Method for recovering iron and removing arsenic from tin tailings
Through strong magnetic pretreatment and ultrasonic/oxidation collaborative treatment technology, combined with sodium leaching, the problems of low iron recovery and poor arsenic removal in tin tailings are solved, and efficient iron recovery and efficient arsenic removal in tin tailings are achieved. In addition, the efficiency of resource utilization has been improved.
Patent Information
- Application Number
- CN202410925843.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art has low iron recovery rate and poor arsenic removal effect in tin tailings, making it difficult to achieve efficient utilization.
The method of strong magnetic pretreatment-reducing roasting-grinding-weak magnetic separation-ultrasonic/oxidation collaborative treatment-sodium leaching is adopted to reduce ore treatment volume and cost through pretreatment, improve iron grade, and further use ultrasonic/oxidation collaborative treatment Reduce arsenic content.
The high-value utilization of iron in tin tailings has been achieved, the iron grade and arsenic removal rate have been improved, and it has the advantages of strong operability and low cost.
Smart Images

Figure CN118880025A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for recovering iron and removing arsenic from tin tailings, belonging to the technical field of solid waste resource utilization. Background Art
[0002] With the continuous development of tin ore resources by humans, a large amount of solid waste - tin tailings - has been generated. The accumulation of tin tailings not only occupies a large area and causes serious environmental pollution, but also the tailings often contain a large amount of iron minerals, which have the value of secondary utilization. At present, the methods for recovering iron minerals in tailings are mainly divided into single beneficiation and beneficiation and smelting combined technology. Single beneficiation technology mainly includes gravity separation, magnetic separation and flotation. The use of a single beneficiation technology to recover iron minerals in tailings has problems such as low iron recovery rate and substandard grade, making it difficult to achieve efficient utilization of iron in tailings. The beneficiation and smelting combined process is mainly a method of gravity / magnetic / flotation and pyrometallurgical combined treatment, which can efficiently recover iron minerals in tailings. At present, the reduction roasting-magnetic separation technology has achieved remarkable results in the resource utilization of difficult-to-select iron-containing tailings, but the removal effect of arsenic in iron concentrate is not ideal. Arsenic in iron concentrate is generally removed by roasting and leaching. Roasting can be divided into oxidative roasting and reduction roasting, both of which aim to volatilize arsenic. However, the roasting volatilization method has strict requirements on the strength of the atmosphere, and the temperature required for the effective volatilization of arsenic is relatively high. Oxidative roasting needs to reach above 1200°C under some conditions, while reduction roasting volatilization of arsenic generally requires the temperature to be maintained above 900°C. The wet leaching process separates arsenic by acid leaching, alkali leaching or salt leaching, but acid leaching will also cause iron loss while leaching arsenic, and the effect of direct alkali leaching or salt leaching is not ideal. Therefore, for tin tailings resources containing arsenic and iron, it is urgent to develop an efficient method for iron recovery and arsenic removal.
[0003] Patent application number is 2018114278665, a method for roasting iron tailings. Roasting: roasting the iron tailings in an inert gas atmosphere, programmed heating and programmed cooling; recovery: recovering the volatile flue gas to obtain metal chloride, taking out the roasting slag after the roasting temperature in S1 drops to 50-150°C, and magnetically separating the roasting slag to obtain magnetite. Through the specific inert gas roasting atmosphere, the amount of chlorinating agent added and the roasting temperature rise and fall program control, the magnetization separation of iron tailings is realized, and a good iron ore magnetization and valuable metal separation effect is achieved. The removal rates of lead, copper, zinc and cadmium reach 98.89%, 66.71%, 60.51% and 96.6% respectively, and the magnetic separation recovery rate reaches 98.29%. No reducing agent needs to be added. The magnetization of iron in the tailings is achieved by controlling the roasting atmosphere, which fundamentally reduces the problem of large pollution in the iron tailings treatment process and the impact on metal recovery in flue gas. It is easy to operate and has low cost, and has obvious benefits for the reduction and resource utilization of iron tailings. However, the invention does not further process the arsenic in the iron tailings. How to effectively remove the arsenic in the iron tailings and efficiently recover iron is a technical problem. Summary of the invention
[0004] In view of the problems and shortcomings of the above-mentioned prior art, the present invention provides a method for recovering iron and removing arsenic from tin tailings. The present invention realizes the high-value utilization of iron in tin tailings through the method of strong magnetic pretreatment-reduction roasting-grinding-weak magnetic separation-ultrasonic / oxidation co-treatment-sodium leaching. The present invention reduces the ore processing amount, processing cost, and arsenic content in the reduction roasting-leaching process through pretreatment, and improves the iron grade. The arsenic content in the iron concentrate is further reduced through ultrasonic / oxidation co-treatment-sodium leaching technology, and has the advantages of strong operability and high arsenic removal rate. The present invention is implemented through the following technical solutions.
[0005] A method for recovering iron and removing arsenic from tin tailings, the specific steps of which are as follows:
[0006] S1. Use strong magnetic separation technology to treat iron-tin tailings, pre-enrich and discard a large amount of gangue minerals, filter and dry to obtain strong magnetic separation concentrate;
[0007] S2, mixing the strong magnetic separation concentrate obtained in S1 and the reducing agent uniformly for reduction roasting, and obtaining the roasting material after cooling in the furnace;
[0008] S3, subjecting the roasted material obtained in S2 to ore grinding and multi-stage weak magnetic separation to obtain arsenic-containing iron concentrate;
[0009] S4, subjecting the arsenic-containing iron concentrate obtained in S3 to ultrasonic treatment, adding it to a H2O2 solution for oxidation treatment after the treatment, and obtaining an oxidation product after solid-liquid separation;
[0010] S5. Add the oxidation product obtained in S4 into a NaOH solution with a concentration of 5-15wt% for stirring and leaching. After the leaching is completed, perform solid-liquid separation to obtain a high-quality iron ore concentrate.
[0011] The iron content of the iron-containing tin tailings in S1 is 10-30wt%, and the arsenic content is 0.2-0.7wt%; the iron phases in the iron-containing tin tailings are mainly hematite, limonite and goethite, and the arsenic phase is arsenopyrite.
[0012] The intensity of the strong magnetic separation in S1 is 0.8-1.4T.
[0013] The reducing agent in S2 is lignite, bituminous coal or anthracite, and the mass ratio of the strong magnetic separation concentrate to the reducing agent is 1:0.1 to 1:0.2.
[0014] The reduction roasting temperature in S2 is 650-850° C., and the roasting holding time is 0.5-1 h.
[0015] In the S3, the ore is ground to a particle size of -0.074 mm, which accounts for more than 75wt%, and the weak magnetic separation intensity is 0.15-0.30T.
[0016] The ultrasonic treatment in S4 has an ultrasonic frequency of 10 to 60 KHz and an ultrasonic time of 5 to 30 minutes.
[0017] The concentration of the H2O2 solution in the S4 is 5wt% to 15wt%, the solid-liquid ratio of the arsenic-containing iron concentrate to the H2O2 solution is 1:20 to 1:100 g / mL, and oxidation is performed at room temperature for 30 to 90 minutes.
[0018] The solid-liquid ratio of the oxidation product to the NaOH solution in the S5 is 1:20-1:50 g / mL, the leaching temperature is 70-90° C., and the leaching time is 1.5-3 hours.
[0019] The working principle of the present invention is:
[0020] The weakly magnetic minerals hematite and limonite are pre-enriched by strong magnetic separation, which improves the iron grade in the roasting feed and removes most of the gangue minerals and arsenic-containing minerals, reducing the energy consumption and cost of subsequent roasting and leaching. In the reduction roasting heating stage, hematite and limonite are reduced to Fe3O4, and in the reduction roasting insulation stage, arsenopyrite reacts with Fe3O4 to generate FeAs (as shown in Formula 1). The newly generated arsenic-containing substances will adhere to the surface of Fe3O4 through magnetism. Grinding is used to dissociate Fe3O4 and gangue minerals, and Fe3O4 loaded with FeAs is enriched by weak magnetic separation to obtain high-arsenic iron concentrate. Ultrasonic treatment is used for high-arsenic iron concentrate to disperse Fe3O4 and FeAs attached to its surface, and then FeAs is oxidized to ferric arsenate by H2O2 treatment (as shown in Formula 2). Then, by sodium leaching, ferric arsenate is converted into sodium arsenate with higher solubility (as shown in Formula 3), thereby achieving the removal of arsenic in the iron concentrate.
[0021] 10FeAsS+10C+3Fe3O4=10FeAs+9FeS+SO2(g)+10CO(g) (1)
[0022] FeAs+4H2O2(l)=FeAsO4+4H2O (2)
[0023] FeAsO4+3NaOH=Fe(OH)3+Na3AsO4 (3)
[0024] The beneficial effects of the present invention are:
[0025] 1. For tin tailings containing arsenic and iron, the present invention proposes a new technology for the combined selection and smelting of strong magnetic pretreatment - reduction roasting - grinding - weak magnetic separation - ultrasonic / oxidation coordinated treatment - sodium leaching, which realizes the high-value utilization of iron resources in tin tailings.
[0026] 2. The present invention reduces the ore processing volume, processing cost, and arsenic content in the reduction roasting-leaching process through pretreatment, and improves the iron grade. The arsenic content in the iron concentrate is further reduced through ultrasonic / oxidation coordinated treatment-sodium leaching technology, and has the advantages of strong operability and high arsenic removal rate.
[0027] 3. The present invention converts hematite into magnetite through low-temperature reduction roasting, and at the same time converts arsenopyrite in the tailings into FeAs, and combines oxidation-sodium salt leaching to convert iron arsenide into iron arsenate, and then into soluble sodium arsenate, thereby efficiently removing arsenic from the iron concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.
[0030] Example 1
[0031] like Figure 1 As shown, the method for recovering iron and removing arsenic from tin tailings has the following specific steps:
[0032] S1. Using strong magnetic separation technology to treat iron-containing tin tailings (the iron content of the iron-containing tin tailings is 22.83wt%, the arsenic content is 0.36wt%; the gangue minerals are mainly dolomite, calcite, quartz, etc.), under the condition of a magnetic field intensity of 1.4T, a large amount of gangue minerals are discarded by strong magnetic pre-enrichment, filtered, and dried to obtain a strong magnetic separation concentrate; after this treatment step, the iron and arsenic grades in the strong magnetic separation concentrate reach 37.23wt% and 0.497wt%, the iron recovery rate reaches 84.76%, and the arsenic removal rate reaches 28.24%;
[0033] S2, the strong magnetic separation concentrate obtained in S1 and the reducing agent (lignite) are mixed uniformly in a mass ratio of 1:0.12 and then reduction roasted at a temperature of 800° C. for 40 min, and then cooled in a furnace to obtain a roasted material;
[0034] S3, grinding and two-stage weak magnetic separation are performed on the roasted material obtained in S2, each grinding is performed until the particle size is -0.074mm and the particle size accounts for 85wt%, and the weak magnetic separation intensity is 0.30T, to obtain arsenic-containing iron concentrate;
[0035] S4, subjecting the arsenic-containing iron concentrate obtained in S3 to ultrasonic treatment, wherein the ultrasonic frequency is 60 KHz, the ultrasonic time is 30 min, and after the treatment is completed, it is added to a 10 wt% H2O2 solution at a solid-liquid ratio of 1:25 g / mL, and an oxidation treatment is performed at room temperature for 40 min, and an oxidation product is obtained after solid-liquid separation;
[0036] S5. The oxidation product obtained in S4 is added into a 10wt% NaOH solution at a solid-liquid ratio of 1:25g / mL, and stirred and leached for 2h at 80°C. After leaching, solid-liquid separation is performed to obtain high-quality iron ore concentrate.
[0037] The high-quality iron concentrate obtained in this embodiment contains 0.175wt% arsenic and 61.59wt% iron. The comprehensive recovery rate of iron reaches 56.08%, and the cumulative removal rate of arsenic reaches 89.90%.
[0038] Comparative Example 1 (without ultrasound, oxidation treatment and sodium leaching)
[0039] The ore sample in Example 1 was treated by strong magnetic separation pretreatment-reduction roasting-grinding-magnetic separation technology, and the parameters were consistent with the treatment steps and Example 1, except that there was no ultrasound, oxidation treatment and sodium leaching in this comparative example. The pre-enriched iron concentrate was mixed with the reducing agent lignite to obtain a mixed ore sample, and the roasted product was obtained by roasting for 40 minutes at a roasting temperature of 800°C. The roasted product was ground and then subjected to weak magnetic separation with a magnetic separation intensity of 0.30T. An iron concentrate with a grade and recovery rate of 61.56% and 56.27% was obtained, respectively, wherein the grade of arsenic was reduced to 0.348%, and the cumulative removal rate of arsenic reached 79.83%. It can be seen that the arsenic removal effect of tin tailings only subjected to magnetic separation pretreatment-reduction roasting-grinding-magnetic separation is not ideal.
[0040] Example 2
[0041] like Figure 1 As shown, the method for recovering iron and removing arsenic from tin tailings has the following specific steps:
[0042] S1. Using strong magnetic separation technology to treat iron-containing tin tailings (the iron content of the iron-containing tin tailings is 12.76wt%, the arsenic content is 0.47wt%; the gangue minerals are mainly calcite and quartz), and a large amount of gangue minerals are removed by strong magnetic pre-enrichment under the condition of a magnetic field intensity of 1.0T, and then filtered and dried to obtain a strong magnetic separation concentrate; after this treatment step, the iron and arsenic grades in the strong magnetic separation concentrate reach 30.36wt% and 0.668wt%, the iron recovery rate reaches 69.95%, and the arsenic removal rate reaches 58.22%;
[0043] S2, the strong magnetic separation concentrate obtained in S1 and the reducing agent (lignite) are mixed uniformly in a mass ratio of 1:0.12 and then reduction roasted. The reduction roasting temperature is 650° C. and roasted for 60 min. After cooling in the furnace, a roasting material is obtained;
[0044] S3, grinding and two-stage weak magnetic separation are performed on the roasted material obtained in S2, each grinding is performed until the particle size is -0.074mm and the particle size accounts for 80wt%, and the weak magnetic separation intensity is 0.30T, to obtain arsenic-containing iron concentrate;
[0045] S4, subjecting the arsenic-containing iron concentrate obtained in S3 to ultrasonic treatment, wherein the ultrasonic frequency is 40 KHz, the ultrasonic time is 30 min, and after the treatment is completed, it is added to a 13 wt% H2O2 solution at a solid-liquid ratio of 1:35 g / mL, and an oxidation treatment is performed at room temperature for 60 min, and an oxidation product is obtained after solid-liquid separation;
[0046] S5. The oxidation product obtained in S4 is added into a 10wt% NaOH solution at a solid-liquid ratio of 1:35g / mL, and stirred and leached for 2h at 90°C. After leaching, solid-liquid separation is performed to obtain high-quality iron ore concentrate.
[0047] The high-quality iron concentrate obtained in this embodiment contains 0.164wt% arsenic and 60.94% iron. The comprehensive recovery rate of iron reaches 44.36%, and the cumulative removal rate of arsenic reaches 96.76%.
[0048] Comparative Example 2 (Arsenic removal by reduction roasting and volatilization)
[0049] The ore sample in Example 2 was treated by the reduction roasting volatilization method. The ore sample parameters were the same as those in Example 1, except that there was no grinding-weak magnetic separation-ultrasonic / oxidation coordinated treatment-sodium leaching step in this comparative example, and the reduction roasting temperature was increased to 950°C, and the roasting was performed for 60 minutes to obtain a roasted product. The iron grade in the roasted product was 35.10%, the arsenic grade was reduced to 0.477%, the arsenic volatilization rate was 15.98%, and the cumulative arsenic removal rate was 74.20%. It can be seen that under this condition, the reduction roasting method has a poor arsenic removal effect.
[0050] Example 3
[0051] like Figure 1 As shown, the method for recovering iron and removing arsenic from tin tailings has the following specific steps:
[0052] S1. Using strong magnetic separation technology to treat iron-containing tin tailings (the iron content of the iron-containing tin tailings is 18.56wt%, the arsenic content is 0.43wt%; the gangue minerals are mainly calcite and quartz), under the condition of a magnetic field intensity of 0.8T, a large amount of gangue minerals are discarded by strong magnetic pre-enrichment, filtered, and dried to obtain a strong magnetic separation concentrate; after this treatment step, the iron and arsenic grades in the strong magnetic separation concentrate reach 34.05% and 0.611%, the iron recovery rate reaches 83.05%, and the arsenic removal rate reaches 35.68%;
[0053] S2, the strong magnetic separation concentrate obtained in S1 and the reducing agent (lignite) are mixed uniformly in a mass ratio of 1:0.20 and reduced and roasted at a temperature of 850° C. for 40 min, and then cooled in a furnace to obtain a roasted material;
[0054] S3, grinding and two-stage weak magnetic separation are performed on the roasted material obtained in S2, each grinding is performed until the particle size is -0.074mm and the particle size accounts for 75wt%, and the weak magnetic separation intensity is 0.30T, to obtain arsenic-containing iron concentrate;
[0055] S4, subjecting the arsenic-containing iron concentrate obtained in S3 to ultrasonic treatment, wherein the ultrasonic frequency is 60 KHz, the ultrasonic time is 30 min, and after the treatment is completed, it is added to a 15 wt% H2O2 solution at a solid-liquid ratio of 1:50 g / mL, and an oxidation treatment is performed at room temperature for 90 min, and an oxidation product is obtained after solid-liquid separation;
[0056] S5. The oxidation product obtained in S4 is added into a 10 wt% NaOH solution at a solid-liquid ratio of 1:40 g / mL, and stirred and leached for 2 h at 90°C. After leaching, solid-liquid separation is performed to obtain a high-quality iron ore concentrate.
[0057] The high-quality iron concentrate obtained in this embodiment contains 0.136wt% arsenic and 60.96wt% iron. The comprehensive recovery rate of iron reaches 54.05%, and the cumulative removal rate of arsenic reaches 94.80%.
[0058] Comparative Example 3 (No Sodium Leaching)
[0059] The tin tailings are the same as in Example 3, with the conditions from strong magnetic pretreatment to ultrasonic / oxidation synergistic treatment being the same, except that there is no S5 sodium leaching process. After weak magnetic separation, an arsenic-containing iron concentrate with an iron grade of 61.02% and an arsenic grade of 0.371% is obtained, and the iron recovery rate and arsenic removal rate are 54.26% and 85.76%, respectively. After ultrasonic / oxidation synergistic treatment, the arsenic grade is reduced to 0.352%, and the cumulative removal rate of arsenic is 86.51%. It can be seen that sodium leaching is the main subsequent arsenic removal process.
[0060] Comparative Example 4 (without ultrasound / oxidation synergistic treatment)
[0061] The tin tailings are the same as in Example 3, from strong magnetic pretreatment to weak magnetic separation and sodium leaching treatment in S5 and the corresponding parameters are the same, except that there is no ultrasonic / oxidation co-treatment step. The arsenic-containing iron concentrate obtained in S3 in Example 3 is added to a NaOH solution with a concentration of 10wt% according to a solid-liquid ratio of 1:40g / mL, stirred and leached for 2h at a temperature of 90°C, and solid-liquid separation is performed after leaching to obtain the iron concentrate. The arsenic content in the iron concentrate is 0.348%, and the cumulative removal rate of arsenic is 86.66%. It can be seen from this that it is impossible to obtain an efficient arsenic removal effect without ultrasonically dispersing Fe3O4 and FeAs attached to its surface and then oxidizing it.
[0062] The following table compares the indicators of each example.
[0063] Table 1 Comparison of indicators of various instances
[0064]
[0065] Note: Unless otherwise specified in the present invention, the percentages are all by mass.
[0066] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A method for recovering iron and removing arsenic from tin tailings, Features The specific steps are as follows: S1. Use strong magnetic separation technology to treat iron-tin tailings, and obtain strong magnetic separation concentrate after pre-enrichment, filtration and drying; S2, mixing the strong magnetic separation concentrate obtained in S1 and the reducing agent uniformly for reduction roasting, and obtaining the roasting material after cooling in the furnace; S3, subjecting the roasted material obtained in S2 to ore grinding and multi-stage weak magnetic separation to obtain arsenic-containing iron concentrate; S4, subjecting the arsenic-containing iron concentrate obtained in S3 to ultrasonic treatment, adding H 2 O 2 Perform oxidation treatment in the solution, and obtain oxidation products after solid-liquid separation; S5. Add the oxidation product obtained in S4 into a NaOH solution with a concentration of 5-15wt% for stirring and leaching. After the leaching is completed, perform solid-liquid separation to obtain a high-quality iron ore concentrate.
2. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The iron content of the iron-containing tin tailings in S1 is 10-30wt%, and the arsenic content is 0.2-0.7wt%; the iron phases in the iron-containing tin tailings are mainly hematite, limonite and goethite, and the arsenic phase is mainly arsenopyrite.
3. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The intensity of the strong magnetic separation in S1 is 0.8-1.4T.
4. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The reducing agent in S2 is lignite, bituminous coal or anthracite, and the mass ratio of the strong magnetic separation concentrate to the reducing agent is 1:0.1 to 1:0.
2.
5. The method for recovering iron and removing arsenic from tin tailings according to claim 4, Features: The reduction roasting temperature in S2 is 650-850° C., and the roasting holding time is 0.5-1 h.
6. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: In the S3, the ore is ground to a particle size of -0.074 mm, which accounts for more than 75wt%, and the weak magnetic separation intensity is 0.15-0.30T.
7. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The ultrasonic treatment in S4 has an ultrasonic frequency of 10 to 60 KHz and an ultrasonic time of 5 to 30 minutes.
8. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The S4H 2 O 2 The solution concentration is 5wt% to 15wt%, and the arsenic iron concentrate and H 2 O 2 The solution has a solid-to-liquid ratio of 1:20 to 1:100 g / mL, and is oxidized at room temperature for 30 to 90 minutes.
9. The method for recovering iron and removing arsenic from tin tailings according to claim 1, Features: The solid-liquid ratio of the oxidation product to the NaOH solution in the S5 is 1:20-1:50 g / mL, the leaching temperature is 70-90° C., and the leaching time is 1.5-3 hours.
Citation Information
Cited By
Method for recovering tin in high-mud-content multi-metal tailings
CN119506582A
A method for recovering tin from high-mud polymetallic tailings
CN119506582B