Production method for thinning HRB500E niobium-added steel bar pearlite interlamellar spacing
By using high nitrogen + niobium and vanadium microalloy systems in rebar, changing the recrystallization temperature characteristics and refining the grain boundaries, the problem of insufficient flexibility and ductility of rebar in the prior art is solved, and the strength is not reduced In the case of improving the ductile performance of steel bars and reducing production costs.
Patent Information
- Application Number
- CN202410935719.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to improve the flexibility and ductility of rebar HRB500E without reducing strength, especially in meeting the toughness and ductility requirements of the new national standard for seismic steel bars while reducing production costs.
Using high nitrogen + niobium and vanadium microalloy systems, by changing the recrystallization temperature characteristics of rebar, selecting appropriate temperature intervals for deformation, thinning the spacing of pearlite sheets, refining ferrite grains, and increasing the precipitation of nitrides , to promote NbN, VN, etc. to precipitate at the austenite grain boundary, refine the grain boundary, and then shorten the length of the pearlite sheet and change its growth direction, thereby improving the extension performance of the steel bars.
On the basis of maintaining strength, the ductility and toughness of the steel bars are significantly improved, the Agt and R°m/R°eL indicators of seismic steel bars are improved, and the production cost is reduced by 0.2-0.5%, meeting the performance of the new national standard against seismic steel bars is achieved. Require.
Smart Images

Figure CN118880002A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of threaded steel production, in particular to a production method for thinning the pearlite lamellar spacing of HRB500E niobium-added steel bars. Background Art
[0002] Rebar is a steel material that is not available in building frames. The new standard for rebar (Steel for Reinforced Concrete GB / T1499.2-2018) has clear provisions on the nitrogen content of the element: "7.2.3 The nitrogen content of steel shall not exceed 0.012wt%. No analysis is required if the supplier can guarantee this. If there is a sufficient amount of nitrogen-binding elements in the steel, the limit on the nitrogen content may be appropriately relaxed." In other words, if nitrogen-binding elements such as V, Nb, and Ti are added to the steel, the nitrogen content of the steel can be greater than 0.012wt%.
[0003] The biggest difference between non-seismic and seismic steel bars in the national standard "Steel for reinforced concrete" GB / T1499.2-2018 is that: ① The maximum force total elongation Agt of seismic steel bar HRB500E is more than 1.5% higher than that of non-seismic HRB500 (Agt of HRB500E ≥ 9.0%, Agt of HRB500 ≥ 7.5%); ② The strength-yield ratio R of HRB500E ° m / R ° eL ≥1.25, yield strength ratio R ° eL / R eL ≤1.30, while HRB500 has no restrictions on strength-to-yield ratio and yield-to-yield ratio.
[0004] There are two main structures in threaded steel: ferrite and pearlite. Ferrite has good ductility and toughness, but low strength; while pearlite has high strength, certain ductility, and poor toughness. Elements such as V, Nb, Ti, and N are added to steel. One is to use their precipitation strengthening to increase the strength of the steel bar, and to appropriately reduce the amount of ferrite and increase the amount of pearlite to improve the strength; the other is to use the fine grains precipitated to pin the grain boundaries and refine the grains, especially the ferrite grain size, to simultaneously improve the strength, severity, and toughness.
[0005] With the implementation of the new national standard and the large-scale use of high-strength earthquake-resistant steel bars, the above-mentioned process technology is difficult to meet the requirements of good toughness and ductility of steel while reducing production costs. The present invention adopts: high nitrogen + niobium, vanadium microalloy system, using niobium elements to change the recrystallization temperature characteristics of threaded steel, selecting an appropriate temperature range for deformation, thinning the pearlite lamella spacing, and improving the flexibility of pearlite without reducing strength, thereby improving the ductility of the steel bar and ensuring the A, Agt, R of the earthquake-resistant steel bar. ° m / R °eL index.
[0006] Pearlite is a lamellar structure, which is a mechanical mixture of ferrite and cementite, that is, a layer of ferrite covered by a layer of cementite. The lamellar spacing of pearlite is 150-450nm (the lamellar spacing is about 80-150nm for troostite, and the lamellar spacing is about 30-80nm for troostite; as the tire cord steel standard clearly requires, the troostite structure in the steel is >85%). Under the same strength, the elongation of troostite steel is 15-25% higher than that of pearlite steel, and that of troostite steel is as high as 40-50%. Therefore, reducing the lamellar spacing of pearlite can slightly increase the strength while greatly improving the elongation performance.
[0007] Through searching domestic relevant databases and network information, it was found that "The influence of alloying element Nb on the structure and properties of rebar" (Lu Xinxin et al. Industrial Heating, 2021, 50 (4), TG142.33, National Natural Science Foundation), "Research on the technology of stable nitrogen content in HRB500E" (Zhong Yunqing et al. [C] China High-tech, 2019, No. 19: 61-63), "Analysis of nitrogen increase in nitrided alloys" (Fu Yudong. [C] Southern Metals, December 2018, No. 225: 18-20, 30), "Research on the whole process of nitrogen blowing technology for bottom blowing of converter" (Wu Wei et al. No. 8 (2 011) China Steel Annual Conference Special) and other articles and patents such as "HRB500E earthquake-resistant steel bar and its preparation method" (China, CN104745968B, Lin Zhiming et al.), "HRB500E vanadium-nitrogen high-strength earthquake-resistant steel bar and its production method" (China, CN103451516A, Xu Zhidong et al.), "HRB500E niobium-titanium microalloy high-strength earthquake-resistant steel bar and production process" (China, CN201910724803.4, Dou Weixue et al.), and "HRB500 earthquake-resistant and corrosion-resistant steel bar" (China, CN201510286425.8, Ke Xueli et al.).
[0008] These existing articles describe the nitrogen content range of the chromium smelting process of rebar HRB500E. Some articles even list the process parameters such as the pressure and flow rate of bottom blowing nitrogen, but none of them describe how to obtain [N] in steel and the process control measures adopted. Summary of the invention
[0009] The invention provides a production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, which is used to solve the defects in the prior art.
[0010] The present invention is achieved through the following technical solutions:
[0011] A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, comprising the following steps:
[0012] Step 1: Cut the steel billet into small square billets for continuous casting, with a cross-sectional size of 150mm×150mm-165mm×165mm;
[0013] Step 2: sending the small square billet cut in step 1 into a heating furnace for heating;
[0014] Step 3: After heating in step 2, the steel is rolled by a rough rolling unit, a medium rolling unit, and a finishing rolling unit;
[0015] Step 4: After the rolling in step 3 is completed, the temperature in the skirt area is controlled within the range of 890-970°C and maintained for 5-10s to ensure that NbN, VN, etc. are precipitated in the maximum amount at the austenite grain boundary, and the grain boundary is pinned to refine the original austenite grains; then the temperature in the cooling bed alignment roller area is maintained at 610-750°C for 40-100s (the cooling rate of the rolled piece in this area is slow, about 2 / 3 of the other areas of the cooling bed), so as to promote the dispersion and precipitation of NbN, VN, AlN, etc. in the grain, refine the pearlite lamella spacing after phase transformation, shorten the lamella length, change the lamella growth direction, and then cool to room temperature to obtain the finished product.
[0016] According to the production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars as described above, the composition of the steel billet in the step 1 includes the following elements in weight percentage: C: 0.18-0.26wt%; Si: 0.30-0.80wt%; Mn: 1.30-1.60wt%; P: ≤0.045wt%; S: ≤0.045wt%; Nb: 0.008-0.025wt%; V: 0.04-0.08wt%; Al: 0.003-0.008wt%; N: 0.015-0.025wt%; Ceq: ≤0.55wt%; the rest are Fe and unavoidable impurity elements.
[0017] According to the production method of reducing the pearlite interlamellar spacing of HRB500E niobium-added steel bars as described above, the composition of the steel billet includes the following elements in weight percentage: C: 0.21-0.25wt%; Si: 0.30-0.80wt%; Mn: 1.30-1.60wt%; P: ≤0.045wt%; S: ≤0.045wt%; Nb: 0.008-0.016wt%; V: 0.04-0.07wt%; Al: 0.003-0.008wt%; N: 0.015-0.022wt%; Ceq: ≤0.55wt%; the rest are Fe and unavoidable impurity elements.
[0018] In the production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars as described above, the small square billet in step 2 is heated to 1050-1280° C. by a heating furnace.
[0019] In the above-mentioned production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, the starting rolling temperature in step 3 is controlled at 990-1150°C.
[0020] In the above-mentioned production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, the number of rolling passes of the rough rolling unit in step 3 is 6.
[0021] In the above-mentioned production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, the intermediate rolling mill in step 3 has 6 rolling passes.
[0022] In the production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars as described above, the finishing mill of step 3 has 4-6 rolling passes, the temperature before entering the finishing mill is controlled at 930-1080°C, and the temperature of the cooling bed during final rolling is controlled at 920-1050°C.
[0023] In the above-mentioned production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, the final rolling diameter in step three is 10-50 mm.
[0024] According to the production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars, after rolling in step 4, the temperature in the skirt plate area is controlled within the range of 900-960°C and kept warm for 5-8s; then, the temperature is accumulated in the alignment roller area within the range of 620-700°C and kept warm for 50-80s.
[0025] The advantages of the present invention are:
[0026] The present invention, on the basis of refining ferrite grains, focuses on the precipitation of NbN at different temperature stages to reduce the internal structure of pearlite.
[0027] The present invention adds Nb element to steel to change the high temperature recrystallization characteristics of threaded steel, adopts rolling deformation in the non-recrystallization range, refines the original austenite grain size to refine the ferrite grain size, reduces the pearlite plate spacing, etc.
[0028] The nitrogen content of the steel of the present invention is 150-220ppm (the use of converter bottom blowing nitrogen can also reduce costs), which is higher than the nitrogen content of conventional HRB500E of 100-180ppm. The amount of NbN, VN and AlN is increased, so that after a large amount of nitrides are precipitated at the original austenite grain boundaries, there are also abundant nitrides precipitated in the pearlite after the phase transformation, thereby achieving the effect of reducing the pearlite lamella spacing, limiting the lamella growth (forming discontinuous short rod-shaped pearlite), and changing the growth direction of the pearlite lamella clusters, thereby enhancing the metal deformation and slip resistance, improving the strength of the steel, and greatly improving the ductility and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0030] Figure 1 This is a schematic diagram of the shear lip of the fracture in Example 1 of the present invention (2.33 mm);
[0031] Figure 2 This is a schematic diagram of the shear lip of the fracture in Example 4 of the present invention (1.97 mm);
[0032] Figure 3 Schematic diagram of the dimple size at the fracture surface of Example 1 of the present invention (9.5 μm);
[0033] Figure 4 Schematic diagram of the dimple size at the fracture of Example 4 of the present invention (12.7 μm);
[0034] Figure 5 Schematic diagram of pearlite plate spacing in Example 1 of the present invention (148 nm);
[0035] Figure 6 Schematic diagram of pearlite plate spacing in Example 4 of the present invention (206 nm);
[0036] Figure 7 This is a schematic diagram of the pearlite growth direction in Example 1 of the present invention;
[0037] Figure 8 This is a schematic diagram of the pearlite growth direction of Example 4 of the present invention;
[0038] Fig. 9 It is a schematic diagram of the present invention in which NbN and VN restrict the growth of pearlite lamellae (forming discontinuous short rod-shaped pearlite). DETAILED DESCRIPTION
[0039] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] HRB500E is smelted in a 120t converter, with a steel output of about 135t;
[0042] 1) Chemical composition (unit: wt%): C: 0.24, Si: 0.58, Mn: 1.51, P: 0.037, S: 0.034, Nb: 0.012, V: 0.059, Al: 0.004, N: 0.0225, Ceq: 0.50, the rest are Fe and unavoidable impurity elements.
[0043] 2) The cross-sectional dimensions of the continuous casting billet are: 165mm×165mm
[0044] 3) Billet heating: The billet is heated to 1160°C in a heating furnace.
[0045] 4) The rolling temperature is controlled at 1100°C. The rolled piece is rolled by 6 roughing mills and 6 intermediate mills, and then by 4 finishing mills to complete the rolling operation. The temperature of the rolled piece before entering the finishing mill is 1000°C, and the temperature of the cooling bed for final rolling is controlled at 981°C. The rolling specification is Φ20mm.
[0046] 5) Temperature control after final rolling: Control the roller speed after rolling to keep the rolled piece at 930℃ for 6.7s in the skirt area; after quickly passing through the cooling bed (close all ventilation windows under the cooling bed and doors and windows used in the factory in winter; close the ventilation windows under the cooling bed in spring and autumn), the rolled piece is piled on the alignment roller at 660℃ and kept warm for 64s, and then cut to length, packaged and stored after cooling.
[0047] 6) Sampling was performed according to the standard, and the test results were as follows:
[0048]
[0049] Embodiment 2:
[0050] HRB500E is smelted in an 80t converter, with a steel output of about 95t.
[0051] 1) Chemical composition (unit: wt%): C: 0.25, Si: 0.49, Mn: 1.45, P: 0.032, S: 0.029, Nb: 0.009, V: 0.043, Al: 0.008, N: 0.0188, Ceq: 0.50, the rest are Fe and unavoidable impurity elements.
[0052] 2) The cross-sectional dimensions of the continuous casting billet are: 150mm×150mm.
[0053] 3) Billet heating: The billet is heated to 1060°C in a heating furnace.
[0054] 4) The starting rolling temperature is controlled at 962°C. The rolled piece is rolled by 6 rough rolling mills and 6 intermediate rolling mills, and then rolled by 5 finishing mills. The rolling operation is completed. The temperature of the rolled piece before entering the finishing mill is controlled at 952°C, and the temperature of the cooling bed for final rolling is controlled at 925°C. The rolling specification is Φ12mm.
[0055] 5) Temperature control after final rolling: Control the roller speed after rolling to keep the rolled piece at 908℃ for 5.1s in the skirt area; after quickly passing through the cooling bed (close all ventilation windows under the cooling bed and doors and windows used in the factory in winter; close the ventilation windows under the cooling bed in spring and autumn), the rolled piece is piled on the alignment roller at 624℃ and kept warm for 46s, and then cut to length, packaged and stored after cooling.
[0056] 6) Sampling was performed according to the standard, and the test results were as follows:
[0057]
[0058] Embodiment 3:
[0059] HRB500E is smelted in a 150t converter, with a steel output of about 175t;
[0060] 1) Chemical composition (unit: wt%): C: 0.22, Si: 0.74, Mn: 1.55, P: 0.043, S: 0.039, Nb: 0.016, V: 0.071, Al: 0.006, N: 0.0202, Ceq: 0.49, the rest are Fe and unavoidable impurity elements.
[0061] 2) The cross-sectional dimensions of the continuous casting billet are: 165mm×165mm.
[0062] 3) Billet heating: The billet is heated to 1258°C in a heating furnace.
[0063] 4) The starting rolling temperature is controlled at 1147℃. The rolled piece is rolled by 6 rough rolling mills and 6 intermediate rolling mills, and then rolled by 6 finishing mills. The rolling operation is completed. The temperature of the rolled piece before entering the finishing mill is controlled at 1075℃, and the temperature of the cooling bed for final rolling is controlled at 1042℃. The rolling specification is Φ32mm.
[0064] 5) Temperature control after final rolling: Control the roller speed after rolling to keep the rolled piece at 953℃ for 7.8s in the skirt area; after quickly passing through the cooling bed (close all ventilation windows under the cooling bed and doors and windows used in the factory in winter; close the ventilation windows under the cooling bed in spring and autumn), the rolled piece is piled on the alignment roller at 698℃ and kept warm for 79s, and then cut to length, packaged and stored after cooling.
[0065] 6) Sampling was performed according to the standard, and the test results were as follows:
[0066]
[0067] Comparative Example (without Nb):
[0068] HRB500E is smelted in a 120t converter, with a steel output of about 135t;
[0069] 1) Chemical composition (unit: wt%): C: 0.23, Si: 0.62, Mn: 1.49, P: 0.039, S: 0.026, Nb: 0.002, V: 0.068, Al: 0.004, N: 0.0165%, Ceq: 0.48, the rest are Fe and unavoidable impurity elements.
[0070] 2) The cross-sectional dimensions of the continuous casting billet are: 165mm×165mm.
[0071] 3) Billet heating: The billet is heated to 1158°C in a heating furnace.
[0072] 4) The starting rolling temperature is controlled at 1108℃. The rolled piece is rolled by 6 rough rolling mills and 6 intermediate rolling mills, and then rolled by 5 finishing mills. The rolling operation is completed. The temperature of the rolled piece before entering the finishing mill is controlled at 997℃, and the temperature of the cooling bed for final rolling is controlled at 979℃. The rolling specification is Φ20mm.
[0073] 5) Temperature control after final rolling: Control the roller speed after rolling to keep the rolled piece at 934℃ for 6.6s in the skirt area; after quickly passing through the cooling bed (close all ventilation windows under the cooling bed and doors and windows used in the factory in winter; close the ventilation windows under the cooling bed in spring and autumn), the rolled piece is piled on the alignment roller at 663℃ and kept warm for 68s, and then cut to length, packaged and stored after cooling.
[0074] 6) Sampling was performed according to the standard, and the test results were as follows:
[0075]
[0076] The earthquake-resistant threaded steel HRB500E produced in Examples 1-3 and the comparative example was rolled into Φ8-Φ40mm coil screws and straight screws, and the performance was tested. The results are shown in Table 1.
[0077]
[0078] Table 1
[0079] From Table 1 and Figure 1-9It can be seen from the data that the seismic-resistant threaded steel HRB500E prepared in Examples 1-3 of the present invention have qualified mechanical properties of the steel bars without changing the composition. The thinning of the pearlite plate spacing causes the elongation after fracture A and the total elongation at maximum force Agt to be increased by more than 20% compared with the control example, thereby enhancing the ductility of the steel bars and increasing the redundancy of the seismic-resistant parameters of the steel bars. At the same time, the present invention can reduce the production cost by 0.2-0.5% (reducing the cost by 10-25 yuan / ton of steel) by utilizing the price difference of Nb alloy and V alloy in the market while ensuring the mechanical properties and performance of the seismic-resistant steel bar HRB500E, thereby effectively reducing the production cost.
[0080] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A production method for reducing the pearlite lamellar spacing of HRB500E niobium reinforced steel bars, Features: The steps include: Step 1: Cut the steel billet into small square billets for continuous casting, with a cross-sectional size of 150mm×150mm-165mm×165mm; Step 2: sending the small square billet cut in step 1 into a heating furnace for heating; Step 3: After heating in step 2, the steel is rolled by a rough rolling unit, a medium rolling unit, and a finishing rolling unit; Step 4: After the rolling in step 3 is completed, the temperature in the skirt area is controlled within the range of 890-970℃ for 5-10s, and then kept within the range of 610-750℃ for 40-100s in the cooling bed alignment roller area, and then cooled to room temperature to obtain the finished product.
2. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: The composition of the steel billet in step 1 includes the following elements in weight percentage: C: 0.18-0.26wt%; Si: 0.30-0.80wt%; Mn: 1.30-1.60wt%; P: ≤0.045wt%; S: ≤0.045wt%; Nb: 0.008-0.025wt%; V :0.04-0.08wt%; Al: 0.003-0.008wt%; N: 0.015-0.025wt%; Ceq: ≤0.55wt%; The rest is Fe and inevitable impurity elements.
3. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 2, Features: The composition of the steel billet includes the following elements in weight percentage: C: 0.21-0.25wt%; Si: 0.30-0.80wt%; Mn: 1.30-1.60wt%; P: ≤0.045wt%; S: ≤0.045wt%; Nb: 0.008-0.016wt%; V :0.04-0.07wt%; Al: 0.003-0.008wt%; N: 0.015-0.022wt%; Ceq: ≤0.55wt%; The rest is Fe and inevitable impurity elements.
4. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: The small square billet in the step 2 is heated to 1050-1280° C. by a heating furnace.
5. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: The rolling temperature in step 3 is controlled at 990-1150°C.
6. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: The rough rolling mill in step 3 has 6 rolling passes.
7. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: The intermediate rolling mill in step 3 has 6 rolling passes.
8. A method for reducing the pearlite lamellar spacing of HRB500E niobium reinforced steel bars according to claim 1, Features: The rolling passes of the finishing mill in step 3 are 4-6 stands, the temperature before entering the finishing mill is controlled at 930-1080°C, and the temperature of the cooling bed for final rolling is controlled at 920-1050°C.
9. A method for reducing the pearlite lamellar spacing of HRB500E niobium reinforced steel bars according to claim 1, Features: The final rolling diameter of step 3 is 10-50 mm.
10. A production method for reducing the pearlite lamellar spacing of HRB500E niobium-added steel bars according to claim 1, Features: After the rolling in step 4 is completed, the temperature in the skirt plate area is controlled within the range of 900-960° C. and kept warm for 5-8 seconds; then, the temperature is accumulated in the alignment roller area within the range of 620-700° C. and kept warm for 50-80 seconds.