Method for preparing wafer-level dry photoresist by using molecular layer deposition
Through the combination of molecular layer deposition technology and electron beam exposure, the problem of accurate controllable photoresist thickness and high uniformity is solved, and efficient photoresist preparation in EUV lithography technology is achieved, with super strong anti-etching corrosion performance and good resolution.
Patent Information
- Application Number
- CN202410941055.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing photoresist is difficult to achieve accurate and controllable thickness and high uniformity in EUV lithography technology, especially in high numerical aperture EUV lithography machines. Physical spin coating method is difficult to solve the problem of photoresist thickness below 20 or even 10 nanometers. Requirements.
Using molecular layer deposition technology, using metal and organic sources as precursors, dry photoresist is deposited through the MLD device controlled by LabVIEW, combined with electron beam exposure and ICP etching to achieve precise control of film thickness, and at 70-150 Baking and developing treatments were carried out at °C.
Accurate control of photoresist thickness to angstroms (0.1 nanometers), and has excellent etch resistance and good resolution. It is suitable for dry and wet development, and can process 50 nanometer lines. The selective etch ratio with silicon reaches 150 or higher.
Smart Images

Figure CN118880285A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoresist preparation, and in particular to a universal method for preparing wafer-level dry photoresist by using molecular layer deposition. Background Art
[0002] As a key technology for manufacturing large-scale integrated circuits, the development of photolithography technology directly determines the future direction of integrated circuits. As the process nodes of integrated circuits continue to decrease, photolithography technology is also constantly improving, and has now developed to EUV (EUV, 13.5nm) lithography technology. Although EUV lithography machines are now available, there is a lack of photoresists suitable for EUV lithography, which greatly hinders the development of process nodes below 5nm. At present, organic photoresists are mainly used. However, metal-based photoresists are increasingly gaining attention. This type of photoresist is mainly composed of metal nanoparticles (such as hafnium oxide, zinc oxide, and zirconium oxide) modified by organic ligands (such as para-hydroxystyrene and methacrylic acid). Compared with traditional organic photoresists, inorganic photoresists can better absorb EUV light, have better etching resistance, are more resistant to pattern collapse, and have smaller line edge roughness, which has attracted many people to study this.
[0003] Organic photoresists are composed of light elements such as C, H, and O, and their absorption of EUV light is too weak, resulting in a very low photosensitivity. Metal-based photoresists have become a better option. However, with the advent of high numerical aperture (NA) EUV lithography machines, the thickness of the photoresist is required to be less than 20 or even 10 nanometers. The physical spin-coating photoresist method used by both organic and metal-based photoresists is difficult to solve this problem. Therefore, there is an urgent need for a method for preparing metal-based photoresists with precisely controllable thickness and high uniformity. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a dry photoresist that can accurately control the film thickness. The thickness of the dry photoresist can be accurately controlled by using molecular layer deposition (MLD). The thickness of the photoresist can be accurately controlled to angstroms. The chip has a surface area of 0.1 nanometers and has high uniformity, excellent etching resistance (selective etching ratio with silicon is above 80) and good resolution (can reach at least 25 nm).
[0005] The purpose of the present invention is to provide a method for preparing a dry photoresist that can accurately control the thickness of a thin film. Electron beam, DUV, EUV lithography is used, post-baking is performed at 70-150°C for 50-600s, and weak alkaline solutions such as tetramethylammonium hydroxide and ammonia are used for wet development. Plasma oxygen, CHF3, CF4, etc. can also be used for dry development. Then, the pattern on the photoresist is transferred to the substrate by ICP etching (etching gas is SF6, C4F8). The technical scheme adopted is as follows:
[0006] A metal source and an organic source are used as precursors to carry out molecular layer deposition, and a dry photoresist is obtained after the deposition.
[0007] The metal source includes at least one of metal precursors such as aluminum, hafnium, tin, indium, bismuth, etc. and rare metal precursors such as yttrium, erbium, etc.
[0008] The organic source precursor includes: one of ethylene glycol, propylene glycol, propylene glycol, butanediol and its isomers, butene glycol and its isomers, pentene glycol and its isomers, hexene glycol and its isomers, heptene glycol and its isomers, octenediol and its isomers, phenol, and dithiol.
[0009] The specific steps of the molecular layer deposition are:
[0010] The film was deposited in an MLD device controlled by LabVIEW. The metal source was kept at its evaporation temperature, and the source bottle containing the organic source was heated to a certain temperature. The temperature of the reactor was kept at 80-150°C, and 20 sccm of dry nitrogen was used to purge the reaction. Each cycle reaction consisted of two half cycles: (1) introducing the metal source and purging with nitrogen; (2) introducing the organic source and purging with nitrogen. The deposition thickness was controlled according to the number of deposition cycles. For example, when trimethylaluminum and 1,4-butenediol were used as precursors, the growth thickness of each cycle was 0.1 nanometers; when tetrakis(dimethylamino)hafnium and 1,4-butenediol were used as precursors, the growth thickness of each cycle was 0.075 nanometers.
[0011] The technical effect is: the present invention can accurately control the film thickness, and the desired thickness can be obtained by controlling the number of cycles, which is difficult to achieve with the traditional spin coating method. When using 30keV electron beam exposure, the photoresist of tetrakis(dimethylamino)hafnium and 1,4-butenediol can achieve a resolution of at least 40 nanometers, and when using 50keV electron beam exposure, the photoresist of trimethylaluminum and 1,4-butenediol can achieve a resolution of at least 25 nanometers. And it can be suitable for dry development (ICP development) and wet development (development with alkaline solutions such as tetramethylammonium hydroxide and ammonia water). When using ICP etching, the selective etching ratio of aluminum-based photoresist to silicon can reach 150, and the selective etching ratio of hafnium-based photoresist to silicon can reach 30, and 50-nanometer lines can be processed. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 a is the growth principle diagram of this type of photoresist. Figure 1 b is the growth principle diagram of this type of photoresist prepared using trimethylaluminum and 1,4-butenediol. Figure 1 c Schematic diagram of the growth of this photoresist prepared using tetrakis(dimethylamino)hafnium and 1,4-butenediol.
[0013] Figure 2 a is an AFM side view of the photoresist surface when such photoresist is prepared using trimethylaluminum and 1,4-butenediol and the growth thickness is 30 nanometers, and the surface roughness Rq=0.2nm; b is an AFM side view of the photoresist surface when such photoresist is prepared using tetrakis(dimethylamino)hafnium and 1,4-butenediol and the growth thickness is 30 nanometers, and the surface roughness Rq=0.1nm;
[0014] Figure 3 SEM image of HP=200nm; SEM image of HP=150nm; SEM image of HP=100nm; SEM image of HP=40nm; SEM image of HP=30nm; SEM image of HP=25nm. The exposure voltage was 50kV, and 10wt% ammonia water was used for development for 15s.
[0015] Figure 4 a is the top view and oblique view of AFM after 0 seconds of ICP etching, with a groove depth of 17.5 nanometers; b is the top view and oblique view of AFM after 12 seconds of ICP etching, with a groove depth of 315 nanometers; c is the top view and oblique view of AFM after 24 seconds of ICP etching, with a groove depth of 710 nanometers; d is the top view and oblique view of AFM after 48 seconds of ICP etching, with a groove depth of 1503 nanometers. The line widths of a, b, c, and d are all 2.5 μm.
[0016] Figure 5a is a 200nm SEM pattern, L / S = 1:2 at 2keV. b is a 50nm SEM pattern, L / S = 1:5 at 2keV. c is a 40nm SEM pattern, L / S = 1:5 at 2keV. d is a 1000nm, 500nm, 300nm SEM pattern, L / S = 1:1 at 2kV. e is a 200nm, 100nm, 50nm SEM pattern, L / S = 1:3 at 2kV. f is a 100nm, 50nm SEM pattern, L / S = 1:3 at 2kV. a, b, c are developed using 10wt% tetramethylammonium hydroxide for 15s; d, e, f are developed using ICP (plasma oxygen) dry method for 60s.
[0017] Figure 6 a is the top view of AFM after 0 seconds of ICP etching of 1000nm, 500nm, 300nm lines (L\S=1:1), the groove depth is 15.8 nanometers; b is the top view of AFM after 24 seconds of ICP etching of 1000nm, 500nm, 300nm lines (L\S=1:1), the groove depth of 1000nm is 407 nanometers; c is the top view of AFM after 1000nm ICP etching, the groove depth is 407 nanometers; d is the oblique view of AFM after 24 seconds of ICP etching, the groove depth is 407 nanometers. The line widths of a, b, c, and d are all 2.5μm. DETAILED DESCRIPTION
[0018] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. The methods described are conventional methods unless otherwise specified. The raw materials described can be obtained from public commercial channels unless otherwise specified. The photoresist is prepared using molecular layer deposition. In each complete cycle, the metal source ligand combines with the hydroxyl bond or sulfur bond on the organic source, and the final film is obtained through multiple cycles of growth. The film thickness can be accurately controlled by the number of cycles. The schematic diagram of the principle of the molecular layer deposition method for growing dry photoresist of the present invention is as follows Figure 1 shown.
[0019] Example 1: This photoresist was prepared using trimethylaluminum and 1,4-butenediol.
[0020] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. The source bottle containing trimethylaluminum was kept at room temperature, and the source bottle containing 1,4-butenediol was heated to 85°C. The temperature of the reactor was maintained at 90°C, and 20sccm of dry nitrogen was used to purge the reaction. Each cycle reaction consisted of two half cycles: (1) 50 milliseconds of aluminum source was introduced and nitrogen was purged for 16 seconds; (2) 150 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 25 seconds. The system pressure was 13 Pa, and the film thickness was 32 nanometers after 400 cycles of deposition. The schematic diagram is shown in the figure. Figure 1 b.
[0021] Surface roughness: When the growth thickness is 30 nanometers, Rq = 0.23 nanometers, such as Figure 2 a.
[0022] The photoresist is exposed using an electron beam, then dried at 80°C for 90 seconds, and then developed using 10wt% ammonia water for 15 seconds to obtain exposed lines. 50keV can obtain 200 nanometers to 25 (line / blank = 1:1) nanometer lines, such as Figure 3 .
[0023] The specific etching recipe for ICP etching is: temperature 20℃, chamber pressure 15mTorr, excitation power 400W, bias power 20W, SF6: 15sccm, C4F8: 60sccm. We can etch silicon to a depth of 1500 nanometers with 18 nanometer photoresist, and the selective etching ratio with silicon is 83 (etching line is 2.5μm). Figure 4 .
[0024] Example 2: The photoresist was prepared using tetrakis(dimethylamino)hafnium and 1,4-butenediol.
[0025] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. The source bottle containing tetrakis(dimethylamino)hafnium was heated to 80°C, and the source bottle containing 1,4-butenediol was heated to 85°C. The temperature of the reactor was maintained at 100°C, and 20sccm of dry nitrogen was used to purge the reaction. Each cycle reaction consisted of two half cycles: (1) 100 milliseconds of hafnium source was introduced and nitrogen was purged for 30 seconds; (2) 450 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 50 seconds. The system pressure was 13 Pa. The schematic diagram is shown in the figure. Figure 1 c.
[0026] Surface roughness: When the growth thickness is 30 nanometers, Rq = 0.1 nanometers, such as Figure 2 b.
[0027] The photoresist was exposed using an electron beam, then dried at 80°C for 90 seconds, and then developed using 10wt% tetramethylammonium hydroxide for 15 seconds (negative photoresist) to obtain exposed lines. 30keV can obtain 200nm to 40nm lines. ICP (gas is oxygen) was used for dry development (positive photoresist), and 30keV can obtain 200nm to 50nm lines.
[0028] The specific etching recipe for ICP etching is: temperature 20℃, chamber pressure 15mTorr, excitation power 400W, bias power 20W, SF6: 15sccm, C4F8: 60sccm. We etched 15.8nm photoresist to a depth of 407nm in silicon, with a selective etching ratio of 26 (etched line 1μm).
[0029] Example 3: The photoresist was prepared using tetrakis(dimethylamino)tin and 1,4-butenediol.
[0030] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. The source bottle containing tetrakis(dimethylamino)tin was heated to 70°C, and the source bottle containing 1,4-butenediol was heated to 85°C. The temperature of the reactor was maintained at 100°C, and 20sccm of dry nitrogen was used to purge the reaction. Each cycle reaction consisted of two half cycles: (1) 75 milliseconds of tin source was introduced and nitrogen was purged for 25 seconds; (2) 300 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 45 seconds. The system pressure was 13 Pa. Exposure and etching tests were the same as in Example 1.
[0031] Example 4: The photoresist was prepared using trimethylaluminum and glycerol.
[0032] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. Trimethylaluminum was kept at room temperature, and the source bottle containing glycerol was heated to 180°C. The temperature of the reactor was maintained at 200°C, and 20 sccm of dry nitrogen was used to purge the reaction. Each cycle reaction consisted of two half cycles: (1) 50 milliseconds of aluminum source was introduced and nitrogen was purged for 25 seconds; (2) 300 milliseconds of glycerol was introduced and nitrogen was purged for 40 seconds. The system pressure was 13 Pa. Exposure and etching tests were the same as in Example 1.
[0033] Example 5: This photoresist is prepared using trimethylaluminum, tetrakis(dimethylamino)tin and 1,4-butenediol.
[0034] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. The source bottle containing trimethylaluminum was kept at room temperature, the source bottle containing tetrakis(dimethylamino)tin was heated to 70°C, and the source bottle containing 1,4-butenediol was heated to 180°C. The temperature of the reactor was maintained at 200°C, and the reaction was purged with 20sccm of dry nitrogen. Each cycle reaction consisted of 4 half cycles: (1) 50 milliseconds of aluminum source was introduced and nitrogen was purged for 25 seconds; (2) 300 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 40 seconds; (3) 75 milliseconds of tin source was introduced and nitrogen was purged for 25 seconds; (4) 300 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 40 seconds. The system pressure was 13 Pa. The exposure and etching tests were the same as in Example 1.
[0035] Example 6: This photoresist was prepared using trimethylaluminum, tri(cyclopentadienyl)yttrium and 1,4-butenediol.
[0036] A 4-inch silicon wafer was placed in an MLD device controlled by LabVIEW for deposition. The source bottle containing trimethylaluminum was kept at room temperature, the source bottle containing tri(cyclopentadienyl)yttrium was heated to 170°C, and the source bottle containing 1,4-butenediol was heated to 85°C. The temperature of the reactor was maintained at 200°C, and the reaction was purged with 20 sccm of dry nitrogen. Each cycle reaction consisted of 4 half cycles: (1) 50 milliseconds of aluminum source was introduced and nitrogen was purged for 25 seconds; (2) 300 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 40 seconds; (3) 75 milliseconds of yttrium source was introduced and nitrogen was purged for 25 seconds; (4) 300 milliseconds of 1,4-butenediol was introduced and nitrogen was purged for 40 seconds. The system pressure was 13 Pa. The exposure and etching tests were the same as in Example 1.
[0037] Comparative Example 1: Polymethyl methacrylate (PMMA) photoresist (positive photoresist) was spin-coated at 8000 rpm for 60 seconds and pre-baked at 180°C for 3 minutes. The thickness was about 100 nanometers. The film thickness could not be well controlled. At the same time, ICP was used to etch it, and its selective etching ratio for silicon was about 1.
[0038] Comparative Example 2: Hydrogen silsesquioxane polymer (HSQ) photoresist was patterned using a spin coating method, 4000 rpm for 60 seconds, and pre-baked at 120°C for 5 minutes. The thickness was about 90 nanometers, and the film thickness could not be well controlled. At the same time, ICP was used to etch it, and its selective etching ratio for silicon was about 2.5.
[0039] By comparing with the comparative example, it is shown that the present invention uses molecular layer deposition to prepare wafer-level dry photoresist, which can accurately control the thickness of the photoresist film. At the same time, the etching resistance is more than 10 times that of traditional photoresists and has good resolution.
[0040] It should be further explained that the above implementation modes are only used to illustrate the technical concept and technical solution of the present invention, and are not used to limit the protection scope of the present invention. Obvious adjustments and changes made to the technical solution within the technical concept of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing wafer-level dry photoresist using molecular layer deposition, characterized in that: Using metal source and organic source as precursors, molecular layer deposition is performed to obtain dry photoresist. The specific steps of molecular layer deposition are as follows: The metal source is maintained at its evaporation temperature, and the source bottle containing the organic source is heated to a certain temperature. The temperature of the reactor is maintained at 80-150°C, and 20 sccm of dry nitrogen is used to purge the reaction. Each cycle reaction consists of two half cycles: (1) introducing the metal source and purging with nitrogen; (2) introducing the organic source and purging with nitrogen. The deposition thickness is controlled according to the number of deposition cycles.
2. The method for preparing wafer-level photoresist by using molecular layer deposition according to claim 1, characterized in that: the metal source include: At least one of the metal precursors of aluminum, hafnium, tin, indium, bismuth and the rare earth metal precursors of yttrium, erbium and lanthanum.
3. The method for preparing wafer-level dry photoresist by using molecular layer deposition according to claim 1, characterized in that: The organic source precursor includes: one of ethylene glycol, propylene glycol, propylene glycol, butanediol and its isomers, butene glycol and its isomers, pentene glycol and its isomers, hexene glycol and its isomers, heptene glycol and its isomers, octenediol and its isomers, phenol, and dithiol.
4. The method for preparing wafer-level dry photoresist by using molecular layer deposition according to claim 1, characterized in that: The molecular layer deposition is carried out on a silicon, silicon dioxide or mica substrate.
5. The method for preparing wafer-level dry photoresist by using molecular layer deposition according to claim 1, characterized in that: Its film The thickness is precisely controlled by the number of growth cycles.
6. The method for preparing wafer-level dry photoresist by using molecular layer deposition according to claim 1, characterized in that: In each complete cycle, the metal source ligand combines with the hydroxyl bond or sulfur bond on the organic source ligand, and the final film is obtained through multiple cycles of growth.
Citation Information
Patent Citations
Preparation method of aperture adjustable porous metal oxide based on molecular layer deposition
CN110512189A
Method for preparing wafer-level aluminum-based-enediol dry photoresist by using molecular layer deposition
CN117587380A
Cited By
Method for preparing wafer-level nanoimprint photoresist based on molecular layer deposition technology
CN120044749A
Erasable organic-inorganic hybrid patterned film prepared by molecular layer deposition
CN120122387A
Hafnium oxide-based single magnetoelectric coupling multiferroic material as well as preparation method and application thereof
CN120664601A
Titanium-based-dienediol dry photoresist and preparation method thereof