Ta-Hf-C ceramic material and preparation method and application thereof

The preparation of Ta-Hf-C ceramic materials through multi-target DC magnetron sputtering technology has solved the problems of complex and high cost in the preparation of existing hafnium tantalum carbon-based ceramic materials, and achieved the high temperature, hardness and radiation performance of spacecraft protective coatings Demand, with wide application prospects and industrial production potential.

CN118880237APending Publication Date: 2024-11-01NAT INNOVATION INST OF DEFENSE TECH PLA ACAD OF MILITARY SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410992416.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing hafnium tantalum carbon-based ceramic materials are complex and costly, and it is difficult to meet the multiple requirements of spacecraft protective coatings for high temperature, hardness and radiation performance.

Method used

Ta-Hf-C ceramic materials are prepared by multi-target DC magnetron sputtering technology. By adjusting the target power, angle and distance, it avoids the complex preparation process of a single alloy target, and prepares a single-phase face-centered cubic crystal structure and low surface Ceramic films with roughness, high hardness and elastic modulus.

Benefits of technology

It realizes the controllable composition, uniformity and high performance of Ta-Hf-C ceramic materials, and is suitable for spacecraft protective coatings, with wide application prospects and industrial production potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880237A_ABST
    Figure CN118880237A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic materials, in particular to a Ta-Hf-C ceramic material and a preparation method and application thereof. The chemical formula of the Ta-Hf-C ceramic material is Taa Hf C < c >, wherein 3 < = a < = 4.5, 0.5 < = b < = 2, and a + b + c = 10. The Ta-Hf-C ceramic material is prepared by adopting multi-target direct current magnetron sputtering. The Ta-Hf-C ceramic material thin film provided by the invention has the surface roughness of 1.03 to 1.35 nm, the hardness of 21.34 to 25.23 GPa and the elasticity modulus of 270.1 to 286.6 GPa, has a wider application prospect, and can be applied to extreme service conditions. The Ta-Hf-C ceramic material disclosed by the invention is prepared by adopting a multi-target direct-current magnetron sputtering mode, and the obtained Ta-Hf-C ceramic material is controllable and uniform in component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic materials, and in particular to a Ta-Hf-C ceramic material and a preparation method and application thereof. Background Art

[0002] With the continuous development of aerospace technology, the operating temperatures of aero-engine components, surface structural materials of hypersonic vehicles, rocket engines, and spacecraft are getting higher and higher. For example, the ambient temperature faced by hypersonic vehicles can reach 1900 °C; in the field of deep space exploration, the solar probe needs to withstand a high temperature of up to 1400 °C at the perihelion. These application requirements put forward higher requirements on the high temperature protection performance of materials. At the same time, the protective coatings in spacecraft need to have high hardness to increase the specific stiffness of the material, which will help to resist the impact of micrometeorite particles or spacecraft fragments in space. In addition, the space environment is complex and severe, including various space charged particles, ultraviolet radiation, micrometeorites and various spacecraft fragments, which pose a challenge to the safe service of spacecraft systems and materials. For example, polymer-based composite materials widely used in spacecraft will produce permanent damage under the irradiation of charged particles, resulting in the degradation of the mechanical, optical and electrical properties of the material, thereby affecting the reliability of the spacecraft. Therefore. Spacecraft protective coatings need to have a high melting point, high temperature resistance, strong mechanical properties, and excellent radiation resistance.

[0003] Hafnium-tantalum-based ceramics mainly include three systems: HfC, TaC and Ta-Hf-C ternary ceramics. They are the type of materials with the highest melting points among currently known substances. Among ultra-high temperature ceramic materials, TaC and HfC are binary compounds of metallic tantalum and hafnium with carbon, which have metallic conductivity and face-centered cubic crystal structure. Among them, TaC and HfC have extremely high melting points, both of which are above 3800°C. Compared with pure HfC and TaC binary coatings, ternary Ta-Hf-C coatings can combine the advantages of HfC and TaC, and their hardness, elastic modulus and plastic deformation resistance (H 3 / E 2 ) were significantly increased by about 48%, 21% and 220% respectively. It can be seen that hafnium tantalum carbon-based ceramic materials have great potential in the future thermal protection field. The existing preparation methods of hafnium tantalum carbon-based ceramic materials are complex and costly. Summary of the invention

[0004] The present invention provides a Ta-Hf-C ceramic material and a preparation method and application thereof, so as to solve the above problems existing in the prior art.

[0005] According to a first aspect of the present invention, the present invention provides a Ta-Hf-C ceramic material having a chemical formula of Ta a Hf b Cc ; Among them, 3≤a≤4.5, 0.5≤b≤2 and a+b+c=10.

[0006] Furthermore, the Ta—Hf—C ceramic material satisfies at least one of the following characteristics (1)-(4): (1) The Ta-Hf-C ceramic material has a single-phase face-centered cubic crystal structure; (2) The surface roughness of the Ta-Hf-C ceramic material is 1.03-1.35 nm; (3) The hardness of the Ta-Hf-C ceramic material is 21.34~25.23 Gpa; (4) The elastic modulus of the Ta-Hf-C ceramic material is 270.1~286.6 GPa.

[0007] Ta-Hf-C ceramic materials that meet the above characteristics can be better applied to spacecraft protective coatings.

[0008] According to a second aspect of the present invention, the present invention also provides a method for preparing the above-mentioned Ta—Hf—C ceramic material, wherein the Ta—Hf—C ceramic material is prepared by multi-target DC magnetron sputtering.

[0009] The preparation method of the Ta-Hf-C ceramic material of the present invention adopts multi-target DC magnetron sputtering to prepare the material. The multi-target magnetron sputtering adopts multiple pure metal targets or binary alloy targets, which can effectively avoid the complicated preparation process of a single alloy target. Moreover, by changing the target power and the angle of the target relative to the substrate, a film with diversified components can be prepared, so that the film preparation becomes more flexible and is conducive to high-throughput screening of film composition and performance.

[0010] Further, the following steps are included: Fixing the substrate on the substrate stage; Place the Ta target and the Hf target on different DC target positions respectively, place the C target on the RF target position, and adjust the angle of the target relative to the center line perpendicular to the substrate stage and the vertical distance between the target and the substrate stage; Under inert gas, pre-sputtering the target material; Thin film sputtering is performed on the sputtering surface of the substrate to obtain the Ta-Hf-C ceramic material on the substrate.

[0011] In the above scheme, the preparation method of the Ta-Hf-C ceramic material of the present invention places the Ta target, Hf target and C target on different target positions respectively, avoiding the complicated preparation process of a single alloy target, placing the Ta target and Hf target on the DC target position, and placing the C target on the RF target position. By changing the target power, and the angle and distance of the target relative to the substrate stage, a film with diversified components can be prepared, making the film preparation more flexible, which is conducive to high-throughput screening of film composition and performance. The Ta-Hf-C ceramic material obtained by the preparation method of the present invention has controllable and uniform composition, low surface roughness, high hardness and good elastic modulus.

[0012] Furthermore, the sputtering power of the Ta target is 120-160 W; the sputtering power of the Hf target is 40-80 W; the sputtering power of the C target is 120-160 W; and the sputtering time is 0.5-1.5 h.

[0013] In the above scheme, by limiting the sputtering power of each target material within a reasonable range, it is beneficial to improve the sputtering effect of each target material and improve the sputtering efficiency. For the sputtering power, when it is lower than the required sputtering power, the target material is not easy to ignite, and when it is higher than the required sputtering power, it is easy to cause the equipment to overheat and affect the sputtering effect.

[0014] Furthermore, the substrate is a single crystal silicon wafer, the silicon wafer is P-type, and the crystal orientation is <100> .

[0015] In the above scheme, by appropriately selecting the specifications of the substrate, it is beneficial to the deposition of the target material, thereby preparing a uniform Ta-Hf-C ceramic material that meets the requirements.

[0016] Furthermore, the Ta target, the Hf target and the C target are all high-purity blocks with a purity greater than or equal to 99.95%, a diameter of 50-70 mm, and a thickness of 4-6 mm.

[0017] In the above scheme, by appropriately selecting the specifications of each target material, it is beneficial to improve the sputtering efficiency and the quality of the Ta-Hf-C ceramic material.

[0018] Furthermore, the angle of the target relative to the center line perpendicular to the substrate stage is 20~40°; and / or, the vertical distance between the Ta target, the Hf target and the C target and the substrate stage is 5~15 cm; and / or, the pre-sputtering time is 10~15 min.

[0019] In the above scheme, under the condition of the same other preparation parameters, the angle of the target relative to the center line perpendicular to the substrate stage will affect the deposition rate of the film. Too small or too large will affect the thickness of the film. When the target is 20-40°, the projected area of ​​the target relative to the substrate is relatively large, the deposition rate is relatively fast, and the efficiency is high. The vertical distance between the target and the substrate stage will also affect the deposition rate of the film. Too small or too large will affect the thickness of the film.

[0020] Furthermore, the sputtering is performed in a deposition chamber; preferably, the vacuum of the deposition chamber is 6×10 -3 ~8×10 -3 Pa, the gas pressure is 0.7~0.9 Pa; and / or, the inert gas includes one or more of argon, helium or nitrogen; preferably, the flow rate of the inert gas is 30~50 sccm, and the purity is greater than or equal to 99.999%.

[0021] In the above scheme, the sputtering effect can be improved by reasonably limiting the vacuum conditions, the type, flow rate and purity of the inert gas during the sputtering process.

[0022] Furthermore, before the substrate is fixed on the substrate stage, the substrate is pretreated; preferably, the pretreatment of the substrate comprises the following steps: ultrasonically cleaning the substrate in anhydrous ethanol, and then rinsing the substrate with water; drying the cleaned substrate with compressed nitrogen; preferably, the frequency of the ultrasonic cleaning is 60-80 Hz, and the time is 5-15 min. Preferably, the sputtering surface of the substrate is polished with a damping cloth before ultrasonic cleaning.

[0023] In the above scheme, by pre-treating the substrate, pollutants attached to the surface of the substrate can be removed, and the flatness of the substrate surface can be ensured, which is beneficial to the subsequent deposition of the target material.

[0024] According to the third aspect of the present invention, the present invention also provides an application of a Ta-Hf-C ceramic material, wherein the Ta-Hf-C ceramic material is the above-mentioned Ta-Hf-C ceramic material or the Ta-Hf-C ceramic material prepared by the above-mentioned preparation method; the Ta-Hf-C ceramic material is applied in a protective coating.

[0025] The Ta-Hf-C ceramic material film provided by the present invention has a surface roughness of 1.03-1.35 nm, a hardness of 21.34-25.23 GPa, and an elastic modulus of 270.1-286.6 GPa, has a broader application prospect, and can be applied to extreme service conditions.

[0026] The present invention discloses a method for preparing Ta-Hf-C ceramic material using multi-target DC magnetron sputtering technology, that is, using a method of co-sputtering of multiple targets, and the target materials are pure metal targets and graphite targets. The method can avoid complicated target material preparation processes, and ceramic films of various chemical compositions can be prepared by changing the target material power or the relative surface fraction of each element in a specific target material. The method has the characteristics of high deposition rate, wide material applicability, good repeatability, etc. Pure metal targets and graphite targets are used in the preparation process of the present invention, and the raw materials are simple and easy to obtain, which is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Attached Figure 1 The surface and cross-sectional SEM images of the Ta4HfC5 ceramic film in Example 1.

[0029] Attached Figure 2 This is the surface scanning EDS image of the elements of the Ta4HfC5 ceramic film in Example 1.

[0030] Attached Figure 3 This is the AFM image of the surface morphology of the Ta4HfC5 ceramic film in Example 1.

[0031] Attached Figure 4 This is the XRD diagram of the Ta4HfC5 ceramic film in Example 1.

[0032] Attached Figure 5 The surface and cross-sectional SEM images of the Ta3Hf2C5 ceramic film in Example 2.

[0033] Attached Figure 6 This is the surface scanning EDS image of the elements of the Ta3Hf2C5 ceramic film in Example 2.

[0034] Attached Figure 7 This is the AFM image of the surface morphology of the Ta3Hf2C5 ceramic film in Example 2.

[0035] Attached Figure 8 This is the XRD diagram of the Ta3Hf2C5 ceramic film in Example 2.

[0036] Attached Fig. 9 is Ta in Example 3 4.5 HkDJ 4.5 SEM images of the surface and cross-sectional morphology of ceramic films.

[0037] Attached Fig.10 is Ta in Example 3 4.5 HkDJ 4.5 Surface scanning EDS map of the elements of ceramic film.

[0038] Attached Fig.11 is Ta in Example 3 4.5 HkDJ 4.5 AFM image of the surface morphology of ceramic films.

[0039] Attached Fig.12 is Ta in Example 3 4.5 HkDJ 4.5 XRD patterns of ceramic films.

[0040] Attached Fig.13 is Ta2Hf in Comparative Example 1 2.5 C 5.5 SEM images of the surface and cross-sectional morphology of ceramic films.

[0041] Attached Fig.14 is Ta2Hf in Comparative Example 1 2.5 C 5.5 Surface scanning EDS map of the elements of ceramic film.

[0042] Attached Fig.15 is Ta2Hf in Comparative Example 1 2.5 C 5.5 AFM image of the surface morphology of ceramic films.

[0043] Attached Fig.16 is Ta2Hf in Comparative Example 1 2.5 C 5.5 XRD patterns of ceramic films. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] The beneficial effects of the present invention will be described below in conjunction with specific embodiments and comparative examples.

[0046] The raw materials used in the following examples can all be purchased commercially: 1. The high-purity Ar gas used in the present invention is purchased from Beijing Qianxi Jingcheng Gas Co., Ltd., with a purity greater than or equal to 99.999%

[0047] 2. The Ta, Hf and C target materials used in the thin film prepared by the present invention are all commercially available products with a purity greater than or equal to 99.95%, and the single crystal silicon wafer is a commercially available commodity.

[0048] 3. The high vacuum magnetron sputtering coating equipment used for preparing the thin film of the present invention is a multi-target high vacuum magnetron sputtering coating machine produced by Shenyang Oute Vacuum Technology Co., Ltd.; the mechanical pump and molecular pump are both supporting equipment of the high vacuum magnetron sputtering coating equipment produced by the same company.

[0049] Example 1

[0050] This embodiment provides a Ta4HfC5 ceramic film, and the preparation method thereof is as follows: The P type, crystal direction is <100> 1. The single crystal Si wafer that had been previously treated with damping polishing was ultrasonically cleaned with anhydrous ethanol at a frequency of 60-80 Hz for 10 minutes to remove pollutants attached to the surface of the substrate. After ultrasonic cleaning, the substrate was rinsed with deionized water and then blown dry with compressed nitrogen to make its surface clean and free of water stains. The single crystal silicon wafer was fixed on a substrate disk, and the substrate disk was fixed on the substrate stage of the deposition chamber of the high vacuum magnetron sputtering coating equipment, and the rotating substrate baffle was adjusted to a position that completely covered the substrate.

[0051] High-purity metal targets Ta and Hf were placed on two different DC target positions in the deposition chamber, and graphite C target was placed on the RF target position. The angles of the targets relative to the center line perpendicular to the substrate stage were adjusted to 30°, and the vertical distance between the targets and the substrate stage was adjusted to 10 cm. The deposition chamber was first evacuated to less than 7.0 Pa using a mechanical pump, and then evacuated to less than 8.0×10 -3 Pa; high-purity Ar gas with a purity greater than or equal to 99.999% at a flow rate of 40 sccm is introduced into the deposition chamber, the working gas pressure is adjusted to 0.7 Pa, the power of the Ta target is set to 140 W, the power of the Hf target is set to 60 W, and the power of the C target is set to 130 W, and the targets are pre-sputtered for 10 min to remove impurities on the target surfaces; after the pre-sputtering is completed, the substrate rotation rate is set to 15 r / min, the substrate baffle is opened, and formal sputtering for 1 h is started; after the sputtering is completed, the DC constant current power supply is turned off, the Ar gas source is turned off, the substrate rotation is turned off, the film is cooled to room temperature in a vacuum state, and then taken out to obtain the Ta4HfC5 ceramic film on a single crystal silicon wafer.

[0052] The chemical composition of the multi-principal alloy film was analyzed using an Oxford X-act energy dispersive spectrometer (EDS, installed on a scanning electron microscope). The surface and cross-sectional morphology SEM images and element surface scanning EDS spectra of the multi-principal alloy film are shown in the attached figure. Figure 1 and 2As shown: According to the quantitative calculation results of the software, the composition of the alloy film is Ta4HfC5.

[0053] The surface morphology of Ta4HfC5 ceramic film was photographed using Dimension ICON atomic force microscope (AFM) from Bruker GmbH, Germany. The tapping mode was used and the scanning area was 2 μm×2 μm. The surface roughness (Ra) of the film was analyzed using NanoScope Analysis software. The results are shown in the attached figure. Figure 3 As shown: The surface AFM morphology of Ta4HfC5 ceramic film is a needle-like structure with a surface roughness of 1.03 nm.

[0054] The surface roughness of the film will affect the wear resistance of the film. The friction coefficient and wear rate of the film generally increase with the increase of surface roughness. This is because the rough surface has a smaller contact area and higher contact pressure, which will lead to a higher friction coefficient and wear loss. Therefore, a smaller surface roughness is conducive to improving the wear resistance of the film.

[0055] The Ta4HfC5 ceramic film was analyzed by XRD using a D8 Advance X-ray diffractometer (XRD) from BRUKER AXS GmbH, Germany. The operating voltage was 40 kV, the operating current was 40 mA, the X-ray source was Cu-Ka (λ=0.15418 nm), the grazing incidence angle was 1°, the scanning speed was 4° / min, the scanning step was 0.02° / step, and the scanning range was 10°~90°. The results are shown in the attached figure. Figure 4 shown.

[0056] Since the film is a micro-nanoscale material, its hardness can only be measured using a nanoindenter. Vickers hardness and Rockwell hardness are usually used to measure the hardness of alloy blocks, but cannot be used to measure the hardness of films. Therefore, the Nano Indenter G200 nanoindenter produced by Agilent Technologies was used to test the hardness of Ta4HfC5 ceramic films using the continuous stiffness mode. The results showed that the nanoindentation hardness value of Ta4HfC5 ceramic films was 25.23 GPa, and the elastic modulus value was 286.6 GPa, which can be used in high hardness and wear-resistant fields.

[0057] Example 2

[0058] This embodiment provides a Ta3Hf2C5 ceramic film, and the preparation method thereof is as follows: The P type, crystal direction is <100> 1. The single crystal Si wafer that had been previously treated with damping polishing was ultrasonically cleaned with anhydrous ethanol at a frequency of 60-80 Hz for 10 minutes to remove pollutants attached to the surface of the substrate. After ultrasonic cleaning, the substrate was rinsed with deionized water and then blown dry with compressed nitrogen to make its surface clean and free of water stains. The single crystal silicon wafer was fixed on a substrate disk, and the substrate disk was fixed on the substrate stage of the deposition chamber of the high vacuum magnetron sputtering coating equipment, and the rotating substrate baffle was adjusted to a position that completely covered the substrate.

[0059] High-purity metal targets Ta and Hf were placed on two different DC target positions in the deposition chamber, and graphite C target was placed on the RF target position. The angles of the targets relative to the center line perpendicular to the substrate stage were adjusted to 30°, and the vertical distance between the targets and the substrate stage was adjusted to 10 cm. The deposition chamber was first evacuated to less than 7.0 Pa using a mechanical pump, and then evacuated to less than 8.0×10 -3 Pa; high-purity Ar gas with a purity greater than or equal to 99.999% is introduced into the deposition chamber at a flow rate of 40 sccm, the working gas pressure is adjusted to 0.7 Pa, the power of the Ta target is set to 120 W, the power of the Hf target is set to 80 W, and the power of the C target is set to 120 W, and the target is pre-sputtered for 10 min to remove impurities on the surface of the target; after the pre-sputtering is completed, the substrate rotation rate is set to 15 r / min, the substrate baffle is opened, and formal sputtering for 1 h is started; after the sputtering is completed, the DC constant current power supply is turned off, the Ar gas source is turned off, the substrate rotation is turned off, the film is cooled to room temperature in a vacuum state, and then taken out to obtain the Ta3Hf2C5 ceramic film on the single crystal silicon wafer.

[0060] The chemical composition of the multi-principal alloy film was analyzed using an Oxford X-act energy dispersive spectrometer (EDS, installed on a scanning electron microscope). The surface and cross-sectional morphology SEM images and element surface scanning EDS spectra of the multi-principal alloy film are shown in the attached figure. Figure 5 and 6 As shown: According to the quantitative calculation results of the software, the composition of the alloy film is Ta3Hf2C5.

[0061] The surface morphology of Ta3Hf2C5 ceramic film was photographed using Dimension ICON atomic force microscope (AFM) from Bruker GmbH, Germany. The tapping mode was used and the scanning area was 2 μm×2 μm. The surface roughness (Ra) of the film was analyzed using NanoScope Analysis software. The results are shown in the attached figure. Figure 7 As shown: The surface AFM morphology of Ta3Hf2C5 ceramic film is a needle-like structure with a surface roughness of 1.35 nm.

[0062] The Ta4HfC5 ceramic film was analyzed by XRD using a D8 Advance X-ray diffractometer (XRD) from BRUKER AXS GmbH, Germany. The operating voltage was 40 kV, the operating current was 40 mA, the X-ray source was Cu-Ka (λ=0.15418 nm), the grazing incidence angle was 1°, the scanning speed was 4° / min, the scanning step was 0.02° / step, and the scanning range was 10°~90°. The results are shown in the attached figure. Figure 8 shown.

[0063] Since the film is a micro-nanoscale material, its hardness can only be measured using a nanoindenter. Vickers hardness and Rockwell hardness are usually used to measure the hardness of alloy blocks, but cannot be used to measure the hardness of films. Therefore, the Nano Indenter G200 nanoindenter produced by Agilent Technologies was used to test the hardness of Ta3Hf2C5 ceramic films using the continuous stiffness mode. The results showed that the nanoindentation hardness value of Ta3Hf2C5 ceramic films was 21.34 GPa, and the elastic modulus value was 270.1 GPa.

[0064] Example 3

[0065] This embodiment provides a Ta 4.5 HkDJ 4.5 Ceramic film, the preparation method thereof is as follows: The P type, crystal direction is <100> 1. The single crystal Si wafer that had been previously treated with damping polishing was ultrasonically cleaned with anhydrous ethanol at a frequency of 60-80 Hz for 10 minutes to remove pollutants attached to the surface of the substrate. After ultrasonic cleaning, the substrate was rinsed with deionized water and then blown dry with compressed nitrogen to make its surface clean and free of water stains. The single crystal silicon wafer was fixed on a substrate disk, and the substrate disk was fixed on the substrate stage of the deposition chamber of the high vacuum magnetron sputtering coating equipment, and the rotating substrate baffle was adjusted to a position that completely covered the substrate.

[0066] High-purity metal targets Ta and Hf were placed on two different DC target positions in the deposition chamber, and graphite C target was placed on the RF target position. The angles of the targets relative to the center line perpendicular to the substrate stage were adjusted to 30°, and the vertical distance between the targets and the substrate stage was adjusted to 10 cm. The deposition chamber was first evacuated to less than 7.0 Pa using a mechanical pump, and then evacuated to less than 8.0×10 -3Pa; high-purity Ar gas with a purity greater than or equal to 99.999% at a flow rate of 40 sccm was introduced into the deposition chamber, the working gas pressure was adjusted to 0.7 Pa, the power of the Ta target was set to 160 W, the power of the Hf target was set to 40 W, and the power of the C target was set to 160 W, and the target was pre-sputtered for 10 min to remove impurities on the surface of the target; after the pre-sputtering was completed, the substrate rotation rate was set to 15 r / min, the substrate baffle was opened, and formal sputtering for 1 h was started; after the sputtering was completed, the DC constant current power supply was turned off, the Ar gas source was turned off, the substrate rotation was turned off, and the film was cooled to room temperature under vacuum and then taken out to obtain the Ta on the single crystal silicon wafer. 4.5 HkDJ 4.5 Ceramic film.

[0067] The chemical composition of the multi-principal alloy film was analyzed using an Oxford X-act energy dispersive spectrometer (EDS, installed on a scanning electron microscope). The surface and cross-sectional morphology SEM images and element surface scanning EDS spectra of the multi-principal alloy film are shown in the attached figure. Fig. 9 and 10 As shown: According to the quantitative calculation results of the software, the composition of the alloy film is Ta 4.5 HkDJ 4.5 .

[0068] The Ta was photographed using the Dimension ICON atomic force microscope (AFM) from Bruker GmbH, Germany. 4.5 HkDJ 4.5 The surface morphology of the ceramic film was analyzed using the tapping mode with a scanning area of ​​2 μm×2 μm. The surface roughness (Ra) of the film was analyzed using NanoScope Analysis software. The results are shown in the attached figure. Fig.11 Shown: Ta 4.5 HkDJ 4.5 The surface AFM morphology of the ceramic film is a needle-like structure with a surface roughness of 1.15 nm.

[0069] The surface roughness of the film will affect the wear resistance of the film. The friction coefficient and wear rate of the film generally increase with the increase of surface roughness. This is because the rough surface has a smaller contact area and higher contact pressure, which will lead to a higher friction coefficient and wear loss. Therefore, a smaller surface roughness is conducive to improving the wear resistance of the film.

[0070] The Ta was characterized by a D8 Advance X-ray diffractometer (XRD) from BRUKER AXS GmbH, Germany. 4.5 HkDJ 4.5The XRD phase analysis of the ceramic film was carried out with an operating voltage of 40 kV, an operating current of 40 mA, an X-ray source of Cu-Ka (λ=0.15418nm) rays, a grazing incidence angle of 1°, a scanning speed of 4° / min, a scanning step of 0.02° / step, and a scanning range of 10°~90°. The results are shown in the attached figure. Fig.12 shown.

[0071] Since the film is a micro-nanoscale material, its hardness can only be measured using a nanoindenter. Vickers hardness and Rockwell hardness are usually used to measure the hardness of alloy blocks, but cannot be used to measure the hardness of films. Therefore, the Nano Indenter G200 nanoindenter produced by Agilent Technologies was used in the continuous stiffness mode to measure the hardness of Ta. 4.5 HkDJ 4.5 The hardness of the ceramic film was tested and the results showed that Ta 4.5 HkDJ 4.5 The nano-indentation hardness value of the ceramic film is 23.83 GPa, and the elastic modulus value is 277.9 GPa. It can be used in high-hardness and wear-resistant fields.

[0072] Comparative Example 1

[0073] This embodiment provides a Ta2Hf 2.5 C 5.5 Ceramic film, the preparation method thereof is as follows: The P type, crystal direction is <100> 1. The single crystal Si wafer that had been previously treated with damping polishing was ultrasonically cleaned with anhydrous ethanol at a frequency of 60-80 Hz for 10 minutes to remove pollutants attached to the surface of the substrate. After ultrasonic cleaning, the substrate was rinsed with deionized water and then blown dry with compressed nitrogen to make its surface clean and free of water stains. The single crystal silicon wafer was fixed on a substrate disk, and the substrate disk was fixed on the substrate stage of the deposition chamber of the high vacuum magnetron sputtering coating equipment, and the rotating substrate baffle was adjusted to a position that completely covered the substrate.

[0074] High-purity metal targets Ta and Hf were placed on two different DC target positions in the deposition chamber, and graphite C target was placed on the RF target position. The angles of the targets relative to the center line perpendicular to the substrate stage were adjusted to 30°, and the vertical distance between the targets and the substrate stage was adjusted to 10 cm. The deposition chamber was first evacuated to less than 7.0 Pa using a mechanical pump, and then evacuated to less than 8.0×10 -3Pa; high-purity Ar gas with a purity greater than or equal to 99.999% at a flow rate of 40 sccm was introduced into the deposition chamber, the working gas pressure was adjusted to 0.7 Pa, the power of the Ta target was set to 80 W, the power of the Hf target was set to 90 W, and the power of the C target was set to 110 W, and the target was pre-sputtered for 10 min to remove impurities on the surface of the target; after the pre-sputtering was completed, the substrate rotation rate was set to 15 r / min, the substrate baffle was opened, and formal sputtering for 1 hour was started; after the sputtering was completed, the DC constant current power supply was turned off, the Ar gas source was turned off, the substrate rotation was turned off, and the film was cooled to room temperature under vacuum and then taken out to obtain the Ta2Hf 2.5 C 5.5 Ceramic film.

[0075] The chemical composition of the multi-principal alloy film was analyzed using an Oxford X-act energy dispersive spectrometer (EDS, installed on a scanning electron microscope). The surface and cross-sectional morphology SEM images and element surface scanning EDS spectra of the multi-principal alloy film are shown in the attached figure. Fig.13 and 14 As shown: According to the quantitative calculation results of the software, the composition of the alloy film is Ta2Hf 2.5 C 5.5 .

[0076] Ta2Hf was photographed using the Dimension ICON atomic force microscope (AFM) from Bruker GmbH, Germany. 2.5 C 5.5 The surface morphology of the ceramic film was analyzed using the tapping mode with a scanning area of ​​2 μm×2 μm. The surface roughness (Ra) of the film was analyzed using NanoScope Analysis software. The results are shown in the attached figure. Fig.15 Shown: Ta2Hf 2.5 C 5.5 The surface AFM morphology of the ceramic film is a needle-like structure with a surface roughness of 1.47 nm.

[0077] The surface roughness of the film will affect the wear resistance of the film. The friction coefficient and wear rate of the film generally increase with the increase of surface roughness. This is because the rough surface has a smaller contact area and higher contact pressure, which will lead to a higher friction coefficient and wear loss. Therefore, a smaller surface roughness is conducive to improving the wear resistance of the film.

[0078] The Ta4HfC5 ceramic film was analyzed by XRD using a D8 Advance X-ray diffractometer (XRD) from BRUKER AXS GmbH, Germany. The operating voltage was 40 kV, the operating current was 40 mA, the X-ray source was Cu-Ka (λ=0.15418 nm), the grazing incidence angle was 1°, the scanning speed was 4° / min, the scanning step was 0.02° / step, and the scanning range was 10°~90°. The results are shown in the attached figure. Fig.16 shown.

[0079] Since the film is a micro-nanoscale material, its hardness can only be measured using a nanoindenter. Vickers hardness and Rockwell hardness are usually used to measure the hardness of alloy blocks, but cannot be used to measure the hardness of films. Therefore, the Nano Indenter G200 nanoindenter produced by Agilent Technologies was used in the continuous stiffness mode to measure the hardness of Ta2Hf 2.5 C 5.5 The hardness of the ceramic film was tested and the results showed that Ta2Hf 2.5 C 5.5 The nanoindentation hardness value of the ceramic film is 16.73 GPa, and the elastic modulus value is 222.8 GPa.

[0080] The properties of the Ta-Hf-C ceramic materials obtained in the examples and comparative examples are shown in Table 1 below.

[0081] Table 1

[0082] It can be seen from the comparison results in Table 1 that, compared with the Ta-Hf-C ceramic material of Comparative Document 1, the Ta-Hf-C ceramic material of the present invention has lower surface roughness, higher hardness and elastic modulus, has a wider application prospect, can be applied to extreme service conditions, and has application potential in the field of protection.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A Ta-Hf-C ceramic material, characterized in that: The chemical formula is Ta a Hf b C c ; Among them, 3≤a≤4.5, 0.5≤b≤2 and a+b+c=10.

2. The Ta-Hf-C ceramic material according to claim 1, characterized in that: The Ta-Hf-C ceramic material satisfies at least one of the following characteristics (1)-(4): (1) The Ta-Hf-C ceramic material has a single-phase face-centered cubic crystal structure; (2) The surface roughness of the Ta-Hf-C ceramic material is 1.03-1.35 nm; (3) The hardness of the Ta-Hf-C ceramic material is 21.34~25.23 Gpa; (4) The elastic modulus of the Ta-Hf-C ceramic material is 270.1~286.6 GPa.

3. The method for preparing the Ta-Hf-C ceramic material according to claim 1 or 2, characterized in that: The Ta-Hf-C ceramic material is prepared by multi-target DC magnetron sputtering.

4. The method for preparing the Ta-Hf-C ceramic material according to claim 3, characterized in that: The steps include: Fixing the substrate on the substrate stage; Place the Ta target and the Hf target on different DC target positions respectively, place the C target on the RF target position, and adjust the angle of the target relative to the center line perpendicular to the substrate stage and the vertical distance between the target and the substrate stage; Under inert gas, pre-sputtering the target material; Thin film sputtering is performed on the sputtering surface of the substrate to obtain the Ta-Hf-C ceramic material on the substrate.

5. The method for preparing the Ta-Hf-C ceramic material according to claim 4, characterized in that: The sputtering power of the Ta target is 120-160 W; the sputtering power of the Hf target is 40-80 W; the sputtering power of the C target is 120-160 W; and the sputtering time is 0.5-1.5 h.

6. The method for preparing the Ta-Hf-C ceramic material according to claim 4 or 5, characterized in that: The substrate is a single crystal silicon wafer, the silicon wafer is P-type, and the crystal orientation is <100> ; And / or, the Ta target, the Hf target and the C target are all high-purity blocks with a purity greater than or equal to 99.95%, a diameter of 50-70 mm, and a thickness of 4-6 mm.

7. The method for preparing the Ta-Hf-C ceramic material according to any one of claims 4 to 6, characterized in that: The angle of the target relative to the center line perpendicular to the substrate stage is 20~40°; and / or, the vertical distance between the Ta target, the Hf target and the C target and the substrate stage is 5~15 cm; and / or, the pre-sputtering time is 10~15 min.

8. The method for preparing the Ta-Hf-C ceramic material according to any one of claims 4 to 7, characterized in that: The sputtering is performed in a deposition chamber; preferably, the vacuum of the deposition chamber is 6×10 -3 ~8×10 -3 Pa, the gas pressure is 0.7~0.9 Pa; and / or, the inert gas includes one or more of argon, helium or nitrogen; preferably, the flow rate of the inert gas is 30~50 sccm, and the purity is greater than or equal to 99.999%.

9. The method for preparing a Ta-Hf-C ceramic material according to any one of claims 4 to 8, characterized in that: Before fixing the substrate on the substrate stage, the substrate is pretreated; preferably, the pretreatment of the substrate comprises the following steps: ultrasonically cleaning the substrate in anhydrous ethanol, and then rinsing the substrate with water; blowing the cleaned substrate dry with compressed nitrogen; preferably, the frequency of the ultrasonic cleaning is 60-80 Hz, and the time is 5-15 min; preferably, the sputtering surface of the substrate is polished with a damping cloth before ultrasonic cleaning.

10. An application of Ta-Hf-C ceramic material, characterized in that: The Ta-Hf-C ceramic material is the Ta-Hf-C ceramic material according to claim 1 or 2, or the Ta-Hf-C ceramic material prepared by the preparation method according to any one of claims 3 to 9; the Ta-Hf-C ceramic material is applied in a protective coating.

Citation Information

Patent Citations

  • Preparation method of Ta-C-N thin-film

    CN102127743A

  • Metallic carbide coating and preparation method thereof

    CN109735804A

  • Organic-metal nano composite film as well as preparation method and application thereof

    CN112030108A

  • High-hardness high-modulus tantalum-hafnium-carbon ternary ceramic carbide coatings and production method thereof

    CN112647043A

  • Tungsten-doped tantalum-hafnium carbide thin film material and preparation method thereof

    CN114959572A