Hot-based zinc-aluminum-magnesium plating product and method for controlling zinc flow line defect of hot-based zinc-aluminum-magnesium plating product

By precisely controlling the hot-dip galvanizing process and cooling method, combined with a nitrogen mixing system, the problem of zinc flow marks in hot-dip zinc-aluminum-magnesium products was solved, achieving high-quality surfaces and excellent corrosion resistance.

CN118880209AActive Publication Date: 2024-11-01МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410845227.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-01
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing technologies cannot effectively control zinc flow defects in thick hot-dip galvanized aluminum-magnesium products, which affect the surface quality and corrosion resistance of the products.

Method used

By precisely controlling the hot-dip galvanizing process parameters and combining mobile and fixed cooling methods, the post-plating cooling rate is controlled. A self-developed nitrogen mixing system is used to improve the air knife cooling capacity, avoiding remelting and agitation after the coating solidifies.

Benefits of technology

It effectively avoids zinc flow defects, improves product surface quality, meets the FB and FC surface grade requirements in GB2518, and reduces the surface defect rate to less than 15%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880209A_ABST
    Figure CN118880209A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hot dipping, and particularly relates to a hot-based zinc-aluminum-magnesium plating product and a method for controlling the hot-based zinc-aluminum-magnesium plating product to generate zinc flow line defects. Comprising the steps that a steel plate base material to be galvanized with a zinc-aluminum-magnesium coating is immersed in a zinc pot and subjected to hot dipping in a plating solution, and the temperature of the steel plate base material immersed in the zinc pot is related to the temperature of the plating solution and the width and thickness of the cross section of the steel plate base material; the hot-dipped steel plate is subjected to air knife blowing and scraping treatment; the steel plate with the molten coating is cooled through an after-plating cooling section, the hot-based zinc-aluminum-magnesium plating product is obtained, the after-plating cooling section comprises a fixed air cooling device and a movable air cooling device, the steel plate with the molten coating sequentially passes through the movable air cooling device and the fixed air cooling device, and the hot-based zinc-aluminum-magnesium plating product is obtained. And the cooling rate of the movable air cooling device is smaller than that of the fixed air cooling device. When the method disclosed by the invention is used for producing the hot-based zinc-aluminum-magnesium-plated product with the thick coating, the zinc flow line defect of the hot-based zinc-aluminum-magnesium-plated product with the thick coating can be effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-dip plating, and in particular relates to a hot-base galvanized aluminum-magnesium product and a method for controlling the generation of zinc flow defects therein. Background Art

[0002] Hot-dip galvanized aluminum-magnesium products are alloy-plated products obtained by adding appropriate Al, Mg and other trace alloy elements to the plating solution on the basis of traditional hot-dip galvanized products. Hot-based galvanized aluminum-magnesium products are directly coated with hot-rolled plates after pickling. Compared with traditional cold-based plating products, they can produce thicker and heavier coated products. Due to the reduction of the cold rolling process and the adjustment of the plating solution composition system, hot-based galvanized aluminum-magnesium products have a shorter production process, lower cost, stronger corrosion resistance, and obvious advantages in green energy saving and environmental protection. They are gradually replacing the higher-priced cold-rolled galvanized products of the same specifications, and are widely used in photovoltaic manufacturing, highway guardrails, construction industry, warehousing and other fields. Thick-coated hot-based galvanized aluminum-magnesium products often refer to products with a coating weight of approximately 275 to 350 g / m 2 , steel plate with a thickness specification of approximately 3.0 to 6.0 mm.

[0003] In the process of producing thick-coated hot-dip galvanized aluminum-magnesium products with existing technology, the air knife pressure is relatively small, the cooling capacity of the strip is insufficient, and the thick material carries more core heat energy. The incompletely solidified coating flows downward under the action of gravity, and surface quality defects such as zinc flow lines are very likely to occur. This defect will cause an obvious thickness difference in the coating thickness along the longitudinal direction of the strip surface, the strip surface is uneven, and the protruding parts of the surface feel tactile when touched by hand, which not only affects the appearance of the product, but also significantly reduces the corrosion resistance of the coating, greatly limiting its application areas.

[0004] Chinese patent CN103966537B discloses a method for controlling zinc flow lines of thick material and thick coating hot-dip galvanized products. The method controls the temperature of the spraying medium within the range of 0 to 10°C by installing an air conditioner in the fan room, thereby improving the cooling capacity of the spraying medium on the strip steel. At the same time, the distance between the air knife lip and the liquid surface is optimized to be 600 to 1000 mm, the distance between the air knife lip and the strip steel is 15 to 30 mm, and the air knife pressure is within the range of 100 to 300 mbar, so as to achieve the purpose of controlling zinc flow line defects. However, due to the different types of coating media and the difference in the solidification temperatures of pure zinc and zinc-aluminum-magnesium plating solutions, the method is not suitable for the product of the present invention. Chinese patent CN111534774A discloses a method for reducing the zinc flow ripple defect of hot-dip galvanizing. The method adjusts the running speed of the strip to 65-95m / min, and adopts air and nitrogen double purging mode according to different annealing temperatures to achieve the purpose of controlling the zinc flow defect. The method lacks the parameter adjustment of key processes such as air knife purging and post-plating cooling, and cannot effectively control the zinc flow defect of thick-coated hot-dip galvanized aluminum-magnesium products. Chinese patent CN112899600A discloses a galvanizing method for high-strength hot-dip galvanized strip with ultra-thick zinc layer. The method optimizes the hot-dip galvanizing furnace control unit, zinc pot control unit, zinc layer control unit, and cooling control unit to obtain high-strength hot-dip galvanized strip with excellent performance and good surface quality. However, the method can only solve the hot-dip galvanized products with a thickness of 2.5-3.0mm, and cannot effectively control the zinc flow defects of hot-dip galvanized aluminum-magnesium products with thicker specifications. Summary of the invention

[0005] The purpose of the present invention is to address the insufficiency of the existing technology in effectively controlling the zinc flow defects of hot-dip galvanized aluminum-magnesium products with thicker specifications, thereby proposing a hot-dip galvanized aluminum-magnesium product and a method for controlling the generation of zinc flow defects. The method of the present invention firstly reduces the core heat carried inside the steel plate by accurately adjusting the hot-dip plating process parameters, prevents the plating solution from melting back after solidification, and avoids the generation of zinc flow defects. Finally, in the cooling process after plating, a combination of movable cooling and fixed cooling is adopted, and the cooling rates of movable cooling and fixed cooling are controlled from small to large, which can effectively reduce the stirring effect of airflow on the incompletely solidified coating and avoid the occurrence of zinc flow defects. When the method of the present invention is used to produce thick-coated hot-dip galvanized aluminum-magnesium products, the occurrence of zinc flow defects of thick-coated hot-dip galvanized aluminum-magnesium products can be effectively avoided, and the surface quality of the product is improved to meet the surface grade requirements of FB (higher-level finishing surface) and FC (high-level finishing surface) in GB2518, and the proportion of surface defects is reduced to less than 15%.

[0006] The first aspect of the present invention provides a method for controlling zinc flow defects in hot-dip galvanized aluminum-magnesium products, the method comprising the following steps:

[0007] S1, immersing the steel plate substrate to be coated with a zinc-aluminum-magnesium coating into a zinc pot for hot-dip coating in a plating solution containing zinc, aluminum and magnesium elements to obtain a hot-dip coated steel plate;

[0008] S2, subjecting the hot-dip plated steel sheet to an air knife scraping treatment to obtain a molten-coated steel sheet;

[0009] S3, cooling the molten-coated steel sheet through a post-coating cooling section to obtain a hot-dip galvanized aluminum-magnesium product, wherein the post-coating cooling section includes a fixed air cooling device and a movable air cooling device, the molten-coated steel sheet passes through the movable air cooling device and the fixed air cooling device in sequence, and the cooling rate of the movable air cooling device is lower than the cooling rate of the fixed air cooling device;

[0010] In step S1, the temperature of the steel plate substrate to be coated with zinc-aluminum-magnesium coating and immersed in the zinc pot is as follows:

[0011] t1=T-2.2*(w*h)*10 -3 ;

[0012] Among them, t1 is the temperature of the steel plate substrate to be coated with zinc, aluminum and magnesium when immersed in the zinc pot, T is the plating solution temperature, w is the cross-sectional width of the steel plate substrate to be coated with zinc, aluminum and magnesium, and h is the cross-sectional thickness of the steel plate substrate to be coated with zinc, aluminum and magnesium.

[0013] Preferably, in step S1, the plating solution temperature is 410-420°C; in the plating solution, the Al content is 1.2-3wt%, the Mg content is 1.0-1.5wt%, the Sb content is 0.07-0.075wt%, and the rest is Zn, and the ratio of Al content to Mg content is 1.2-2:1.

[0014] More preferably, the cross-sectional width of the steel plate substrate to be coated with the zinc-aluminum-magnesium coating is 900-1450 mm, and the cross-sectional thickness of the steel plate substrate to be coated with the zinc-aluminum-magnesium coating is 3.0-6.0 mm.

[0015] Preferably, in step S2, the conditions for the air knife blowing treatment include: the blowing medium is nitrogen, the temperature of the blowing medium is -10 to 0°C, the blowing angle is -0.8 to -0.9°, the height of the air knife lip from the liquid level is 180 to 220 mm, the distance between the air knife lip and the strip is 10 to 20 mm, and the air knife pressure is 100 to 120 mbar.

[0016] Preferably, in step S3, the post-plating cooling section includes three fixed air-cooling devices and one movable air-cooling device, and the molten-coated steel plate passes through the movable air-cooling device, the first fixed air-cooling device, the second fixed air-cooling device and the third fixed air-cooling device in sequence; the cooling rate of the movable air-cooling device is 10-15°C / s, the cooling rate of the first fixed air-cooling device is 15-18°C / s, the cooling rate of the second fixed air-cooling device is 18-20°C / s, and the cooling rate of the third fixed air-cooling device is >25°C / s; the cooling rate of the movable air-cooling device is < the cooling rate of the first fixed air-cooling device < the cooling rate of the second fixed air-cooling device < the cooling rate of the third fixed air-cooling device.

[0017] More preferably, the movable air cooling device is installed at a height of 5 to 10 m from the plating liquid surface, the strip temperature is 315 to 335° C. after exiting the movable air cooling device, and the strip temperature is <205° C. when reaching the tower top roller.

[0018] Preferably, in step S1, the strip steel tension in the zinc pot section is controlled to be about 30-50 KN, and the running speed of the steel plate substrate to be coated with zinc-aluminum-magnesium coating is 40-60 m / min.

[0019] Preferably, in step S2, the blowing medium for the hot-dip plated steel plate to be subjected to air knife blowing and scraping treatment is nitrogen, which is provided by a nitrogen mixing system, and the nitrogen mixing system comprises a liquid nitrogen tank, a flow control valve, a temperature detector, a first delivery pipe, a second delivery pipe, a third delivery pipe, a fan and a mixing tank; the input end of the first delivery pipe is connected to the liquid nitrogen outlet of the liquid nitrogen tank, the output end of the first delivery pipe is connected to the mixing tank, and the first delivery pipe is provided with a flow control valve and a temperature detector in sequence along the flow direction of the liquid nitrogen; the second delivery pipe delivers normal temperature nitrogen to the mixing tank; the fan is installed inside the mixing tank, and is used to mix the liquid nitrogen and normal temperature nitrogen input into the mixing tank to achieve the temperature and pressure required for the blowing medium; the mixing tank is connected to the third delivery pipe, and is used to provide a gas source for the air knife with the blowing medium obtained by mixing liquid nitrogen and normal temperature nitrogen, and the third delivery pipe is provided with a temperature detector and a flow control valve in sequence along the flow direction of the blowing medium.

[0020] The second aspect of the present invention provides a hot-dip galvanized aluminum-magnesium product prepared by the method described above.

[0021] Preferably, the coating mass of the hot-dip galvanized aluminum-magnesium product is 275-350 g / m 2 , the coating thickness is 3.0~6.0mm.

[0022] The hot-dip galvanized aluminum-magnesium product and the method for controlling the generation of zinc flow defects therein described in the present invention have at least the following beneficial effects:

[0023] (1) In the present invention, firstly, the temperature of the substrate entering the pot in the hot-dip plating process is precisely controlled to reduce the core heat carried by the steel plate, prevent the plating solution from melting again after solidification, and avoid the generation of zinc flow defects. Finally, in the post-plating cooling process, a combination of movable cooling and fixed cooling is adopted, and the cooling rates of movable cooling and fixed cooling are controlled from small to large. This can effectively reduce the stirring effect of the airflow on the incompletely solidified coating, avoid the occurrence of zinc flow defects, improve the surface quality of the product, meet the FB and FC surface grade requirements in GB2518, and reduce the surface defect ratio to less than 15%;

[0024] (2) Under the preferred conditions, by controlling the temperature of the plating solution and the content and proportion of different components in the plating solution, it is possible to ensure that the steel plate has excellent corrosion resistance, increase the viscosity of the plating solution, reduce the fluidity of the plating solution, thereby reducing the generation of scum and zinc flow defects, and improving the surface quality of the coating; at the same time, during the air knife scraping process, by keeping the air knife low pressure and the air knife height and angle within a certain range, the thick coating (275-350g / m 2 ), specifications (3.0mm ~ 6.0mm) of hot-dip galvanized products, and improved the surface quality of the products, meeting the FC surface grade requirements in GB2518, and the proportion of surface defects is reduced to less than 3%. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A nitrogen mixer system is provided for the blowing medium used in the air knife blowing process of the present invention.

[0026] Reference numerals

[0027] 1. Liquid nitrogen tank; 2. Flow control valve; 3. Temperature detector; 4. First delivery pipe; 5. Second delivery pipe; 6. Third delivery pipe; 7. Fan; 8. Mixing tank. DETAILED DESCRIPTION

[0028] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0029] The first aspect of the present invention provides a method for controlling zinc flow defects in a thick-coated hot-dip galvanized aluminum-magnesium product, the method comprising the following steps:

[0030] S1, immersing the steel plate substrate to be coated with a zinc-aluminum-magnesium coating into a zinc pot for hot-dip coating in a plating solution containing zinc, aluminum and magnesium elements to obtain a hot-dip coated steel plate;

[0031] S2, subjecting the hot-dip plated steel sheet to an air knife scraping treatment to obtain a molten-coated steel sheet;

[0032] S3, cooling the molten-coated steel sheet through a post-coating cooling section to obtain a hot-dip galvanized aluminum-magnesium product, wherein the post-coating cooling section includes a fixed air cooling device and a movable air cooling device, the molten-coated steel sheet passes through the movable air cooling device and the fixed air cooling device in sequence, and the cooling rate of the movable air cooling device is lower than the cooling rate of the fixed air cooling device;

[0033] In step S1, the temperature of the steel plate substrate to be coated with zinc-aluminum-magnesium coating and immersed in the zinc pot is as follows:

[0034] t1=T-2.2*(w*h)*10 -3 ;

[0035] Among them, t1 is the temperature of the steel plate substrate to be coated with zinc, aluminum and magnesium when immersed in the zinc pot, T is the plating solution temperature, w is the cross-sectional width of the steel plate substrate to be coated with zinc, aluminum and magnesium, and h is the cross-sectional thickness of the steel plate substrate to be coated with zinc, aluminum and magnesium.

[0036] In a specific embodiment of the method of the present invention, the steel plate substrate to be coated with a zinc-aluminum-magnesium coating is a substrate obtained by degreasing, rinsing, drying and continuous annealing.

[0037] In a preferred embodiment of the method of the present invention, the cross-sectional width of the steel sheet substrate to be coated with the zinc-aluminum-magnesium coating is 900-1450 mm, for example, 900 mm, 1100 mm, 1250 mm, 1300 mm or 1450 mm; the cross-sectional thickness of the steel sheet substrate to be coated with the zinc-aluminum-magnesium coating is 3.0-6.0 mm, for example, 3.0 mm, 4.0 mm, 5.0 mm or 6.0 mm. In a more preferred case, the cross-sectional width of the steel sheet substrate to be coated with the zinc-aluminum-magnesium coating is 900-1450 mm, and the cross-sectional thickness of the steel sheet substrate to be coated with the zinc-aluminum-magnesium coating is 4.0-5.0 mm.

[0038] In a specific embodiment of the method of the present invention, in order to reduce the core heat carried inside the steel plate and prevent the plating solution from melting back after solidification, thereby generating zinc flow defects, therefore, in step S1, the temperature of the plating solution is controlled to be 410-420° C., for example, 410° C., 415° C., 418° C. or 420° C. In a preferred embodiment, the plating solution temperature is 415-418° C.

[0039] In a specific embodiment of the method of the present invention, by controlling the content and proportion of different components in the plating solution, it is possible to ensure that the steel plate has excellent corrosion resistance, improve the viscosity of the plating solution, reduce the fluidity of the plating solution, thereby reducing the generation of scum and zinc flow defects, and improving the surface quality of the coating. Specifically, in step S1, in the plating solution, the Al content is 1.2-3wt%, for example, 1.2wt%, 1.4wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2.0wt%, 2.2wt%, 2.7wt% or 3wt%; the Mg content is 1.2-3wt%, for example, 1.2wt%, 1.4wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2.0wt%, 2.2wt%, 2.7wt% or 3wt%; The content of Sb is 0.07-0.075wt%, for example, it can be 0.07wt%, 0.072wt%, 0.074wt% or 0.075wt%; the rest is Zn; and the ratio of Al content to Mg content is 1.2-2:1, for example, it can be 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1 or 2:1.

[0040] In a preferred embodiment, in the plating solution, the Al content is 1.4-2.2wt%, the Mg content is 1.1-1.4wt%, the Sb content is 0.075wt%, and the rest is Zn; and the ratio of the Al content to the Mg content is 1.3-1.6:1.

[0041] In a specific implementation manner of the method of the present invention, tension control and operating speed can effectively avoid jittering of the steel plate during operation, and improve the uniformity and stability of the coating. In step S1, the tension of the zinc pot section strip is controlled to be about 30-50KN, specifically, for example, it can be 30KN, 35KN, 38KN, 40KN, 42KN, 43KN, 45KN, 48KN or 50KN; the operating speed of the steel plate substrate to be galvanized, aluminum-magnesium coated is 40-60m / min, specifically, for example, it can be 40m / min, 45m / min, 52m / min or 60m / min.

[0042] Since the formation of zinc flow lines is closely related to the air knife pressure and the distance between the air knife and the steel plate, the close distance and low pressure method and a certain air knife height and angle are used as much as possible in the strip production process, which can effectively avoid the occurrence of zinc flow line defects in thick-coated hot-dip galvanized products. In a specific embodiment of the method described in the present invention, in step S2, the conditions for the air knife scraping treatment include: the blowing medium is nitrogen, and the temperature of the blowing medium is -10 to 0°C, specifically, for example, -10°C, -8°C, -5°C or 0°C; the blowing angle is -0.8 to -0.9°, specifically, for example, -0.8° or -0.9°; the height of the air knife lip from the plating solution level is 180 to 220 mm, specifically, for example, 180 mm, 1 90mm, 200mm or 220mm; the vertical distance between the air knife lip and the strip surface is 10-20mm, specifically, for example, it can be 10mm, 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm, 18mm, 19mm or 20mm; the air knife pressure is 100-120mbar, specifically, for example, it can be 100mbar, 110mbar, 115mbar or 120mbar. In this article, the blowing angle refers to the air knife nozzle angle.

[0043] In a preferred case, in step S2, the conditions for the air knife scraping treatment include: the blowing medium is nitrogen, the temperature of the blowing medium is -5 to -8°C, the blowing angle is -0.8 to -0.9°, the height of the air knife lip from the plating solution level is 190 to 200 mm, the vertical distance between the air knife lip and the surface of the strip is 13 to 17 mm, and the air knife pressure is 110 to 115 mbar.

[0044] In the present invention, the temperature of the sprayed medium nitrogen is achieved by cooling the nitrogen mixing system independently developed by the manufacturer. Figure 1 As shown, the system includes a liquid nitrogen tank 1, a flow control valve 2, a temperature detector 3, a first delivery pipe 4, a second delivery pipe 5, a third delivery pipe 6, a fan 7 and a mixing tank 8; the input end of the first delivery pipe 4 is connected to the liquid nitrogen outlet of the liquid nitrogen tank 1, and the output end of the first delivery pipe 4 is connected to the mixing tank 8, and the flow control valve 2 and the temperature detector 3 are sequentially arranged on the first delivery pipe 4 along the flow direction of the liquid nitrogen; the second delivery pipe 5 delivers the normal temperature nitrogen to the mixing tank 8; the fan 7 is installed inside the mixing tank 8, and is used to mix the liquid nitrogen and the normal temperature nitrogen input into the mixing tank 8 to achieve the temperature and pressure required for the spraying medium; the mixing tank 8 is connected to the third delivery pipe, and is used to provide an air source for the air knife with the spraying medium after the liquid nitrogen and the normal temperature nitrogen are mixed, and the temperature detector 3 and the flow control valve 2 are sequentially arranged on the third delivery pipe along the flow direction of the spraying medium.

[0045] Specifically, the first delivery pipe 4 is a copper alloy delivery pipe, the second delivery pipe is a room temperature nitrogen delivery pipe, the third delivery pipe is a mixed gas delivery pipe, and the fan 7 is a stirring fan.

[0046] In the specific operation process, the liquid nitrogen in the liquid nitrogen tank 1 is extracted into the interior of the mixing tank 8 through the first delivery pipe 4, and at the same time, nitrogen at room temperature is introduced into the tank body, and after being fully mixed by the fan 7, the gas source is finally provided for the air knife through the third delivery pipe 6; the pressure and temperature of the gas source flow can be instantly controlled and adjusted by the flow control valve 2 and the temperature detector 3 in the mixer system.

[0047] By controlling the cooling rate of mobile and fixed cooling fans and adopting a progressive cooling mode with cooling rate increasing from small to large, the stirring effect of airflow on the incompletely solidified coating can be effectively reduced, avoiding the occurrence of zinc flow defects, and obtaining a coating with dense phase structure and good corrosion resistance.

[0048] In a specific embodiment of the method of the present invention, in step S3, the post-plating cooling section includes three fixed air cooling devices and one movable air cooling device, and the molten-coated steel plate passes through the movable air cooling device, the first fixed air cooling device, the second fixed air cooling device and the third fixed air cooling device in sequence; the cooling rate of the movable air cooling device is 10 to 15°C / s, specifically, for example, it can be 10°C / s, 12°C / s, 13°C / s or 15°C / s; the cooling rate of the first fixed air cooling device is 15 to 18°C / s, specifically, for example, it can be The cooling rate of the second fixed air-cooling device is 18-20°C / s, specifically, for example, it can be 18°C / s, 19°C / s or 20°C / s; the cooling rate of the third fixed air-cooling device is greater than 25°C / s, specifically, for example, it can be 25°C / s, 26°C / s, 27°C / s or 28°C / s; and the cooling rate of the movable air-cooling device is less than the cooling rate of the first fixed air-cooling device, less than the cooling rate of the second fixed air-cooling device, and less than the cooling rate of the third fixed air-cooling device.

[0049] In a preferred embodiment of the method of the present invention, in step S3, the cooling rate of the movable air cooling device is 12-13°C / s, the cooling rate of the first fixed air cooling device is 16-17°C / s, the cooling rate of the second fixed air cooling device is 19°C / s, and the cooling rate of the third fixed air cooling device is 26-27°C / s.

[0050] The temperature of the plate after exiting the mobile fast cooling section is controlled to be lower than 335°C, mainly because under the composition system of the plating solution, according to the phase diagram, a eutectic reaction will occur before the coating structure is completely solidified, and finally the process of transformation from liquid phase to ternary eutectic phase is completed at a temperature of 335.8°C. In a specific embodiment, the height of the movable air cooling device is 5 to 10m above the plating liquid surface, and the temperature of the strip steel plate after exiting the movable air cooling device is 315 to 335°C, specifically, for example, it can be 315°C, 325°C, 330°C or 335°C; when reaching the tower top roller, the temperature of the strip steel plate is less than 205°C, specifically, for example, it can be 195°C, 198°C, 202°C or 205°C.

[0051] The second aspect of the present invention provides a hot-dip galvanized aluminum-magnesium product prepared by the method described above.

[0052] In a specific embodiment of the hot-base galvanized aluminum-magnesium product of the present invention, the coating mass of the hot-base galvanized aluminum-magnesium product is 275-350 g / m 2 Specifically, for example, it can be 275g / m 2 , 300g / m 2 or 350g / m 2 ; The coating thickness is 3.0 to 6.0 mm, specifically, for example, it can be 3.0 mm, 4.0 mm, 5.0 mm or 6.0 mm.

[0053] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0054] The preparation process of the steel plate substrate to be plated with zinc-aluminum-magnesium coating is as follows: the substrate is obtained through degreasing, rinsing, drying and continuous annealing.

[0055] A method for controlling zinc flow defects in hot-dip galvanized aluminum-magnesium products, the method comprising the following steps:

[0056] S1, immersing the steel plate substrate to be coated with a zinc-aluminum-magnesium coating into a zinc pot for hot-dip coating in a plating solution containing zinc, aluminum and magnesium elements to obtain a hot-dip coated steel plate;

[0057] S2, subjecting the hot-dip plated steel sheet to an air knife scraping treatment to obtain a molten-coated steel sheet;

[0058] S3. The molten-coated steel sheet is cooled in a post-coating cooling section to obtain a hot-dip galvanized aluminum-magnesium product, wherein the post-coating cooling section includes three fixed air cooling devices and one movable air cooling device, and the molten-coated steel sheet is sequentially cooled by a first fixed air cooling device, a second fixed air cooling device and a third fixed air cooling device.

[0059] Examples 1 to 14 use the above method to control the generation of zinc flow defects in hot-dip galvanized aluminum-magnesium products. The hot-dip coating process parameters are shown in Table 1.

[0060] Table 1 Hot dip coating process parameters

[0061]

[0062]

[0063] Examples 1 to 14 use the above method to control the generation of zinc flow defects in hot-dip galvanized aluminum-magnesium products. The key parameters of the air knife scraping treatment are shown in Table 2.

[0064] Table 2 Key parameters of air knife scraping treatment

[0065]

[0066]

[0067] Examples 1 to 14 use the above method to control the generation of zinc flow defects in hot-dip galvanized aluminum-magnesium products. The key parameters of the cooling process are shown in Table 3.

[0068] Table 3 Key parameters of cooling treatment

[0069]

[0070] Comparative Example 1: The method of Example 1 is followed, except that the temperature of entering the pot in the hot dip plating process parameters is adjusted. In this comparative example, the temperature of entering the pot is 405°C.

[0071] Comparative Example 2: The method of Example 1 is followed, except that during the cooling process, the cooling rate of the movable air cooling device is 15°C / s.

[0072] The surface quality grade and effect of the hot-dip galvanized aluminum-magnesium products prepared in Examples 1 to 14 and Comparative Examples 1 to 2 were measured, and the results are shown in Table 4, wherein FA refers to an ordinary finished surface, FB refers to a higher-grade finished surface, and FC refers to a high-grade finished surface; the defect ratio is measured by dynamically detecting the defect type and length of the hot-dip galvanized aluminum-magnesium products using a surface detector, and the defect ratio = defective steel plate length / total steel plate length.

[0073] Table 4

[0074] Surface quality grade Defect ratio Example 1 FB 8% Example 2 FB 5% Example 3 FB 7% Example 4 FB 7% Example 5 FC 3% Example 6 FB 5% Example 7 FC 3% Example 8 FB 6% Example 9 FC 2% Example 10 FB 7% Embodiment 11 FB 6% Example 12 FB 7% Example 13 FB 10% Embodiment 14 FB 15% Comparative Example 1 FA 32% Comparative Example 2 FA 24%

[0075] According to the results in Table 4, it can be seen that by optimizing and adjusting the key manufacturing processes of hot-dip plating, air knife parameters, post-plating cooling and other key manufacturing processes of hot-dip plating products, and adopting the independently developed nitrogen mixer system to improve the cooling capacity of the spraying medium, the thick coating (275-350g / m 2 ), and the occurrence of zinc flow defects in hot-dip galvanized aluminum-magnesium products with specifications (3.0mm~6.0mm); at the same time, Examples 5, 7 and 9 improve the surface quality of the product by controlling the temperature of the plating solution and the content and proportion of different components in the plating solution, and by coordinating the low pressure of the air knife with the height and angle of the air knife within a certain range, meeting the FC surface grade requirements in GB2518, and reducing the proportion of surface defects to less than 3%.

[0076] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for controlling zinc flow defects in hot-dip galvanized aluminum-magnesium products. It is characterized in that The method comprises the following steps: S1, immersing the steel plate substrate to be coated with a zinc-aluminum-magnesium coating into a zinc pot and hot-dip coating in a plating solution containing zinc, aluminum and magnesium elements to obtain a hot-dip coated steel plate; S2, subjecting the hot-dip plated steel sheet to an air knife scraping treatment to obtain a molten-coated steel sheet; S3, cooling the molten-coated steel sheet through a post-coating cooling section to obtain a hot-dip galvanized aluminum-magnesium product, wherein the post-coating cooling section includes a fixed air cooling device and a movable air cooling device, the molten-coated steel sheet passes through the movable air cooling device and the fixed air cooling device in sequence, and the cooling rate of the movable air cooling device is lower than the cooling rate of the fixed air cooling device; In step S1, the temperature of the steel plate substrate to be coated with zinc-aluminum-magnesium coating and immersed in the zinc pot is as follows: t 1 =T-2.2*(w*h)*10 -3 ; Among them, t 1 is the temperature of the steel plate substrate to be coated with galvanized aluminum-magnesium coating when immersed in the zinc pot, T is the plating solution temperature, w is the cross-sectional width of the steel plate substrate to be coated with galvanized aluminum-magnesium coating, and h is the cross-sectional thickness of the steel plate substrate to be coated with galvanized aluminum-magnesium coating.

2. The method according to claim 1, It is characterized in that In step S1, the plating solution temperature is 410-420°C; in the plating solution, the Al content is 1.2-3wt%, the Mg content is 1.0-1.5wt%, the Sb content is 0.07-0.075wt%, and the rest is Zn, and the ratio of Al content to Mg content is 1.2-2:

1.

3. The method according to claim 2, It is characterized in that The cross-sectional width of the steel plate substrate to be coated with the zinc-aluminum-magnesium coating is 900-1450 mm, and the cross-sectional thickness of the steel plate substrate to be coated with the zinc-aluminum-magnesium coating is 3.0-6.0 mm.

4. The method according to claim 1, It is characterized in that In step S2, the conditions for the air knife scraping treatment include: the blowing medium is nitrogen, the temperature of the blowing medium is -10 to 0°C, the blowing angle is -0.8 to -0.9°, the air knife lip is 180 to 220 mm from the liquid level, the air knife lip is 10 to 20 mm from the strip, and the air knife pressure is 100 to 120 mbar.

5. The method according to claim 1, It is characterized in that In step S3, the post-plating cooling section includes three fixed air cooling devices and one movable air cooling device, and the molten-plated steel plate passes through the movable air cooling device, the first fixed air cooling device, the second fixed air cooling device and the third fixed air cooling device in sequence; The cooling rate of the movable air cooling device is 10-15°C / s, the cooling rate of the first fixed air cooling device is 15-18°C / s, the cooling rate of the second fixed air cooling device is 18-20°C / s, and the cooling rate of the third fixed air cooling device is greater than 25°C / s; The cooling rate of the movable air cooling device is less than the cooling rate of the first fixed air cooling device and less than the cooling rate of the second fixed air cooling device and less than the cooling rate of the third fixed air cooling device.

6. The method according to claim 5, It is characterized in that The movable air cooling device is installed at a height of 5 to 10 m from the plating liquid surface. The strip temperature is 315 to 335°C after leaving the movable air cooling device, and is <205°C when reaching the tower top roller.

7. The method according to claim 1, It is characterized in that In step S1, the strip steel tension in the zinc pot section is controlled to be about 30-50 KN, and the running speed of the steel plate substrate to be coated with zinc-aluminum-magnesium coating is 40-60 m / min.

8. The method according to claim 1, It is characterized in that In step S2, the blowing medium for the air knife blowing treatment of the hot-dip coated steel plate is nitrogen, and the nitrogen is provided by a nitrogen mixing system, and the nitrogen mixing system comprises a liquid nitrogen tank (1), a flow control valve (2), a temperature detector (3), a first delivery pipe (4), a second delivery pipe (5), a third delivery pipe (6), a fan (7) and a mixing tank (8); The input end of the first delivery pipe (4) is connected to the liquid nitrogen outlet of the liquid nitrogen tank (1), and the output end of the first delivery pipe (4) is connected to the mixing tank (8); a flow control valve (2) and a temperature detector (3) are sequentially arranged on the first delivery pipe (4) along the flow direction of the liquid nitrogen; the second delivery pipe (5) delivers normal temperature nitrogen to the mixing tank (8); The fan (7) is installed inside the mixing tank (8) and is used to mix the liquid nitrogen and the nitrogen at room temperature input into the mixing tank (8) to achieve the temperature and pressure required by the spraying medium; the mixing tank (8) is connected to the third delivery pipe and is used to provide an air source for the air knife with the spraying medium obtained by mixing the liquid nitrogen and the nitrogen at room temperature; the third delivery pipe is provided with a temperature detector (3) and a flow control valve (2) in sequence along the flow direction of the spraying medium.

9. A hot-dip galvanized aluminum-magnesium product prepared according to the method according to any one of claims 1 to 8.

10. The hot-dip galvanized aluminum-magnesium product according to claim 9, It is characterized in that The coating mass of the hot-dip galvanized aluminum-magnesium product is 275-350 g / m 2 , the coating thickness is 3.0~6.0mm.

Citation Information

Patent Citations

  • A method for controlling zinc flow marks of thick material and thick coating hot-dip galvanized products

    CN103966537B

  • Method for reducing hot galvanizing zinc flow ripple defects

    CN111534774A

  • Galvanizing method of super-thick zinc layer high-strength hot-galvanized strip steel

    CN112899600A

  • Method for producing high-surface-quality zinc-aluminum-magnesium coated steel strip / plate by using air knife

    CN113481455A

  • Production method for eliminating black spot defect on surface of thick-specification thick-plating-layer coated steel plate and thick-specification thick-plating-layer coated steel plate

    CN114107866A