Seamless steel tube and processing technology thereof
By using specific elements and process processing in seamless steel pipes to form a composite passivation film, the problem of insufficient corrosion resistance of seamless steel pipes in corrosive environments is solved, and its corrosion resistance and service life are significantly improved.
Patent Information
- Application Number
- CN202410938928.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing seamless steel pipes are insufficient in corrosion resistance in corrosive environments, especially in humid climates in coastal areas, resulting in reduced material strength and plasticity and shortened service life.
Use a specific composition of seamless steel pipe, including C, Si, Cr, Mo, Al, P, S, V, Ni, Ti and other elements, to form composite passivation through smelting, forging, pickling, surface treatment and passivation processes. Films to improve corrosion resistance.
It significantly improves the mechanical strength and corrosion resistance of seamless steel pipes, extends the service life, and is suitable for large-scale industrial production.
Smart Images

Figure BDA0004943414110000271 
Figure BDA0004943414110000281
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of seamless steel pipes and preparation related thereto, and in particular to a seamless steel pipe and a processing technology thereof. Background Art
[0002] Seamless steel pipes have hollow cross-sections and are widely used in the fluid transportation pipeline industry. With the development trend of lightweighting, more and more industries are using seamless steel pipe components to replace the original solid components while ensuring strength and safety performance.
[0003] Due to the limitations of production technology, seamless steel pipes still have many quality defects, and some production defects cannot be eliminated through grinding and repairing processes, which greatly limits the application scope of seamless steel pipes. Patent CN104264044A discloses a new type of seamless steel pipe, ingots include the following substances by mass: C: 3-12 parts, SiO: 5-16 parts, MnO: 2-8 parts, V: 1-7 parts, Al: 4-16 parts, Ti: 1-3 parts, Mo: 2-6 parts, Zr: 0.4-3 parts, Mg: 4-9 parts, B: 0.1-0.5 parts and rare earth elements: 0.05-0.3 parts, the rest is Fe: 200-800 parts and impurities: 1-5 parts. The preparation process includes the following steps: a. using continuous casting to make a steel tube blank, cooling it to room temperature, and then immersing the surface of the steel tube in lubricating liquid; b. cold drawing the steel tube for multiple times, then heating the steel tube to 1200-1600℃ for normalizing, cooling it after insulation, and then heating it to 600-680℃ for tempering; c. then treating the surface of the steel tube with chromium-free Dacromet coating, and the baking and curing temperature is 350-400℃. The seamless steel tube prepared in the above manner has improved physical properties, long service life, corrosion resistance, and simple preparation process, but the seamless steel tube prepared in this way cannot meet the corrosion resistance requirements of seamless steel tubes in the prior art.
[0004] Different working environments have different quality requirements for seamless steel pipes. In coastal areas, due to the humid climate and salt content, after a period of use, the surface of some pipes is severely corroded, the strength and plasticity of the material are seriously reduced or lost, and the service life is shortened. Therefore, in the production process of seamless steel pipes, special smelting technology and processing technology are required to reduce the corrosion sensitivity of seamless steel pipes while ensuring the mechanical strength of seamless steel pipes, so as to achieve long-term use of seamless steel pipes in corrosive environments. Summary of the invention
[0005] 1. Technical issues to be solved
[0006] In view of the deficiencies in the prior art, the present invention provides a seamless steel pipe and a processing technology thereof, which solves the problems raised in the above-mentioned background technology.
[0007] (II) Technical solution
[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0009] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.12-0.18%, Si 0.20-0.25%, Cr 1.8-2.2%, Mo 0.2-0.3%, Al 0.05-0.15%, P 0.002-0.01%, S 0.01-0.02%, V 0.03-0.04%, Ni 0.3-0.5%, Ti 0.06-0.1%, and the balance is Fe and inevitable impurities.
[0010] Furthermore, the following components are included in weight percentage: C 0.15%, Si 0.22%, Cr 2.0%, Mo 0.25%, Al 0.1%, P 0.005%, S 0.015%, V 0.035%, Ni 0.4%, Ti 0.08%, and the balance is Fe and inevitable impurities.
[0011] A processing technology for a seamless steel pipe comprises the following steps:
[0012] S1: Weigh all the components of the seamless steel pipe according to weight percentage, then mix all the components, smelt at a temperature of 1210-1250° C., turn the material every 10-20 minutes during the smelting process, heat to 1280-1300° C. for forging, then cool to 1050-1080° C. to terminate forging, and form a round billet;
[0013] S2: heating the round billet at 1170-1210° C. for 3-4 hours, then piercing at 1110-1140° C., rolling at 1010-1030° C., with a tension reduction temperature of 850-870° C., and then cooling to 800-820° C. to terminate rolling to obtain a rough tube;
[0014] S3: Pickle the capillary tube with a 10-20% sulfuric acid aqueous solution at a temperature of 35-40°C for 15-30 minutes, wash it with water for 3-5 minutes, and then cold draw it at a temperature of 1000-1050°C, and size it at a temperature of 580-610°C.
[0015] Then straighten at a temperature of 300°C to 350°C;
[0016] S4: The straightened steel pipe is heated at 820-850°C, then kept warm for 1.5-2h, then quenched with water for 0.5-1h, then tempered at 600-630°C, kept warm for 1-2h, and straightened at 400-450°C;
[0017] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 20 to 30 minutes, then washed with water for 1 to 2 minutes, and then passivated with a passivation liquid for 30 to 40 minutes to obtain a finished seamless steel tube.
[0018] Furthermore, the surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0019] Furthermore, the surface treatment liquid includes the following components in terms of weight percentage: 30-40% phosphoric acid, 5-7% nitric acid, 0.2-0.4% polyoxyethylene alkylphenol ether, 1.5-2.5% sodium metasilicate, and the balance is water.
[0020] Furthermore, the preparation method of the passivation solution is:
[0021] A1: Add 3-5 parts of potassium fluorozirconate and 1-2 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until all are dissolved;
[0022] A2: Add 0.3-0.5 parts of isopropanolamine and 0.5-0.7 parts of sodium silicate to the stirred solution obtained in A1 under stirring, stir for 0.5-1h, heat to 60-65°C, and stir thoroughly;
[0023] A3: Slowly add 15-20 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction of A2 for 10-15 minutes, heat to 80-85°C, stir and react for 1-2 hours, add 8-12 parts of modified acrylic resin, stir and react for 20-30 minutes;
[0024] A4: Add 1-2 parts of hydrophobic nano-silica and 4-6 parts of a linker to the solution after the reaction of A3 by weight, and stir well to obtain a passivation concentrate;
[0025] A5: dilute the passivation concentrated solution with water to a mass concentration of 6-8% to obtain the passivation solution.
[0026] Furthermore, the preparation method of the modified acrylic resin is:
[0027] B1: Dissolve 0.05-0.15 parts of ammonium persulfate in 8-10 parts of deionized water to obtain an initiator solution;
[0028] B2: By weight, 80 parts of methyl methacrylate monomer, 15-25 parts of polyethylene glycol diacrylate monomer, 1-3 parts of diacetone acrylamide and 3-4 parts of methacrylic acid were mixed and ground for 5-10 minutes, and half of the initiator solution obtained in B1 and 20-30 parts of ethanol were added, and the grinding was continued for 5-8 minutes to obtain a prepolymer;
[0029] B3; Add 80 to 100 parts by weight of deionized water and the prepolymer obtained from B2 to the reactor, heat to 85 to 95°C, slowly drop the other half of the initiator solution for 5 to 10 minutes. After the addition is completed, keep warm for 20 to 30 minutes, adjust the pH to 8 to 9 with an ammonia solution, stir for 5 to 10 minutes, and obtain a modified acrylic resin.
[0030] Furthermore, the preparation method of the hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.5-0.7 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added to 25-35 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 0.5-1h, and then dried in an oven at 60-70°C to prepare hydrophobic nano-silica.
[0031] Furthermore, the preparation method of the linking agent is:
[0032] C1: Add 6 to 10 parts of sodium hydroxide by weight to 50 parts of 70 to 80% ethanol solution, stir until completely dissolved, then add 0.5 to 1 part of sodium lignin sulfonate and 0.4 to 0.6 parts of hydroxylated carbon nanotubes, stir for 10 to 20 minutes, and obtain a mixed solution;
[0033] C2: Add 8 to 12 parts of aniline methyl trimethoxy silane and 3 to 4 parts of isooctyl alcohol polyoxyethylene ether to the mixed solution by weight, react for 2 to 3 hours, seal and degas, and obtain a linker.
[0034] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0035] 1. Mo and Ti can make the internal structure of steel dense, refine the grain force, improve the hardenability and mechanical properties. The presence of Al, Si, S and P can reduce the brittleness of the material. By properly controlling the content of Ti and C, it can stabilize the lattice and improve the strength and corrosion resistance of the seamless steel pipe. V can refine the grain structure, improve the strength and toughness. The combination of V with Cr and Si can significantly improve the corrosion resistance of steel.
[0036] 2. The present invention provides a seamless steel pipe and processing technology, with a reasonable raw material composition ratio, a simple and environmentally friendly production process, and is suitable for large-scale industrial production. By selecting the components and controlling a series of process parameters, the prepared seamless steel pipe has high mechanical strength and corrosion resistance.
[0037] 3. The present invention performs pickling, surface roughening and passivation treatment on the seamless steel pipe, so that a composite passivation film that is effectively bonded to the steel pipe inside and hydrophobic outside is finally formed on the surface of the pipe. The composite passivation film is uniform and dense, has good film-forming properties, has high substrate adhesion, interlayer bonding strength and hydrophobic ability, forms an effective coating on the surface of the seamless steel pipe, and significantly improves the corrosion resistance of the seamless steel pipe.
[0038] 4. Phosphoric acid and nitric acid in the surface treatment liquid can etch the surface of the pipe; polyoxyethylene alkylphenol ether can reduce surface tension and the contact angle of the treatment liquid on the pipe, so that the treatment liquid can be well combined with the pipe surface and uniform etching can be achieved on the pipe surface; sodium metasilicate has certain dispersing, wetting and penetrating abilities, and by cooperating with polyoxyethylene alkyl ether, the treatment liquid can be better wetted and etched, and at the same time, the etched surface can have a higher hydrophilicity, forming a hydrophilic roughened surface, preparing for the next passivation treatment.
[0039] 5. Potassium fluorozirconate and modified acrylic resin are the main film-forming agents, potassium permanganate is the auxiliary film-forming agent, sodium silicate plays a stabilizing and corrosion-inhibiting role, and isopropanolamine can adjust the viscosity and surface tension of the passivation liquid, improve the intimacy and affinity between the passivation liquid and the pipe, and enable the passivation liquid to completely penetrate into the contour of the pipe surface treatment.
[0040] Acrylic resin has good mechanical properties, chemical resistance and film-forming ability. The present invention modifies acrylic resin to obtain a modified acrylic resin with good hydrophilicity, good compatibility with other hydrophilic components of the passivation solution, and forms an organic-inorganic composite hydrophilic layer with strong bonding force together with inorganic film-forming agents potassium fluorozirconate and permanganate. The steel pipe has a certain roughened surface and good hydrophilicity through surface treatment, so that the organic-inorganic composite hydrophilic layer has a high bonding ability with the steel pipe, thereby forming an effective coating on the steel pipe.
[0041] By modifying the nano-silica and adding side chains and hydrophobic groups on its surface, it has a certain dispersibility and hydrophobic properties. In addition, since fluoride has a high mobility, trifluoropropylmethyldiethoxysilane is used for surface modification to give the nano-silica a higher migration ability, so that it can precipitate from the inside of the system and migrate to the outside, and freely disperse on the outer surface of the passivation layer to form a uniform and dense hydrophobic layer, thereby improving the defense ability of the passivation film against corrosive liquids.
[0042] 6. Add a connector to the passivation solution. The connector can be inserted between the modified acrylic resin and the hydrophobic nano-silica, so that the two are tightly combined and the interlayer bonding force of the passivation film is enhanced. In addition, due to the addition of the connector, the hydrophilic groups in the modified acrylic resin can be attracted by the active groups in the connector, which can reduce the hydrophilicity of the modified acrylic resin in the outer direction, further improve the overall hydrophobicity of the passivation film, and finally form a composite passivation film with effective internal bonding and external hydrophobicity on the surface of the steel pipe, so as to achieve effective protection of the seamless steel pipe. DETAILED DESCRIPTION
[0043] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Embodiment 1:
[0045] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.15%, Si 0.22%, Cr 2.0%, Mo 0.25%, Al 0.1%, P 0.005%, S 0.015%, V 0.035%, Ni 0.4%, Ti 0.08%, and the balance is Fe and inevitable impurities.
[0046] The processing technology of seamless steel pipe includes the following steps:
[0047] S1: Weigh all the components of the seamless steel pipe by weight, then mix all the components, smelt at 1230° C., turn the material every 15 minutes during the smelting process, heat to 1290° C. for forging, then cool to 1060° C. to terminate forging, and form a round billet;
[0048] S2: heating the round billet at 1180° C. for 4 hours, then piercing at 1120° C., rolling at 1120° C., with a tension reduction temperature of 860° C., and then cooling to 810° C. to terminate rolling to obtain a rough tube;
[0049] S3: pickling the wool tube with a 15% sulfuric acid aqueous solution at 40°C for 20 minutes, washing it with water for 4 minutes, cold drawing it with a cold drawing temperature of 1020°C, sizing it at 600°C, and then straightening it at 350°C;
[0050] S4: The straightened steel pipe is heated at 830°C, then kept at this temperature for 2 hours, and then quenched with water for 1 hour, and then tempered at 620°C, kept at this temperature for 1.5 hours, and straightened at 450°C to obtain a steel pipe blank;
[0051] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 25 minutes, then washed with water for 2 minutes, and then passivated with a passivation liquid for 30 minutes to obtain a finished seamless steel tube.
[0052] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0053] The surface treatment liquid includes the following components by weight percentage: 35% phosphoric acid, 6% nitric acid, 0.3% polyoxyethylene alkylphenol ether, 2% sodium metasilicate, and the balance is water.
[0054] The preparation method of the passivation solution is:
[0055] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0056] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0057] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 minutes, heat to 85°C, stir and react for 1 hour, add 10 parts of modified acrylic resin, and stir and react for 30 minutes;
[0058] A4: Add 1.5 parts of hydrophobic nano-silica and 5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0059] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0060] The preparation method of modified acrylic resin is:
[0061] B1: Dissolve 0.1 parts of ammonium persulfate in 9 parts of deionized water to obtain an initiator solution;
[0062] B2: 80 parts by weight of methyl methacrylate monomer, 20 parts of polyethylene glycol diacrylate monomer, 2 parts of diacetone acrylamide and 3.5 parts of methacrylic acid were mixed and ground for 8 minutes, half of the initiator solution obtained in B1 and 25 parts of ethanol were added, and the grinding was continued for 7 minutes to obtain a prepolymer;
[0063] B3; Add 90 parts by weight of deionized water and the prepolymer obtained from B2 to the reactor, heat to 90°C, slowly drop the other half of the initiator solution, the dropping time is 8 minutes, after the dropping is completed, keep warm for 25 minutes, adjust the pH to 8 with an ammonia solution, stir for 10 minutes, and obtain a modified acrylic resin.
[0064] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.6 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added into 30 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 1 hour, and then dried in an oven at 60°C to prepare hydrophobic nano-silica.
[0065] The preparation method of the linker is:
[0066] C1: By weight, 8 parts of sodium hydroxide were added to 50 parts of 75% ethanol solution, stirred until completely dissolved, and then 0.7 parts of sodium lignin sulfonate and 0.5 parts of hydroxylated carbon nanotubes were added, stirred for 15 minutes, to obtain a mixed solution;
[0067] C2: 10 parts of aniline methyl trimethoxy silane and 3.5 parts of isooctyl polyoxyethylene ether were added to the mixed solution by weight, and after fully reacting for 3 hours, the mixture was sealed and degassed to obtain a linker.
[0068] Embodiment 2:
[0069] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.12%, Si 0.20%, Cr 1.8%, Mo 0.2%, Al 0.05%, P 0.002%, S 0.01%, V 0.03%, Ni 0.3%, Ti 0.06%, and the balance is Fe and inevitable impurities.
[0070] The processing technology of seamless steel pipe includes the following steps:
[0071] S1: Weigh all the components of the seamless steel pipe by weight, then mix all the components, smelt at 1210° C., turn the material every 10 minutes during the smelting process, heat to 1280° C. for forging, then cool to 1050° C. to terminate forging, and form a round billet;
[0072] S2: heating the round billet at 1170° C. for 3 hours, then piercing at 1110° C., rolling at 1010° C., with a tension reduction temperature of 860° C., and then cooling to 810° C. to terminate rolling to obtain a rough tube;
[0073] S3: pickling the wool tube with a 15% sulfuric acid aqueous solution at 40°C for 15 minutes, washing it with water for 3 minutes, cold drawing it with a cold drawing temperature of 1000°C, sizing it at 600°C, and then straightening it at 300°C;
[0074] S4: The straightened steel pipe is heated at 820°C, then kept at this temperature for 1.5 hours, then quenched with water for 0.5 hours, then tempered at 600°C, kept at this temperature for 1 hour, and straightened at 400°C to obtain a steel pipe blank;
[0075] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 20 minutes, then washed with water for 1 minute, and then passivated with a passivation liquid for 30 minutes to obtain a finished seamless steel tube.
[0076] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0077] The surface treatment liquid includes the following components by weight percentage: 30% phosphoric acid, 5% nitric acid, 0.2% polyoxyethylene alkylphenol ether, 1.5% sodium metasilicate, and the balance is water.
[0078] The preparation method of the passivation solution is:
[0079] A1: Add 3 parts of potassium fluorozirconate and 1 part of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0080] A2: Add 0.3 parts of isopropanolamine and 0.5 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 0.5 hours, heat to 60°C, and stir thoroughly;
[0081] A3: Slowly add 15 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 minutes, heat to 80°C, stir and react for 1 hour, add 8 parts of modified acrylic resin, and stir and react for 20 minutes;
[0082] A4: Add 1 part of hydrophobic nano-silica and 4 parts of a linker to the solution after the reaction of A3 by weight, and stir well to obtain a passivation concentrate;
[0083] A5: The passivation concentrated solution is diluted with water to a mass concentration of 6% to obtain the passivation solution.
[0084] The preparation method of modified acrylic resin is:
[0085] B1: Dissolve 0.05 parts of ammonium persulfate in 8 parts of deionized water to obtain an initiator solution;
[0086] B2: 80 parts by weight of methyl methacrylate monomer, 15 parts of polyethylene glycol diacrylate monomer, 1 part of diacetone acrylamide and 3 parts of methacrylic acid were mixed and ground for 5 minutes, half of the initiator solution obtained in B1 and 20 parts of ethanol were added, and the grinding was continued for 5 minutes to obtain a prepolymer;
[0087] B3; Add 80 parts by weight of deionized water and the prepolymer obtained from B2 to the reactor, heat to 85°C, slowly drop the other half of the initiator solution, the dropping time is 5 minutes, after the dropping is completed, keep warm for 20 minutes, adjust the pH to 8 with an ammonia solution, stir for 5 minutes, and obtain a modified acrylic resin.
[0088] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.5 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added to 25 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 0.5 hours, and then dried in an oven at 60°C to prepare hydrophobic nano-silica.
[0089] The preparation method of the linker is:
[0090] C1: by weight, 6 parts of sodium hydroxide were added to 50 parts of 70% ethanol solution, stirred until completely dissolved, and then 0.5 parts of sodium lignin sulfonate and 0.4 parts of hydroxylated carbon nanotubes were added, stirred for 10 minutes, to obtain a mixed solution;
[0091] C2: Add 8 parts of aniline methyl trimethoxy silane and 3 parts of isooctyl alcohol polyoxyethylene ether to the mixed solution by weight, react for 2 hours, seal and degas, and obtain a linker.
[0092] Embodiment 3:
[0093] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.18%, Si 0.25%, Cr 2.2%, Mo 0.3%, Al 0.15%, P 0.01%, S 0.02%, V 0.04%, Ni 0.5%, Ti 0.1%, and the balance is Fe and inevitable impurities.
[0094] The processing technology of seamless steel pipe includes the following steps:
[0095] S1: Weigh all the components of the seamless steel pipe by weight, then mix all the components, smelt at 1250° C., turn the material every 20 minutes during the smelting process, heat to 1300° C. for forging, then cool to 1080° C. to terminate forging, and form a round billet;
[0096] S2: heating the round billet at 1210° C. for 4 hours, then piercing at 1140° C., rolling at 1030° C., with a tension reduction temperature of 870° C., and then cooling to 820° C. to terminate rolling to obtain a rough tube;
[0097] S3: pickling the wool tube with a 20% sulfuric acid aqueous solution at 40°C for 30 minutes, washing it with water for 5 minutes, cold drawing it with a cold drawing temperature of 1050°C, sizing it at 580°C, and then straightening it at 300°C;
[0098] S4: The straightened steel pipe is heated at 850°C, then kept at this temperature for 2 hours, and then quenched with water for 1 hour, and then tempered at 630°C, kept at this temperature for 2 hours, and straightened at 450°C to obtain a steel pipe blank;
[0099] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 30 minutes, then washed with water for 2 minutes, and then passivated with a passivation liquid for 40 minutes to obtain a finished seamless steel tube.
[0100] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0101] The surface treatment liquid comprises the following components: 40% phosphoric acid, 7% nitric acid, 0.4% polyoxyethylene alkylphenol ether, 2.5% sodium metasilicate, and the balance is water.
[0102] The preparation method of the passivation solution is:
[0103] A1: Add 5 parts of potassium fluorozirconate and 2 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0104] A2: Add 0.5 parts of isopropanolamine and 0.7 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 65°C, and stir thoroughly;
[0105] A3: Slowly add 20 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution obtained in A2 for 15 minutes, heat to 85°C, stir and react for 2 hours, add 12 parts of modified acrylic resin, and stir and react for 30 minutes;
[0106] A4: Add 2 parts of hydrophobic nano-silica and 6 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0107] A5: The passivation concentrated solution is diluted with water to a mass concentration of 8% to obtain the passivation solution.
[0108] The preparation method of modified acrylic resin is:
[0109] B1: Dissolve 0.15 parts of ammonium persulfate in 10 parts of deionized water to obtain an initiator solution;
[0110] B2: 80 parts by weight of methyl methacrylate monomer, 25 parts of polyethylene glycol diacrylate monomer, 3 parts of diacetone acrylamide and 4 parts of methacrylic acid were mixed and ground for 10 minutes, half of the initiator solution obtained in B1 and 30 parts of ethanol were added, and the grinding was continued for 8 minutes to obtain a prepolymer;
[0111] B3; Add 100 parts by weight of deionized water and the prepolymer obtained from B2 to the reactor, heat to 95°C, slowly drop the other half of the initiator solution, the dropping time is 10 minutes, after the dropping is completed, keep warm for 30 minutes, adjust the pH to 9 with an ammonia solution, stir for 10 minutes, and obtain a modified acrylic resin.
[0112] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.7 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added to 35 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 1 hour, and then dried in an oven at 70°C to prepare hydrophobic nano-silica.
[0113] The preparation method of the linker is:
[0114] C1: By weight, 10 parts of sodium hydroxide were added to 50 parts of 80% ethanol solution, stirred until completely dissolved, and then 1 part of sodium lignin sulfonate and 0.6 parts of hydroxylated carbon nanotubes were added, stirred for 20 minutes, to obtain a mixed solution;
[0115] C2: Add 12 parts of aniline methyl trimethoxy silane and 4 parts of isooctyl alcohol polyoxyethylene ether to the mixed solution by weight, react for 3 hours, seal and degas, and obtain a linker.
[0116] Embodiment 4:
[0117] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.14%, Si 0.22%, Cr 1.9%, Mo 0.23%, Al 0.08%, P 0.005%, S 0.013%, V 0.034%, Ni 0.35%, Ti 0.07%, and the balance is Fe and inevitable impurities.
[0118] The processing technology of seamless steel pipe includes the following steps:
[0119] S1: Weigh all the components of the seamless steel pipe by weight, then mix all the components, smelt at 1220° C., turn the material every 12 minutes during the smelting process, heat to 1285° C. for forging, then cool to 1060° C. to terminate forging, and form a round billet;
[0120] S2: heating the round billet at 1180° C. for 3.3 h, then piercing at 1120° C., rolling at 1015° C., with a tension reduction temperature of 855° C., and then cooling to 805° C. to terminate rolling to obtain a rough tube;
[0121] S3: pickling the wool tube with a 12% sulfuric acid aqueous solution at 36°C for 20 minutes, washing it with water for 3.5 minutes, cold drawing it with a cold drawing temperature of 1010°C, sizing it at 590°C, and then straightening it at 310°C;
[0122] S4: The straightened steel pipe is heated at 825°C, then kept at this temperature for 1.6 hours, then quenched with water for 0.6 hours, then tempered at 605°C, kept at this temperature for 1.2 hours, and straightened at 410°C to obtain a steel pipe blank;
[0123] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 22 minutes, then washed with water for 1 to 2 minutes, and then passivated with a passivation liquid for 32 minutes to obtain a finished seamless steel tube.
[0124] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0125] The surface treatment liquid includes the following components by weight percentage: 32% phosphoric acid, 5.5% nitric acid, 0.25% polyoxyethylene alkylphenol ether, 1.8% sodium metasilicate, and the balance is water.
[0126] The preparation method of the passivation solution is:
[0127] A1: Add 3.5 parts of potassium fluorozirconate and 1.2 parts of potassium permanganate, by weight, to 20 parts of water at the same time, stirring until all are dissolved;
[0128] A2: Add 0.35 parts of isopropanolamine and 0.55 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 0.6 hours, heat to 62°C, and stir thoroughly;
[0129] A3: Slowly add 17 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution obtained in A2 for 12 minutes, heat to 82°C, stir and react for 1.2 hours, add 9 parts of modified acrylic resin, and stir and react for 22 minutes;
[0130] A4: Add 1.2 parts of hydrophobic nano-silica and 4.5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0131] A5: The passivation concentrated solution is diluted with water to a mass concentration of 6.5% to obtain the passivation solution.
[0132] The preparation method of modified acrylic resin is:
[0133] B1: Dissolve 0.08 parts of ammonium persulfate in 8.5 parts of deionized water to obtain an initiator solution;
[0134] B2: 80 parts by weight of methyl methacrylate monomer, 18 parts of polyethylene glycol diacrylate monomer, 1.5 parts of diacetone acrylamide and 3.2 parts of methacrylic acid were mixed and ground for 6 minutes, half of the initiator solution obtained in B1 and 22 parts of ethanol were added, and the grinding was continued for 6 minutes to obtain a prepolymer;
[0135] B3; Add 85 parts of deionized water and the prepolymer obtained from B2 to the reactor by weight, heat to 88°C, slowly add the other half of the initiator solution dropwise for 6 minutes. After the addition is completed, keep warm for 22 minutes, adjust the pH to 8 with an ammonia solution, stir for 6 minutes, and obtain a modified acrylic resin.
[0136] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.55 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added to 28 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 0.6 hours, and then dried in an oven at 63°C to prepare hydrophobic nano-silica.
[0137] The preparation method of the linker is:
[0138] C1: 7 parts of sodium hydroxide were added to 50 parts of 72% ethanol solution by weight, and stirred until completely dissolved. Then, 0.8 parts of sodium lignin sulfonate and 0.45 parts of hydroxylated carbon nanotubes were added, and stirred for 12 minutes to obtain a mixed solution.
[0139] C2: Add 9 parts of aniline methyl trimethoxy silane and 3.2 parts of isooctyl polyoxyethylene ether to the mixed solution by weight, react for 2 hours, seal and degas, and obtain a linker.
[0140] Embodiment 5:
[0141] A seamless steel pipe comprises the following components, measured by weight percentage: C 0.17%, Si 0.24%, Cr2.1%, Mo 0.28%, Al 0.13%, P 0.008%, S 0.018%, V 0.038%, Ni 0.45%, Ti 0.09%, and the balance is Fe and inevitable impurities.
[0142] The processing technology of seamless steel pipe includes the following steps:
[0143] S1: Weigh all the components of the seamless steel pipe by weight, then mix all the components, smelt at 1240° C., turn the material every 18 minutes during the smelting process, heat to 1295° C. for forging, then cool to 1075° C. to terminate forging, and form a round billet;
[0144] S2: heating the round billet at 1200° C. for 3.8 h, then piercing at 1130° C., rolling at 1025° C., with a tension reduction temperature of 865° C., and then cooling to 815° C. to terminate rolling to obtain a rough tube;
[0145] S3: The wool tube is pickled with an 18% sulfuric acid aqueous solution at a temperature of 38°C for 25 minutes, then washed with water for 4.5 minutes, then cold drawn at a temperature of 1045°C, sized at a temperature of 600°C, and then straightened at a temperature of 340°C;
[0146] S4: The straightened steel pipe is heated at 840°C, then kept at this temperature for 1.8 hours, then quenched with water for 0.8 hours, then tempered at 625°C, kept at this temperature for 1.8 hours, and straightened at 440°C to obtain a steel pipe blank;
[0147] S5: The steel tube blank obtained in S4 is surface treated with a surface treatment liquid for 29 minutes, then washed with water for 1.8 minutes, and then passivated with a passivation liquid for 39 minutes to obtain a finished seamless steel tube.
[0148] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
[0149] The surface treatment liquid includes the following components by weight percentage: 38% phosphoric acid, 6.5% nitric acid, 0.35% polyoxyethylene alkylphenol ether, 2.3% sodium metasilicate, and the balance is water.
[0150] The preparation method of the passivation solution is:
[0151] A1: Add 4.5 parts of potassium fluorozirconate and 1.9 parts of potassium permanganate, by weight, to 20 parts of water at the same time, stirring until all are dissolved;
[0152] A2: Add 0.45 parts of isopropanolamine and 0.65 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 0.8 hours, heat to 64°C, and stir thoroughly;
[0153] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution obtained in A2 for 14 minutes, heat to 84°C, stir and react for 1.8 hours, add 10 parts of modified acrylic resin, and stir and react for 28 minutes;
[0154] A4: Add 1.9 parts of hydrophobic nano-silica and 5.5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0155] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7.5% to obtain the passivation solution.
[0156] The preparation method of modified acrylic resin is:
[0157] B1: Dissolve 0.13 parts of ammonium persulfate in 9.5 parts of deionized water to obtain an initiator solution;
[0158] B2: 80 parts by weight of methyl methacrylate monomer, 23 parts of polyethylene glycol diacrylate monomer, 2.5 parts of diacetone acrylamide and 3.5 parts of methacrylic acid were mixed and ground for 9 minutes, half of the initiator solution obtained in B1 and 28 parts of ethanol were added, and the grinding was continued for 7.5 minutes to obtain a prepolymer;
[0159] B3: Add 95 parts of deionized water and the prepolymer obtained from B2 to the reactor by weight, heat to 93°C, slowly drop the other half of the initiator solution, the drop time is 8 minutes, after the drop addition is completed, keep warm for 28 minutes, adjust the pH to 9 with an ammonia solution, stir for 8 minutes, and obtain a modified acrylic resin
[0160] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.65 parts of trifluoropropylmethyldiethoxysilane are mixed evenly, and then added to 33 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 0.9 hours, and then dried in an oven at 68°C to prepare hydrophobic nano-silica.
[0161] The preparation method of the linker is:
[0162] C1: 9 parts of sodium hydroxide were added to 50 parts of 79% ethanol solution by weight, and stirred until completely dissolved. Then, 0.7 parts of sodium lignin sulfonate and 0.55 parts of hydroxylated carbon nanotubes were added, and stirred for 18 minutes to obtain a mixed solution.
[0163] C2: 11 parts of aniline methyl trimethoxy silane and 3.8 parts of isooctyl polyoxyethylene ether were added to the mixed solution by weight, and after fully reacting for 3 hours, the mixture was sealed and degassed to obtain a linker.
[0164] Comparative Example 1
[0165] Compared with Example 1, the difference is that Ti in the raw material composition of the seamless steel pipe is replaced by Mo.
[0166] A seamless steel pipe comprises the following components, measured by weight percentage: 0.15% C, 0.22% Si, 2% Cr, 0.33% Mo, 0.1% Al, 0.005% P, 0.015% S, 0.035% V, 0.4% Ni, and the balance is Fe and inevitable impurities.
[0167] Comparative Example 2
[0168] Compared with Example 1, the difference is that: V in the raw material composition of the seamless steel pipe is replaced by Al;
[0169] A seamless steel pipe comprises the following components, measured by weight percentage: 0.15% C, 0.22% Si, 2% Cr, 0.25% Mo, 0.135% Al, 0.005% P, 0.015% S, 0.4% Ni, 0.08% Ti, and the balance is Fe and inevitable impurities.
[0170] Comparative Example 3
[0171] Compared with Example 1, the difference is that in the surface treatment liquid, sodium metasilicate is replaced by polyoxyethylene alkylphenol ether.
[0172] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid and polyoxyethylene alkylphenol ether.
[0173] The surface treatment liquid includes the following components by weight percentage: 35% phosphoric acid, 6% nitric acid, 2.3% polyoxyethylene alkylphenol ether, and the balance is water.
[0174] Comparative Example 4
[0175] Compared with Example 1, the difference is that: in the surface treatment liquid, the polyoxyethylene alkylphenol ether is replaced by sodium metasilicate;
[0176] The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid and sodium metasilicate.
[0177] The surface treatment liquid includes the following components by weight percentage: 35% phosphoric acid, 6% nitric acid, 2.3% sodium metasilicate, and the balance is water.
[0178] Comparative Example 5
[0179] Compared with Example 1, the difference is that: no polyoxyethylene alkylphenol ether and sodium metasilicate are added to the surface treatment liquid;
[0180] The surface treatment solution is a mixed aqueous solution of phosphoric acid and nitric acid.
[0181] The surface treatment liquid includes the following components by weight percentage: 35% phosphoric acid, 6% nitric acid, and the balance is water.
[0182] Comparative Example 6
[0183] Compared with Example 1, the difference is that no hydrophobic nano-silica is added in the preparation of the passivation solution.
[0184] The preparation method of the passivation solution is:
[0185] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0186] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0187] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 minutes, heat to 85°C, stir and react for 1 hour, add 10 parts of modified acrylic resin, and stir and react for 30 minutes;
[0188] A4: Add 5 parts of linker by weight to the solution after the reaction of A3, stir thoroughly to obtain a passivation concentrated solution;
[0189] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0190] Comparative Example 7
[0191] Compared with Example 1, the difference is that no modified acrylic resin is added in the preparation of the passivation solution.
[0192] The preparation method of the passivation solution is:
[0193] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0194] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0195] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 min, heat to 85°C, and stir for 1 h.
[0196] A4: Add 1.5 parts of hydrophobic nano-silica and 5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0197] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0198] Comparative Example 8
[0199] Compared with Example 1, the difference is that no linking agent is added in the preparation of the passivation solution.
[0200] The preparation method of the passivation solution is:
[0201] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0202] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0203] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 minutes, heat to 85°C, stir and react for 1 hour, add 10 parts of modified acrylic resin, and stir and react for 30 minutes;
[0204] A4: Add 1.5 parts by weight of hydrophobic nano-silica to the solution after the reaction in A3, stir thoroughly to obtain a passivation concentrate;
[0205] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0206] Comparative Example 9
[0207] Compared with Example 1, the difference is that in the preparation of the passivation solution, the modified acrylic resin is replaced by commercially available acrylic resin 6727 purchased from Qingdao Jinwanli Chemical Company.
[0208] The preparation method of the passivation solution is:
[0209] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0210] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution of A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0211] A3: Slowly add 18 parts by weight of 30% potassium fluorozirconate aqueous solution to the solution after the reaction of A2 for 10 minutes, heat to 85°C, stir and react for 1 hour, add 10 parts of acrylic resin 6727, and stir and react for 30 minutes;
[0212] A4: Add 1.5 parts of hydrophobic nano-silica and 5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0213] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0214] Comparative Example 10
[0215] Compared with Example 1, the difference is that in the preparation of the passivation solution, the hydrophobic nano-silica is replaced by untreated nano-silica.
[0216] The preparation method of the passivation solution is:
[0217] A1: Add 4 parts of potassium fluorozirconate and 1.5 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring until they are completely dissolved;
[0218] A2: Add 0.4 parts of isopropanolamine and 0.6 parts of sodium silicate to the solution obtained in A1 under stirring, stir for 1 hour, heat to 60°C, and stir thoroughly;
[0219] A3: Slowly add 18 parts by weight of a 30% potassium fluorozirconate aqueous solution to the solution after the reaction in A2 for 10 minutes, heat to 85°C, stir and react for 1 hour, add 10 parts of modified acrylic resin, and stir and react for 30 minutes;
[0220] A4: Add 1.5 parts of nano-silicon dioxide and 5 parts of a linker to the solution after the reaction in A3 by weight, and stir well to obtain a passivation concentrate;
[0221] A5: The passivation concentrated solution is diluted with water to a mass concentration of 7% to obtain the passivation solution.
[0222] Nano-silica is not treated.
[0223] Comparative Example 11
[0224] Compared with Example 1, the difference is that in the passivation solution, during the preparation of the connecting agent, the hydroxylated carbon nanotubes are replaced by untreated carbon nanotubes.
[0225] The preparation method of the linker is:
[0226] C1: By weight, 8 parts of sodium hydroxide were added to 50 parts of 75% ethanol solution, stirred until completely dissolved, and then 0.7 parts of sodium lignin sulfonate and 0.5 parts of carbon nanotubes were added, stirred for 15 minutes, and a mixed solution was obtained;
[0227] C2: 10 parts of aniline methyl trimethoxy silane and 3.5 parts of isooctyl polyoxyethylene ether were added to the mixed solution by weight, and after fully reacting for 3 hours, the mixture was sealed and degassed to obtain a linker.
[0228] Comparative Example 12
[0229] Compared with Example 1, the difference is that: in the passivation solution, during the preparation of the hydrophobic nano-silica, trifluoropropylmethyldiethoxysilane is replaced by γ-aminopropyltriethoxysilane;
[0230] The preparation method of hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.6 parts of γ-aminopropyltriethoxysilane are mixed evenly, and then added into 30 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 1 hour, and then dried in an oven at 60° C. to prepare hydrophobic nano-silica.
[0231] Performance Testing
[0232] The seamless steel pipes prepared by the schemes described in the embodiment and the comparative example were respectively tested for mechanical properties and corrosion resistance. The corrosion resistance test was carried out according to the method described in the national industry standard "GB / T10125-2021". The neutral salt spray resistance of the seamless steel pipe was tested. The test cycle was 30 days. The tensile strength was the tensile strength before corrosion, and the test was carried out according to the ASTM standard.
[0233]
[0234]
[0235] According to Table 1 and the examples, Examples 1 to 5 show that the corrosion resistance and tensile strength of the technical solution provided by the present invention are relatively excellent.
[0236] Comparative Example 1
[0237] Compared with Example 1, the difference is that Ti in the raw material composition of the seamless steel pipe is replaced by Mo.
[0238] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 , the tensile strength is 933.4Mpa. The corrosion rate of the seamless steel pipe in Comparative Example 1 is 31.5g / m 2 , and the tensile strength is 756.3Mpa. The corrosion rate of the seamless steel pipe in Comparative Example 1 is higher than that of the seamless steel pipe prepared in Example 1, and the tensile strength of the seamless steel pipe in Comparative Example 1 is lower than that of the seamless steel pipe prepared in Example 1, indicating that Ti can improve the corrosion resistance and tensile strength of the seamless steel pipe.
[0239] Comparative Example 2
[0240] Compared with Example 1, the difference is that V in the raw material composition of the seamless steel pipe is replaced by Al.
[0241] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 , the tensile strength is 933.4Mpa. The corrosion rate of the seamless steel pipe in Comparative Example 2 is 39.6g / m 2 , the tensile strength is 810.8Mpa. The corrosion rate of the seamless steel pipe in Comparative Example 2 is higher than that of the seamless steel pipe prepared in Example 1, and the tensile strength of the seamless steel pipe in Comparative Example 2 is lower than that of the seamless steel pipe prepared in Example 1, indicating that V can improve the corrosion resistance and tensile strength of the seamless steel pipe.
[0242] Comparative Example 3
[0243] Compared with Example 1, the difference is that in the surface treatment liquid, sodium metasilicate is replaced by polyoxyethylene alkylphenol ether.
[0244] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 3 is 37.2 g / m 2 , which is higher than the corrosion rate of the seamless steel pipe prepared in Example 1, indicating that sodium metasilicate can improve the corrosion resistance of the seamless steel pipe.
[0245] Comparative Example 4
[0246] Compared with Example 1, the difference is that in the surface treatment liquid, the polyoxyethylene alkylphenol ether is replaced by sodium metasilicate.
[0247] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 4 is 39.8 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 4 is higher than that of the seamless steel pipe prepared in Example 1, indicating that polyoxyethylene alkylphenol ether can improve the corrosion resistance of the seamless steel pipe.
[0248] Comparative Example 5
[0249] Compared with Example 1, the difference is that no polyoxyethylene alkylphenol ether and sodium metasilicate are added to the surface treatment liquid.
[0250] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 5 is 51.6 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 5 is higher than the corrosion rates of the seamless steel pipes prepared in Example 1, Comparative Example 3 and Comparative Example 4, respectively, indicating that polyoxyethylene alkylphenol ether and sodium metasilicate have a positive synergistic effect on improving the corrosion resistance of the seamless steel pipe.
[0251] Comparative Example 6
[0252] Compared with Example 1, the difference is that no hydrophobic nano-silica is added in the preparation of the passivation solution.
[0253] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 6 is 65.3 g / m 2 , indicating that hydrophobic silica can improve the corrosion resistance of seamless steel pipes.
[0254] Comparative Example 7
[0255] Compared with Example 1, the difference is that no modified acrylic resin is added in the preparation of the passivation solution.
[0256] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m2 , the tensile strength is 933.4Mpa. The corrosion rate of the seamless steel pipe in Comparative Example 7 is 71.4g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 7 is higher than that of the seamless steel pipe prepared in Example 1, indicating that the modified acrylic resin can improve the corrosion resistance of the seamless steel pipe.
[0257] Comparative Example 8
[0258] Compared with Example 1, the difference is that no linking agent is added in the preparation of the passivation solution.
[0259] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 8 is 60.7 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 8 is higher than that of the seamless steel pipe prepared in Example 1, indicating that the connecting agent can improve the corrosion resistance of the seamless steel pipe.
[0260] Comparative Example 9
[0261] Compared with Example 1, the difference is that in the preparation of the passivation solution, the modified acrylic resin is replaced by commercially available acrylic resin 6727 purchased from Qingdao Jinwanli Chemical Company.
[0262] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 9 is 58.7 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 9 is higher than that of the seamless steel pipe prepared in Example 1. Combined with the corrosion rate of the seamless steel pipe prepared in Comparative Example 7, it is shown that the modified acrylic resin can improve the corrosion resistance of the seamless steel pipe.
[0263] Comparative Example 10
[0264] Compared with Example 1, the difference is that in the preparation of the passivation solution, the hydrophobic nano-silica is replaced by untreated nano-silica.
[0265] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 10 is 57.1 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 10 is higher than that of the seamless steel pipe prepared in Example 1. Combined with the corrosion rate of the seamless steel pipe prepared in Comparative Example 6, it is shown that the corrosion resistance of the seamless steel pipe can be improved after the hydrophobic treatment of nano-silicon dioxide.
[0266] Comparative Example 11
[0267] Compared with Example 1, the difference is that in the passivation solution, during the preparation of the connecting agent, the hydroxylated carbon nanotubes are replaced by untreated carbon nanotubes.
[0268] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 11 is 50.2 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 11 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1, indicating that hydroxylated carbon nanotubes can improve the corrosion resistance of the seamless steel pipe.
[0269] Comparative Example 12
[0270] Compared with Example 1, the difference is that in the passivation solution, during the preparation of the hydrophobic nano-silica, trifluoropropylmethyldiethoxysilane is replaced by γ-aminopropyltriethoxysilane.
[0271] The corrosion rate of the seamless steel pipe in Example 1 is 15.4 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 12 is 53.6 g / m 2 The corrosion rate of the seamless steel pipe in Comparative Example 12 is higher than the corrosion rate of the seamless steel pipe prepared in Example 1, indicating that trifluoropropylmethyldiethoxysilane can improve the corrosion resistance of the seamless steel pipe.
[0272] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A seamless steel pipe, Features: Calculated by weight percentage, the invention comprises the following components: C 0.12-0.18%, Si 0.20-0.25%, Cr 1.8-2.2%, Mo 0.2-0.3%, Al 0.05-0.15%, P 0.002-0.01%, S 0.01-0.02%, V 0.03-0.04%, Ni 0.3-0.5%, Ti 0.06-0.1%, and the balance is Fe and unavoidable impurities.
2. A seamless steel pipe according to claim 1, Features: Calculated by weight percentage, the alloy comprises the following components: C 0.15%, Si 0.22%, Cr 2.0%, Mo 0.25%, Al 0.1%, P 0.005%, S 0.015%, V 0.035%, Ni 0.4%, Ti 0.08%, and the balance is Fe and unavoidable impurities.
3. A process for processing a seamless steel pipe according to any one of claims 1 or 2, Features: The following steps are involved: S 1 : Weigh all the components of the seamless steel pipe by weight percentage, then mix all the components, smelt at a temperature of 1210-1250° C., turn the material every 10-20 minutes during the smelting process, heat to 1280-1300° C. for forging, then cool to 1050-1080° C. to terminate forging, and form a round billet; S 2 : The round billet is heated at 1170-1210° C. for 3-4 hours, then pierced at 1110-1140° C., rolled at 1010-1030° C., the tension reducing temperature is 850-870° C., then cooled to 800-820° C. to terminate the rolling to obtain a rough tube; S 3 : The capillary tube is pickled with a 10-20% sulfuric acid aqueous solution at a temperature of 35-40°C for 15-30 minutes, and then washed with water for 3-5 minutes. After washing with water, it is cold drawn at a temperature of 1000-1050°C, sized at a temperature of 580-610°C, and then straightened at a temperature of 300-350°C; S 4 : The straightened steel pipe is heated at 820-850°C, then kept warm for 1.5-2h, then quenched with water for 0.5-1h, then tempered at 600-630°C, kept warm for 1-2h, and then straightened at 400-450°C to obtain a steel pipe blank; S 5 :S 4 The obtained steel tube billet is surface treated with a surface treatment liquid for 20 to 30 minutes, then washed with water for 1 to 2 minutes, and then passivated with a passivation liquid for 30 to 40 minutes to obtain a finished seamless steel tube.
4. A processing technology for a seamless steel pipe according to claim 3, Features: The surface treatment liquid is a mixed aqueous solution of phosphoric acid, nitric acid, polyoxyethylene alkylphenol ether and sodium metasilicate.
5. A processing technology for a seamless steel pipe according to claim 4, Features: The surface treatment liquid comprises the following components by weight percentage: 30-40% phosphoric acid, 5-7% nitric acid, 0.2-0.4% polyoxyethylene alkylphenol ether, 1.5-2.5% sodium metasilicate, and the balance is water.
6. A processing technology for a seamless steel pipe according to claim 3, Features: The preparation method of the passivation solution is: A 1 : Add 3-5 parts of potassium fluorozirconate and 1-2 parts of potassium permanganate by weight to 20 parts of water at the same time, stirring while adding until all are dissolved; A 2 : By weight, under stirring, add A 1 Add 0.3-0.5 parts of isopropanolamine and 0.5-0.7 parts of sodium silicate to the obtained solution, stir for 0.5-1h, heat to 60-65°C, and stir thoroughly; A 3 : By weight, to A 2 Slowly drop 15 to 20 parts of a 30% potassium fluorozirconate aqueous solution into the solution obtained, the dropping time is 10 to 15 minutes, heat to 80 to 85°C, stir and react for 1 to 2 hours, add 8 to 12 parts of a modified acrylic resin, stir and react for 20 to 30 minutes; A 4 : By weight, to A 3 Add 1-2 parts of hydrophobic nano-silicon dioxide and 4-6 parts of a linker to the solution after the reaction, stir well to obtain a passivation concentrated solution; A 5 : The passivation concentrated solution is diluted with water to a mass concentration of 6-8% to obtain the passivation solution.
7. A processing technology for a seamless steel pipe according to claim 6, Features: The preparation method of the modified acrylic resin is: B 1 : Dissolve 0.05-0.15 parts of ammonium persulfate in 8-10 parts of deionized water to obtain an initiator solution; B 2 : By weight, 80 parts of methyl methacrylate monomer, 15-25 parts of polyethylene glycol diacrylate monomer, 1-3 parts of diacetone acrylamide and 3-4 parts of methacrylic acid were mixed and ground for 5-10 minutes, and B was added. 1 Half of the obtained initiator solution and 20-30 parts of ethanol are ground for 5-8 minutes to obtain a prepolymer; B 3 ; Add 80 to 100 parts by weight of deionized water and B to the reactor 2 The obtained prepolymer is heated to 85-95° C., and the other half of the initiator solution is slowly added dropwise for 5-10 minutes. After the addition is completed, it is kept warm for 20-30 minutes, and the pH is adjusted to 8-9 with an ammonia solution, and stirred for 5-10 minutes to obtain a modified acrylic resin.
8. A process for processing a seamless steel pipe according to claim 6, Features: The preparation method of the hydrophobic nano-silica is as follows: by weight, 10 parts of nano-silica and 0.5-0.7 parts of trifluoropropylmethyldiethoxysilane are uniformly mixed, and then added into 25-35 parts of ethanol solution with a mass fraction of 5% octadecylamine to prepare a suspension, the suspension is continuously stirred for 0.5-1h, and then dried in an oven at 60-70°C to prepare the hydrophobic nano-silica.
9. A process for processing a seamless steel pipe according to claim 6, Features: The preparation method of the connecting agent is: C 1 : Add 6 to 10 parts of sodium hydroxide by weight to 50 parts of 70 to 80% ethanol solution, stir until completely dissolved, then add 0.5 to 1 part of sodium lignin sulfonate and 0.4 to 0.6 parts of hydroxylated carbon nanotubes, stir for 10 to 20 minutes, and obtain a mixed solution; C 2 : Add 8 to 12 parts of aniline methyl trimethoxy silane and 3 to 4 parts of isooctyl alcohol polyoxyethylene ether to the mixed solution by weight, react for 2 to 3 hours, seal and degas, and obtain a linker.
Citation Information
Patent Citations
Novel seamless steel pipe and preparation technology thereof