3, characterized in that: In step S33, the homogenization treatment time is 3-5 minutes.

9. The method for smelting low-density steel according to claim 3, characterized in that: In the step S34, the amount of metallic manganese added is 50.96-51.86 kg / ton of molten steel.

10. The method for smelting low-density steel according to claim 3, characterized in that: In step S34, the homogenization treatment time is 3-5 minutes.