Catalytic pyrolysis method of small-particle oil shale
By uniformly covering the catalyst with small-particle oil shale powder and fluidized roasting, the problem of low utilization of oil shale is solved, the oil and gas conversion rate and oil quality of oil shale are improved, and more efficient resource utilization is achieved.
Patent Information
- Application Number
- CN202410971552.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing technology cannot effectively utilize small-particle oil shale, resulting in low overall utilization of oil shale and its direct waste will lead to waste of resources and environmental pollution.
By grinding small-particle oil shale into powder, uniformly covering the catalyst, then drying and fluidized calcining is carried out at low temperature, and the catalyst is used to accelerate the conversion of the otrocardium into oil and gas, reducing the cracking temperature, and improving the oil and gas conversion rate of oil shale.
The pyrolysis efficiency of organic matter of small-particle oil shale is improved, the aliphatic hydrocarbon content of oil shale oil products is increased, the heavy distillate product is reduced, the coking amount is reduced, and the overall utilization rate of oil shale is improved.
Smart Images

Figure CN118956441A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic pyrolysis of oil shale, in particular to a catalytic pyrolysis method of small-particle oil shale. Background Art
[0002] Oil shale is an important unconventional energy resource in my country. The production of shale oil through oil shale is an important supplement to petroleum energy today. After crushing, screening and sorting, about 30% of small particles of oil shale with a particle size of less than 12mm will be produced, which cannot be directly used to refine shale oil. The reason is that after small particles of oil shale enter the retort furnace, the permeability in the furnace will be poor and the resistance will increase, which will affect the retort effect and result in the overall utilization rate of oil shale being only 70%. Usually, small particles of oil shale are directly discarded, which not only occupies a large amount of land but also causes environmental pollution and waste of resources.
[0003] Suspension roasting technology is a technology that transforms the crystal form of ores through high-temperature roasting. It is mainly used for the development and utilization of complex and difficult-to-select metal ore resources such as poor hematite, siderite, and limonite. It has the advantages of high roasting efficiency and effective removal of impurities, and has good industrial application prospects. However, the current application scope of suspension roasting technology is relatively small, and it is generally only used for the separation of difficult-to-select metal minerals, and has not yet been developed in the field of shale oil.
[0004] In summary, there is an urgent need for a method that can effectively utilize small-particle oil shale and improve the overall utilization rate of oil shale. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for catalytic pyrolysis of small-particle oil shale, so as to at least achieve the effective utilization of discarded small-particle oil shale.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] The catalytic pyrolysis method of small-particle oil shale is characterized by comprising the following steps:
[0008] S1: grinding small particles of oil shale to obtain oil shale powder, and then evenly covering the surface of the oil shale powder with a catalyst to obtain catalyst-containing oil shale;
[0009] S2: The catalyst-containing oil shale is dried at low temperature, and then fluidized roasted, and the obtained gaseous pyrolysis products are dedusted and cooled in sequence to obtain an oil shale oil product.
[0010] Furthermore, in step S1, the particle size of the small particles of oil shale is less than 200 meshes.
[0011] It is worth noting that, in the present invention, the smaller the particle size is, the larger the specific surface area is, the more complete the gas-solid contact is, the less time is required for the reaction, and the lower the energy consumption is.
[0012] Furthermore, in step S1, the catalyst is a mesoporous molecular sieve catalyst;
[0013] The catalyst is a permeable surfactant comprising rare earth elements or transition metal elements and a long-chain alkyl derivative.
[0014] Further, the rare earth element includes at least one of lanthanum, cerium, praseodymium or yttrium;
[0015] The transition metal element includes at least one of nickel, cobalt, iron and molybdenum.
[0016] Further, the long-chain alkyl derivative includes at least one of dodecyl ethoxy sulfobetaine, dodecyl hydroxypropyl sulfobetaine, dodecyl dimethyl sulfopropyl betaine, dodecyl sulfopropyl betaine, tetradecyl sulfopropyl betaine, hexadecyl sulfopropyl betaine, octadecyl sulfopropyl betaine, dodecyl dimethyl betaine, tetradecyl dimethyl betaine, octadecyl dimethyl betaine, dodecyl dihydroxyethyl betaine, octadecyl dihydroxyethyl betaine, lauroyl amidopropyl betaine, cocamidopropyl betaine, octadecyl amidopropyl betaine, dodecyl hydroxypropyl phosphate betaine, and tetradecyl hydroxypropyl phosphate betaine.
[0017] The preparation method of the catalyst refers to Chinese patent CN202210181054.7, specifically: mixing the hydrogen-type Y molecular sieve and the pore expanding agent solution, mixing the mixture with the pore-opening agent after sufficient reaction, then filtering, adjusting the pH to 7, adding the pore-opening agent, filtering after reacting at 80°C, and then calcining at 450°C; adding the ion solution of the rare earth element or the transition metal element to the obtained material, filtering after reacting at 80°C, adjusting the pH to 7, and then calcining at 450°C, and then adding the long-chain alkyl derivative, mixing evenly, to obtain.
[0018] Furthermore, the catalyst needs to be prepared into a 0.1-1 wt% aqueous solution.
[0019] Furthermore, in step S1, the mass ratio of the catalyst to the oil shale powder is 1:500-1000.
[0020] Furthermore, in step S2, the temperature of the low-temperature drying is below 60°C.
[0021] Furthermore, the low-temperature drying includes natural air drying or low-temperature drying.
[0022] Furthermore, in step S2, the fluidized roasting is suspended roasting.
[0023] Furthermore, in step S2, the calcination temperature is 350-600°C.
[0024] It is worth noting that the pyrolysis reaction temperature in the present invention is relatively low, and the conversion of solid organic matter in oil shale begins at 350°C, which indicates that the addition of catalyst can accelerate the process of kerogen conversion to oil and gas, reduce the cracking conversion temperature of oil shale, improve the quality components of oil shale oil, and increase the oil and gas conversion rate of oil shale. Compared with the catalytic effect of solid organic matter in oil shale without adding catalyst, the content of aliphatic hydrocarbons (alkanes + olefins) in oil shale oil products is significantly increased, the content of heavy fraction products is significantly reduced, the oil yield is significantly increased, and the amount of coking is reduced.
[0025] The beneficial effects of the present invention are:
[0026] The present invention combines catalytic pyrolysis and suspension roasting technology to form a new technology for suspended fluidized catalytic heating cracking test of small-particle oil shale. During the gaseous pyrolysis process, the oil shale powder is suspended in the gas phase and is in a better dispersed state, which can enable full gas-solid contact. The mass and heat transfer rates are fast during the reaction, and the temperature and air flow field are evenly distributed, so that the pyrolysis efficiency of organic matter in small-particle oil shale is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.
[0029] Example 1
[0030] Weigh 1000g of Xinjiang small-particle oil shale, crush it to 100 mesh, and determine the oil content to be 10.13%. According to the weight ratio of oil shale and catalyst (prepared by the above preparation method using cerium and dodecyl hydroxypropyl sulfobetaine) (oil shale: catalyst is 1:800), spray the catalyst solution evenly on the surface of small-particle oil shale, fully immerse for more than 12 hours, and dry it by natural ventilation. Then, the suspended roasting pyrolysis method is adopted, and the dried catalyst-containing oil shale powder is added to the suspended roasting test furnace, and after fluidization preheating, it enters the fluidized heating tank, and an oxygen-free catalytic thermal cracking reaction (nitrogen atmosphere) is carried out at 450°C. The gas product after the reaction enters the cooling system after the dust removal device to obtain the oil shale oil product.
[0031] After testing (the oil content test mainly refers to GB / T 480-2000, and the four-component analysis of shale oil mainly refers to NBSHT0509-2010), the total content of alkanes and olefins in the oil shale oil product increased from 12% to 42.6%, the heavy fraction product decreased from 49% to 17.5%, and the collected oil shale oil increased from 56.9g before adding catalyst to 70.2g.
[0032] Example 2
[0033] Weigh 800g of Xinjiang small-particle oil shale, crush it to 80 mesh, the oil content is 5.15%, according to the weight ratio of oil shale and catalyst (made by lanthanum and dodecyl hydroxypropyl sulfobetaine according to the above preparation method) (oil shale: catalyst is 1:1000), spray the catalyst solution evenly on the surface of small-particle oil shale, fully immerse for more than 12 hours, and heat and dry at 55°C. Then, the suspended roasting pyrolysis test method is adopted, the dried catalyst-containing oil shale powder is added to the suspended roasting test furnace, and after fluidization preheating, it enters the fluidized heating tank, and an oxygen-free catalytic thermal cracking reaction (nitrogen atmosphere) is carried out at 400°C. The gas product after the reaction enters the cooling system after the dust removal device to obtain the oil shale oil product.
[0034] After testing, the maximum content of alkanes + olefins increased from 11% to 26%, the heavy fraction product decreased from 46% to 35%, and the collected oil shale oil product increased from 24.7g before adding the catalyst to 32.5g.
[0035] Comparative Example 1
[0036] 800g of Xinjiang small-particle oil shale (blocky small particles) were weighed and crushed to a particle size of less than 6mm without fine grinding, and the oil content was 5.15%. According to the weight ratio of oil shale and catalyst (prepared by the above preparation method using lanthanum and dodecyl hydroxypropyl sulfobetaine) (oil shale: catalyst is 1:1000), the catalyst solution was evenly sprayed on the surface of the small-particle oil shale, fully immersed for more than 12 hours, and heated to dry at 55°C. Then, the suspended roasting pyrolysis method was adopted, and the dried catalyst-containing oil shale was added to the suspended roasting furnace, and after fluidization preheating, it entered the fluidized heating tank, and an oxygen-free catalytic thermal cracking reaction (nitrogen atmosphere) was carried out at 400°C. The gas product after the reaction entered the cooling system after the dust removal device to obtain the oil shale oil product.
[0037] After testing, the maximum content of alkanes + olefins increased from 11% to 16%, the heavy fraction product decreased from 46% to 42%, and the collected oil shale oil product increased from 24.7g before adding the catalyst to 27.5g.
[0038] Comparative Example 2
[0039] Weigh 1000g of Xinjiang small-particle oil shale, crush it to about 100 mesh, and determine the oil content to be 10.13%. According to the weight ratio of oil shale and catalyst (prepared by the above-mentioned preparation method using cerium and dodecyl hydroxypropyl sulfobetaine) (oil shale: catalyst is 1:800), spray the catalyst solution evenly on the surface of small-particle oil shale, fully immerse for more than 12 hours, dry it with natural ventilation, and use the ground retort test method to add the dried catalyst-containing oil shale powder into the retort test furnace. Under the condition of 450℃, the total content of alkanes and olefins increased from 12% to 37%, and the heavy fraction product decreased from 49% to 37%. The collected oil shale oil increased from 51.7g before adding the catalyst to 62.5g.
[0040] Comparative Example 3
[0041] Weigh 1000g of Xinjiang small-particle oil shale, crush it to 100 mesh, and determine the oil content to be 10.13%. The oil shale is naturally ventilated and dried. Then, a suspension roasting pyrolysis method is used, and the dried catalyst-containing oil shale is added to a suspension roasting furnace, and after fluidization preheating, it enters a fluidized heating tank, and an oxygen-free catalytic thermal cracking reaction (nitrogen atmosphere) is carried out at 380°C. The gas product after the reaction enters a cooling system after a dust removal device to obtain an oil shale oil product.
[0042] After testing, the total content of alkanes and olefins in the oil shale oil products increased from 12% to 12.4%, the heavy fraction products decreased from 49% to 48.6%, and the collected oil shale oil increased from 56.5g to 65.1g. It can be seen that when no catalyst is added, it has little effect on improving the quality of shale oil, but the amount of shale oil produced by suspension roasting pyrolysis is significantly higher than that of ground distillation.
[0043] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.
Claims
1. A method for catalytic pyrolysis of small-particle oil shale, characterized in that: The following steps are involved: S1: grinding small particles of oil shale to obtain oil shale powder, and then evenly covering the surface of the oil shale powder with a catalyst to obtain catalyst-containing oil shale; S2: The catalyst-containing oil shale is dried at low temperature, and then fluidized roasted, and the obtained gaseous pyrolysis products are dedusted and cooled in sequence to obtain an oil shale oil product.
2. The catalytic pyrolysis method of oil shale according to claim 1, characterized in that: In step S1, the particle size of the small particles of oil shale is less than 200 meshes.
3. The catalytic pyrolysis method of oil shale according to claim 1, characterized in that: In step S1, the catalyst is a permeable surfactant comprising a rare earth element or a transition metal element and a long-chain alkyl derivative.
4. The catalytic pyrolysis method of oil shale according to claim 3, characterized in that: The rare earth element includes at least one of lanthanum, cerium, praseodymium or yttrium; The transition metal element includes at least one of nickel, cobalt, iron and molybdenum.
5. The method for catalytic pyrolysis of oil shale according to claim 3, characterized in that: The long-chain alkyl derivative includes at least one of dodecyl ethoxy sulfobetaine, dodecyl hydroxypropyl sulfobetaine, dodecyl dimethyl sulfopropyl betaine, dodecyl sulfopropyl betaine, tetradecyl sulfopropyl betaine, hexadecyl sulfopropyl betaine, octadecyl sulfopropyl betaine, dodecyl dimethyl betaine, tetradecyl dimethyl betaine, octadecyl dimethyl betaine, dodecyl dihydroxyethyl betaine, octadecyl dihydroxyethyl betaine, lauroyl amidopropyl betaine, cocamidopropyl betaine, octadecyl amidopropyl betaine, dodecyl hydroxypropyl phosphate betaine, and tetradecyl hydroxypropyl phosphate betaine.
6. The method for catalytic pyrolysis of oil shale according to claim 3, characterized in that: The catalyst also needs to be prepared into a 0.1-1 wt% aqueous solution.
7. The method for catalytic pyrolysis of oil shale according to claim 1, characterized in that: In step S1, the mass ratio of the catalyst to the oil shale powder is 1:500-1000.
8. The method for catalytic pyrolysis of oil shale according to claim 1, characterized in that: In step S2, the temperature of the low-temperature drying is below 60°C.
9. The method for catalytic pyrolysis of oil shale according to claim 1, characterized in that: In step S2, the fluidized calcination is suspension calcination.
10. The method for catalytic pyrolysis of oil shale according to claim 1, characterized in that: In step S2, the calcination temperature is 350-600°C.
Citation Information
Patent Citations
Rare earth mesoporous molecular sieve, preparation method thereof and catalyst containing molecular sieve
CN114522722A
Cited By
Liquid catalyst system for in-situ conversion of oil shale as well as preparation method and application of liquid catalyst system
CN120961229A
In-situ catalytic conversion method of medium-low-maturity shale oil or oil shale
CN122609264A
Continuous effect-taking method for improving in-situ conversion oil and gas recovery ratio
CN122610831A