Hydroelectric steel with narrow yield strength and production method thereof
By controlling the chemical composition and process, narrow yield strength hydropower steel was produced, solving the problems of difficult production control and performance fluctuations. This resulted in hydropower steel plates with high strength, toughness, and fatigue resistance, meeting the usage requirements of key parts of hydropower stations.
Patent Information
- Application Number
- CN202410909072.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
The production and control of narrow yield strength hydropower steel is difficult. The yield strength range is narrow and the performance fluctuates greatly, making it difficult to meet the high strength, toughness and fatigue resistance requirements of key parts of hydropower stations.
By designing and manufacturing processes with appropriate chemical composition, controlling the chemical composition of the steel and the heating and rolling processes of the slab, a narrow yield strength range is ensured. The microstructure is pearlite + ferrite with a grain size of 9.0 or higher. The yield strength is 335-400 MPa, the tensile strength is 500-630 MPa, and the impact toughness at -20℃ is good.
The performance qualification rate of narrow yield strength hydropower steel has reached over 98%, which improves the reliability and safety of steel plate use, reduces the occurrence rate of surface cracks, and meets the performance requirements of key parts of hydropower stations.
Smart Images

Figure CN118880171A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgy, specifically relating to a narrow yield strength hydroelectric steel and its production method. Background Technology
[0002] Hydropower stations, as facilities that convert water energy into electrical energy, have strict requirements for the quality and performance of steel. Narrow yield strength hydropower steel, due to its high strength, good toughness, and fatigue resistance, is widely used in hydropower station construction. It is mainly used in key components such as dams, turbine generator support structures, and water pipelines, improving the reliability and safety of the hydropower station. The narrow yield strength range of narrow yield strength hydropower steel presents significant challenges in production control. However, through reasonable chemical composition design and matching with production processes, the performance qualification rate can be ensured to be controlled at over 98%. Summary of the Invention
[0003] To achieve the above objectives, this invention provides a narrow yield strength hydroelectric steel and its production method. The chemical composition of the steel, by mass percentage, is as follows: C: 0.14%–0.15%, Si: 0.30%–0.40%, Mn: 1.35%–1.40%, P≤0.020%, S≤0.005%, Alt: 0.030%–0.050%, Nb: 0.010%–0.015%, Ti: 0.015%–0.020%, with the remainder being Fe and residual elements.
[0004] The slab thickness of this invention is 180–350 mm, the thickness of the produced steel ranges from 16–40 mm, and the width is 2000–4200 mm. The steel plates produced using the slab heating and rolling method must meet the following mechanical properties: room temperature tensile yield strength ReL = 335–400 MPa, tensile strength Rm = 500–630 MPa, elongation A ≥ 21%, and Charpy V-notch impact value KV2 ≥ 47 J at -20℃. Specific details are shown in Table 1.
[0005] A method for producing narrow yield strength hydroelectric steel, the process flow of which involves slab heating and rolling, specifically including the following process steps:
[0006] a. Slab heating: The slab is heated in a walking beam furnace, with the furnace temperature limited to ≤1250℃. The slab is held in the soaking zone for ≥50min, and the billet tapping temperature is controlled at 1160~1220℃.
[0007] b. Rolling: The first stage rolling temperature is 1120~1180℃, the roughing rolling temperature is >920℃, and the intermediate billet thickness is ≥3 times the finished steel plate thickness; the second stage rolling temperature is 850~880℃, and the finishing rolling temperature is 780~820℃.
[0008] This invention discloses a narrow yield strength hydroelectric steel and its production method. Through reasonable chemical composition design and slab heating process, the furnace temperature is limited to ≤1250℃ to ensure that the original austenite grain size does not grow excessively. The slab is held in the soaking zone for ≥50min to fully promote the solid solution of Nb and Ti alloying elements. The two-stage rolling temperature is controlled at 850~880℃, and the finishing rolling temperature is controlled at 780~820℃. The final product has a pearlite + ferrite microstructure, a grain size of ≥9.0, a yield strength of 335~400MPa, a tensile strength of 500~630MPa, and good impact toughness at -20℃, with an impact strength ≥47J.
[0009] Explanation of the invention principle:
[0010] Narrowly controlled C content serves two purposes: First, it ensures minimal fluctuations in the composition of steel plates within the same batch, minimizing normal fluctuations in subsequent rolling processes. This prevents the yield strength of the steel plates from exceeding the acceptable range, resulting in minimal fluctuations in the overall performance of the steel plates. This improves both the performance qualification rate and the reliability and safety of steel plate use. Second, the design of lower C and Mn contents corresponds to lower carbon equivalent and Pcm values, reducing component segregation in the steel plates and significantly improving their internal quality, which is beneficial for weldability. The addition of 0.015%–0.020% Ti plays a nitrogen-fixing role during smelting, greatly reducing the incidence of surface cracks in the slab. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0012] Figure 1 This is a metallographic diagram of Embodiment 1 of the present invention;
[0013] Figure 2 This is a metallographic diagram of Embodiment 2 of the present invention. DETAILED DESCRIPTION
[0014] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0015] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0016] Example 1:
[0017] In this embodiment, the slab thickness is 260mm, and its chemical composition and mass percentage are as follows: C: 0.14%, Si: 0.32%, Mn: 1.38%, P: 0.015%, S: 0.0039%, Nb: 0.012%, Ti: 0.016%, Alt: 0.035%, as shown in Table 2.
[0018] Steel rolling process implementation:
[0019] (1) Slab heating: The slab is heated in a walking beam furnace at a furnace temperature of 1220℃. The slab is held in the soaking zone for 55 minutes and the slab tapping temperature is 1200℃.
[0020] (2) Rolling: The first stage rolling temperature is 1180℃, the roughing and finishing rolling temperature is 1060℃, and the thickness of the intermediate slab is 80mm; the second stage rolling temperature is 855℃, the finishing rolling temperature is 791℃, and the thickness of the rolled product is 28mm and the width is 3560mm.
[0021] The steel plate in this embodiment has a stable ferrite and pearlite microstructure. Its mechanical properties are as follows: room temperature tensile yield strength ReL: 371 MPa, tensile strength Rm: 532 MPa, elongation A: 25%, and Charpy V-notch impact values KV at -20℃: 180 J, 164 J, and 176 J, as shown in Table 3.
[0022] The final metallographic structure of the steel plate is shown in the attached figure. Figure 1 As shown in the figure, its grain size is above level 9.
[0023] Example 2:
[0024] In this embodiment, the slab thickness is 180mm, and its chemical composition and mass percentage are: C: 0.14%, Si: 0.33%, Mn: 1.39%, P: 0.014%, S: 0.0045%, Nb: 0.013%, Ti: 0.017%, Alt: 0.036%;
[0025] Steel rolling process implementation:
[0026] (1) Slab heating: The slab is heated in a walking beam furnace at a furnace temperature of 1230℃. The slab is held in the soaking zone for 60 minutes and the slab tapping temperature is 1215℃.
[0027] (2) Rolling: The first stage rolling temperature is 1190℃, the roughing and finishing rolling temperature is 990℃, and the thickness of the intermediate slab is 65mm; the second stage rolling temperature is 870℃, the finishing rolling temperature is 809℃, and the thickness of the rolled product is 16mm and the width is 2480mm.
[0028] The steel plate in this embodiment has a stable ferrite and pearlite structure. Its mechanical properties are as follows: room temperature tensile yield strength ReL: 381 MPa, tensile strength Rm: 540 MPa, elongation A: 24%, and Charpy V-notch impact values KV at -20℃: 192 J, 196 J, and 183 J, as shown in Table 3.
[0029] The final metallographic structure of the steel plate is shown in the attached figure. Figure 2 As shown in the figure, its grain size is 9-10.
[0030] Table 1 Performance Indicators of Steel Products
[0031]
[0032] Table 2. Chemical composition (wt.%) of the steels in each embodiment.
[0033] chemical composition C Si Mn P S Nb Ti Alt Example 1 0.14 0.32 1.38 0.015 0.0039 0.012 0.016 0.035 Example 2 0.14 0.33 1.39 0.014 0.0045 0.013 0.017 0.036
[0034] Table 3. Results of steel mechanical properties testing in each embodiment.
[0035]
[0036] As shown in Table 3, the room temperature tensile strength ReL is 335-400 MPa, Rm is 500-630 MPa, A ≥ 21%, and the average transverse impact energy KV2 at -20℃ is ≥ 47 J. The hydropower steel of this invention possesses stable narrow yield strength and good low-temperature toughness, while also meeting the ultrasonic flaw detection standard NB / T47013.3-2015 Level II or higher. It can be used in the hydropower industry where high weldability, toughness, and low-temperature impact performance are required.
[0037] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention are included within the scope of protection of the present invention.
Claims
1. A narrow yield strength hydropower steel, characterized in that: The chemical composition and mass percentage of the steel are: C: 0.14% ~ 0.15%, Si: 0.30% ~ 0.40%, Mn: 1.35% ~ 1.40%, P ≤ 0.020%, S ≤ 0.005%, Alt: 0.030% ~ 0.050%, Nb: 0.010% ~ 0.015%, Ti: 0.015% ~ 0.020%, and the rest are Fe and residual elements.
2. A method for producing narrow yield strength hydroelectric steel as claimed in claim 1, characterized in that: The key process steps include: (1) Slab heating: The slab is heated in a walking furnace, the furnace temperature is limited to ≤1250°C, the slab is kept in the soaking section for ≥50 min, and the billet tapping temperature is controlled at 1160-1220°C; (2) Rolling: The first-stage rolling temperature is 1120-1180°C, the rough rolling and final rolling temperature is greater than 920°C, and the intermediate billet thickness is ≥ 3 times the finished steel plate thickness; the second-stage rolling temperature is 850-880°C, and the finishing rolling temperature is 780-820°C.
3. The method for producing narrow yield strength hydroelectric steel according to claim 2, characterized in that: The slab has a thickness of 180 to 350 mm, the thickness of the produced steel ranges from 16 to 40 mm, and the width ranges from 2000 to 4200 mm.
4. A method for producing narrow yield strength hydroelectric steel according to claim 2 or 3, characterized in that: The mechanical properties of the steel plate after rolling are yield strength ReL=335~400Mpa, tensile strength Rm=500~630Mpa, elongation A≥21%, and Charpy V-notch impact value KV2≥47J at -20℃ of the steel plate.
5. The method for producing narrow yield strength hydroelectric steel according to claim 3, characterized in that: The structure of the obtained steel is ferrite and pearlite, and the grain size is above grade 9.
6. The method for producing narrow yield strength hydroelectric steel according to claim 3, characterized in that: The steel can be used in the hydropower industry which has high requirements on welding performance, toughness and low-temperature impact performance.