Treatment method for forming long-life conductive corrosion-resistant coating on surface of metal matrix
By forming a defective TiO layer on the surface of the metal matrix and forming a Ti-O-C bonding composite coating using discharge plasma treatment, the problem of insufficient binding force of the carbon coating is solved, and the metal plate is significantly improved in the hydrogen fuel cell environment service life and corrosion resistance.
Patent Information
- Application Number
- CN202410932698.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The existing carbon coatings are insufficiently bound to the surface of the metal matrix, resulting in poor service life in hydrogen fuel cell environments, especially due to poor lattice compatibility between carbon and metal matrix, resulting in the physical vapor deposition of carbon coatings for a long time. It is easy to fall off during service.
First, a defective TiO layer is formed on the surface of the metal matrix, and then the carbon source gas is excited by the discharge plasma treatment to form a high-active carbon source group, react with the TiO layer to form a Ti-O-C-bonded composite coating, which enhances the carbon layer and The bonding force of the metal matrix.
The bonding force between the carbon doped layer and the metal matrix is significantly improved, the service life of the metal plate in the hydrogen fuel cell environment is extended, the corrosion current density and contact resistance are reduced, and the corrosion resistance and density of the coating are improved.
Smart Images

Figure CN118880322A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of preparation of conductive corrosion-resistant coatings on metal surfaces, in particular to preparation of conductive corrosion-resistant coatings on the surfaces of metal bipolar plates of fuel cells, and in particular to a treatment method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate. Background Art
[0002] Metal plates have the advantages of reliable mechanical strength, high electrical conductivity, high thermal conductivity and high air tightness, and are one of the key components of hydrogen fuel cells. Due to the strong oxidative corrosion in the hydrogen fuel cell environment, in order to ensure the long-term stable service of metal plates in the hydrogen fuel cell environment, high-conductivity and corrosion-resistant coating is an essential and important step in the preparation of high-performance metal plates.
[0003] Carbon coating has good electrical conductivity and chemical stability, and its manufacturing cost is low (compared to precious metal coating, etc.), so carbon coating is the mainstream commercial metal plate coating in the current market. There are two main methods for preparing carbon coating: chemical vapor deposition and physical vapor deposition. Among them, physical vapor deposition has the advantages of adjustable coating thickness and good process reproducibility, and is currently the most important method for preparing carbon coating. However, the main problem facing carbon coating at present is that the bonding force is not ideal. Carbon, as a non-metallic element, has poor lattice compatibility with the metal substrate. For example, chemical vapor deposition directly deposits carbon coating on the surface of the metal substrate, and the prepared carbon coating often has poor bonding force. Physical vapor deposition generally first coats a layer of pure titanium layer or titanium / carbon mixed coating that is compatible with both the metal substrate and the carbon layer as a transition layer, and uses the transition layer to enhance the bonding force between the carbon coating and the metal substrate. This method can improve the film-based bonding force to a certain extent, but the compatibility of the transition titanium layer and the carbon layer is still relatively limited. In long-term service tests, the physical vapor deposition carbon coating still shows obvious shedding.
[0004] Based on the above-mentioned deposition of carbon coating on the surface of metal substrate, the advantages of good conductivity, high stability and low cost of carbon coating are utilized. However, the carbon coatings currently prepared on metal substrates face the problem of insufficient bonding strength, which in turn leads to less than ideal service life of metal plates in corrosive environments such as hydrogen fuel cells. Summary of the invention
[0005] In view of the above-mentioned deficiencies of the prior art, the purpose of the present invention is to provide a treatment method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate. A Ti layer is first formed on the surface of the metal substrate as a base bonding layer, and then a defective titanium oxide (i.e., TiO) layer is prepared in a high vacuum environment. On this basis, a carbon source gas is used to excite and crack to form a high-activity carbon source group to react with the defective TiO to form a Ti-OC bonding transition zone, and finally a carbon-doped layer with excellent bonding strength is obtained, thereby achieving the expected effect of long-life conductivity.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention provides a processing method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate, comprising the following steps:
[0008] forming a Ti layer as a base bonding layer on the surface of the metal substrate;
[0009] A mixed atmosphere consisting of argon and oxygen is introduced into the environment of the metal substrate containing the Ti layer, and the vacuum degree is maintained at 0.1-1.0 Pa, and then a physical vapor deposition coating process is performed to form a defective TiO layer on the surface of the metal substrate;
[0010] The metal substrate containing the TiO layer is placed in a vacuum of 3×10 -3 Pa~5×10 -3 Pa, a carbon source gas and a carrier gas are introduced, and then a discharge plasma treatment is performed to excite and crack the carbon source gas to form a high-activity carbon source group, and then the generated high-activity carbon source group reacts with TiO to form a black coating on the surface of the metal substrate, thereby obtaining a metal substrate with a Ti-OC bonding composite coating.
[0011] Preferably, the Ti layer as the base bonding layer is formed on the surface of the metal substrate by placing the cleaned metal substrate in a vacuum of 6×10 -4 The film is obtained by physical vapor deposition coating process under vacuum environment below Pa, with argon gas introduced and vacuum degree maintained at 0.1-1.0 Pa.
[0012] Preferably, the carbon source gas includes but is not limited to any one of CH4, C2H2 or C3H6.
[0013] Preferably, the carrier gas is argon, and the flow ratio of the carbon source gas to the carrier gas is 1:2.
[0014] Preferably, the flow ratio of argon to oxygen is 1:1.
[0015] Preferably, the physical vapor deposition temperature for forming a Ti layer on the surface of the metal substrate is 200°C to 600°C, the physical vapor deposition power source power is 250W to 350W, the physical vapor deposition time is 200s to 600s, and the target material is a pure titanium target. The physical vapor deposition treatment temperature for forming a defective titanium oxide layer on the surface of the metal substrate is 200°C to 600°C, the physical vapor deposition power source power is 250W to 350W, the physical vapor deposition time is 500s to 2000s, and the target material is a pure titanium target. During the discharge plasma treatment, a plasma generator is used for discharge, the plasma generator power is set to 400W to 500W, the heating temperature is 500 to 700°C, and the treatment time is 1800s to 5500s.
[0016] Preferably, the cleaned metal substrate is obtained by the following steps:
[0017] The metal substrate is placed in anhydrous ethanol cleaning solution for ultrasonic cleaning to remove surface contaminants, and then placed in deionized water for surface cleaning again. The above sequence of cleaning is repeated several times until there is no contaminant visible to the naked eye on the surface of the metal substrate.
[0018] Preferably, the ultrasonic power of ultrasonic cleaning is 300W to 500W, the ultrasonic cleaning time in anhydrous ethanol is 5 to 10 minutes, and the ultrasonic cleaning time in deionized water is 3 to 6 minutes.
[0019] Preferably, the metal substrate with the Ti-OC bonding composite coating is also washed to remove floating carbon in a cleaning solution, and the cleaning solution is a citric acid aqueous solution, wherein the citric acid content is 5% to 15%.
[0020] Preferably, the metal substrate is stainless steel or titanium.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention forms a defective titanium monoxide layer (i.e., TiO) on the surface of the metal substrate, and then uses a physical vapor deposition method to dope carbon elements to form Ti-OC bonds in the TiO layer, thereby greatly enhancing the bonding force between the plated carbon layer and the metal substrate, thereby obtaining an ultra-long service life. The process is simple and efficient, environmentally friendly and non-toxic, and can greatly improve the service life of the metal substrate in a hydrogen fuel cell environment. This new processing technology can not only provide new ideas and means for preparing conductive and corrosion-resistant coatings on metal surfaces, but also promote the multi-scenario application of hydrogen fuel cells.
[0023] 2. The method provided by the present invention prepares a carbon / titanium oxide composite coating metal substrate with long service life, high conductivity and high corrosion resistance, thereby increasing the service life of the metal substrate in a hydrogen fuel cell environment.
[0024] 3. The composite coating obtained by the present invention using the method has a black luster and a dense and uniform surface. The electrochemical test results under a simulated fuel cell environment (80°C, 0.5mM sulfuric acid + 5ppm hydrofluoric acid) show that the minimum corrosion current density of the ordinary carbon coating is about 0.3μA / cm 2 The minimum corrosion current density of the Ti-OC bonded composite coating obtained by the method of the present invention is 0.004μA / cm 2 , decreased by nearly 100 times (e.g. Figure 1 As shown); after 500h, 0.8V constant potential polarization (80℃, 0.5mM sulfuric acid + 5ppm hydrofluoric acid), the surface coating of the traditional carbon coating has completely fallen off and serious oxidation corrosion marks have occurred (as shown Figure 2 As shown), the contact resistance is as high as 10000mΩ·cm 2 The surface of the composite coating only has slight oxidation corrosion, and the contact resistance is only 150mΩ·cm 2 The contact resistance test results show that after the accelerated corrosion test, the contact resistance of the composite coating obtained by the method of the present invention is at least 100 times lower than that of the ordinary carbon coating (such as Figure 3 As shown), the expected service life of the composite coating is much higher than that of the traditional carbon coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The figure is a comparison of polarization curves of the carbon-coated metal substrate and the composite-coated metal substrate of the present invention under a simulated fuel cell environment.
[0026] Figure 2 This is a comparison of the morphologies of the traditional carbon-coated metal substrate and the composite-coated metal substrate after 500h+0.8V constant potential polarization.
[0027] Figure 3 The contact resistance is compared after 500h+0.8V constant potential polarization to simulate the fuel cell environment. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Since the steps and methods used are the same as those in Examples 1-3, in order to avoid redundancy, the present invention describes a preferred embodiment, but the present invention is not limited thereto, but can also be specifically implemented in other ways within the scope of the technical solution defined in the attached claims.
[0030] The present invention provides a method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate, comprising the following steps:
[0031] Step 1: Forming a Ti layer on a metal substrate
[0032] The cleaned metal substrate is placed in a vacuum container, and the vacuum degree of the vacuum container is adjusted to 6×10 -4 Pa, introducing argon gas, maintaining the vacuum degree at 0.1-1.0 Pa, and performing physical vapor deposition coating treatment to form a Ti layer as a base bonding layer on the surface of the metal substrate;
[0033] Step 2: Forming a defective TiO layer on a metal substrate
[0034] A mixed atmosphere consisting of argon and oxygen is introduced into the environment of the metal substrate containing the Ti layer, the vacuum degree of the vacuum container is maintained at 0.1-1.0 Pa, and then a physical vapor deposition coating process is performed to form a defective TiO layer on the surface of the metal substrate;
[0035] Step 3: Forming a Ti-OC bonding composite coating on a metal substrate
[0036] The metal substrate containing the TiO layer is placed in a vacuum furnace, and the vacuum degree of the vacuum furnace is adjusted to 3×10 -3 Pa~5×10 -3 Pa, a carbon source gas and a carrier gas are introduced, and then a discharge plasma treatment is performed to excite and crack the carbon source gas to form a high-activity carbon source group, and the high-activity carbon source group reacts with TiO to form a black coating on the surface of the metal substrate, thereby obtaining a metal substrate with a Ti-TiO-C bonded composite coating.
[0037] The present invention forms a titanium monoxide layer (TiO) with defects on the surface of the metal substrate, and then uses a physical vapor deposition method to dope carbon elements to form Ti-OC bonds in the TiO layer, thereby greatly enhancing the bonding force between the plated carbon layer and the metal substrate, thereby obtaining an ultra-long service life. The process is simple and efficient, environmentally friendly and non-toxic, and can greatly improve the service life of the metal substrate in a hydrogen fuel cell environment.
[0038] Specifically, the carrier gas is argon, and the flow ratio of the carbon source gas to the carrier gas is 1:2. This is because the flow ratio of the carbon source gas to the carrier gas is 1:2, which can ensure both the intensity of plasma ionization and sufficient carbon source for reaction.
[0039] Specifically, the flow ratio of argon gas to oxygen gas is 1:1, because the flow ratio of argon gas to oxygen gas of 1:1 can not only ensure the formation of the TiO layer, but also ensure the intensity of the ignition discharge.
[0040] Specifically, the physical vapor deposition temperature for forming a Ti layer on the surface of the metal substrate is 200°C to 600°C, the physical vapor deposition power source power is 250W to 350W, the physical vapor deposition time is 200s to 600s, and the target material is a pure titanium target. The physical vapor deposition treatment temperature for forming a defective titanium oxide layer on the surface of the metal substrate is 200°C to 600°C, the physical vapor deposition power source power is 250W to 350W, the physical vapor deposition time is 500s to 2000s, and the target material is a pure titanium target. During the discharge plasma treatment, a plasma generator is used for discharge, the plasma generator power is set to 400W to 500W, the heating temperature is 500 to 700°C, and the treatment time is 1800s to 5500s.
[0041] The physical vapor deposition temperature for forming the Ti layer on the surface of the metal substrate is 200°C to 600°C. When the temperature is too high, the metal substrate material on which the Ti layer is formed on the surface will be deformed. The physical vapor deposition power is set to 250W to 350W, and the physical vapor deposition time is set to 200s to 600s, which are setting parameters that can ensure that the Ti layer on the surface of the metal substrate is formed normally.
[0042] The physical vapor deposition processing temperature of the titanium oxide layer with defects formed on the surface of the metal substrate is 200℃~600℃. When the temperature is too high, the metal substrate material with the titanium oxide layer formed on the surface will be deformed. When the temperature is too low, it will be difficult to prepare the metal substrate material with the titanium oxide layer formed on the surface. The physical vapor deposition power supply power is set to 250W~350W, and the physical vapor deposition time is 200s~600s. These are the setting parameters that can ensure the normal formation of the Ti layer on the surface of the metal substrate.
[0043] The heating temperature of the discharge plasma is 500-700°C, the power of the plasma generator is set to 400W-500W, and the processing time is 1800s-5500s. Setting such temperature, power and processing time is to ensure that the discharge plasma treatment proceeds normally and ensures that a black coating is formed on the surface of the metal substrate.
[0044] Specifically, after the heating is completed, the metal substrate with the Ti—OC bonding composite coating is cooled by nitrogen, because the nitrogen gas flow can take away the heat of the metal substrate with the Ti—OC bonding composite coating more quickly.
[0045] Specifically, the cleaned metal substrate is obtained by the following steps:
[0046] The metal substrate is placed in anhydrous ethanol cleaning liquid for ultrasonic cleaning to remove surface contaminants, and then placed in deionized water for surface cleaning again. The above sequence is repeated for several cycles until there is no visible contaminant on the surface of the metal substrate. The purpose of this is to ensure that the surface of the metal substrate is clean, which is conducive to the normal progress of the subsequent surface coating reaction.
[0047] Specifically, the ultrasonic power of ultrasonic cleaning is 200W to 400W, the ultrasonic cleaning time in anhydrous ethanol is 5 to 10 minutes, and the ultrasonic cleaning time in deionized water is 3 to 6 minutes. The ultrasonic cleaning power and cleaning time are set to fully ensure the cleanliness of the metal substrate surface.
[0048] Specifically, the metal substrate with the Ti-OC bonding composite coating will also be washed to remove floating carbon in a cleaning solution, and the cleaning solution is a citric acid aqueous solution, wherein the citric acid content is 5% to 15%.
[0049] Specifically, the metal matrix is stainless steel or metal titanium.
[0050] The inventors found that the compatibility of metal lattices such as stainless steel and titanium with the non-metallic lattices of carbon is poor, and the film-base bonding of direct carbon coatings is often poor. The commonly used method is to form a transition layer by Ti / C co-plating to enhance the bonding between the subsequent carbon coating and the substrate, but the degree of bonding that can be improved by this method is relatively limited, and it is not possible to increase the film-base bonding to a level sufficient to support tens of thousands of hours of service. However, the lattice matching degree of titanium oxide and metallic titanium is extremely high, and the bonding strength is very ideal. Subsequently, carbon elements are doped into the defective TiO layer by element doping, and the carbon elements exist in the coating in the form of Ti-OC chemical bonding, avoiding the problem of poor bonding caused by simple physical deposition between traditional non-metals and metals, thereby achieving the purpose of ultra-long service in a hydrogen fuel cell environment.
[0051] In order to ensure that the carbon source gas can generate sufficient carbon source ion groups during the discharge plasma treatment process, the present invention preferably uses any one of CH4, C2H2 or C3H6 as the carbon source gas, wherein CH4 can form Ti-OC bonds in the TiO layer better and faster due to its short carbon chain, and other carbon sources can also achieve the above-mentioned reaction of forming Ti-OC bonds in the TiO layer, but the carbon chain is longer than CH4, and the difficulty of forming Ti-OC bonds in the TiO layer is greater than that of CH4. This is why the embodiment of the present invention uses CH4 as the most preferred embodiment of the carbon source, but the present invention is not limited to this. Other carbon source gases and liquids can be used according to the treatment method for forming a long-life conductive and corrosion-resistant coating on the surface of a metal substrate given by the present invention to finally obtain a Ti-TiO-C composite coating, which is not described one by one here.
[0052] The technical solution of the present invention is further illustrated below in the form of specific examples.
[0053] Example 1
[0054] This embodiment provides a method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate, comprising the following steps:
[0055] The metal substrate of this embodiment is selected as titanium, and the composite coating is deposited on the metal substrate. The specific steps are as follows:
[0056] Step 1: Forming a Ti layer on a metal substrate
[0057] (1) The selected metal substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min and 5 min, respectively. The metal substrate was purged with clean nitrogen before use and stored in a vacuum drying oven for later use;
[0058] (2) Place the sample in a vacuum container and evacuate the vacuum container to 6×10 -4 Pa. Argon gas was introduced to keep the vacuum degree of the chamber at 0.3 Pa, the temperature was 200°C, the power was 300W, the target material used was pure titanium target, the physical vapor deposition time was 500s, and after the treatment, a pure Ti base layer with metallic luster was obtained.
[0059] Step 2: Forming a defective TiO layer on a metal substrate
[0060] Oxygen and argon were introduced into the vacuum container where the metal substrate with pure Ti as the bottom layer was located, with a ratio of 1:1. The vacuum degree of the cavity was maintained at 0.3 Pa, the temperature was 200°C, the power was 300 W, the target material was pure titanium target, and the physical vapor deposition time was 1000 s. After the treatment, a dark yellow TiO coating was obtained on the surface of the sample.
[0061] Step 3: Forming a Ti-TiO-C composite coating on a metal substrate
[0062] The TiO-coated metal substrate was transferred into a vacuum furnace and the vacuum was first drawn to 4 × 10 -3 Pa, then hydrogen and methane are introduced in a ratio of 2:1, the vacuum tube is heated to 500°C, the plasma generator is turned on, the plasma generator power is set to 400W, the gas is ionized and produces an obvious glow, the processing time is 3600s; after the treatment is completed, a black coating is produced on the surface of the metal substrate.
[0063] After the heating is completed, 60 sccm nitrogen is introduced and the temperature is lowered. After the furnace is cooled, the sample is taken out to obtain a metal substrate with a Ti-OC bonding composite coating.
[0064] Example 2
[0065] The metal substrate of this embodiment is selected as titanium, and the composite coating is deposited on the metal substrate. The specific steps are as follows:
[0066] Step 1: Forming a Ti layer on a metal substrate
[0067] (1) The selected metal substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min and 5 min, respectively. The metal substrate was purged with clean nitrogen before use and stored in a vacuum drying oven for later use;
[0068] (2) Place the sample in a vacuum container and evacuate the vacuum container to 5×10 -4 Pa. Argon gas was introduced to keep the vacuum degree of the chamber at 0.35 Pa, the temperature was 250°C, the power was 350W, the target material used was pure titanium target, the physical vapor deposition time was 200s, and after the treatment, a pure Ti base layer with metallic luster was obtained.
[0069] Step 2: Forming a defective TiO layer on a metal substrate
[0070] Oxygen and argon were introduced into the vacuum container where the pure Ti-based metal substrate was located, with a ratio of 1:1. The vacuum degree of the cavity was maintained at 0.5 Pa, the temperature was 250°C, the power was 350 W, the target material was a pure titanium target, and the physical vapor deposition time was 1500 s. After the treatment, a dark yellow TiO coating was obtained on the surface of the sample.
[0071] Step 3: Forming a Ti-TiO-C composite coating on a metal substrate
[0072] The TiO-coated metal substrate was transferred into a vacuum furnace and the vacuum was first drawn to 5×10 -3Pa, then hydrogen and methane are introduced in a ratio of 2:1, the vacuum tube is heated to 600°C, the plasma generator is turned on, the plasma generator power is set to 420W, the gas is ionized and produces an obvious glow, the processing time is 1800s; after the treatment is completed, a black coating is produced on the surface of the metal substrate.
[0073] After the heating is completed, 80 sccm nitrogen is introduced and the temperature is lowered. After the furnace is cooled, the sample is taken out to obtain a metal substrate with a Ti-OC bonding composite coating.
[0074] Example 3
[0075] The metal substrate of this embodiment is selected as 361L stainless steel, and the composite coating is deposited on the metal substrate. The specific steps are as follows:
[0076] Step 1: Forming a Ti layer on a metal substrate
[0077] (1) The selected metal substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min and 5 min, respectively. The metal substrate was purged with clean nitrogen before use and stored in a vacuum drying oven for later use;
[0078] (2) Place the sample in a vacuum container and evacuate the vacuum container to 3×10 -4 Pa. Argon gas was introduced to keep the vacuum degree of the chamber at 0.31 Pa, the temperature was 300°C, the power was 250W, the target material used was pure titanium target, the physical vapor deposition time was 400s, and after the treatment, a pure Ti base layer with metallic luster was obtained.
[0079] Step 2: Forming a defective TiO layer on a metal substrate
[0080] Oxygen and argon were introduced into the vacuum container where the metal substrate with pure Ti as the bottom layer was located, with a ratio of 1:1. The vacuum degree of the cavity was maintained at 0.1 Pa, the temperature was 300°C, the power was 250 W, the target material was pure titanium target, and the physical vapor deposition time was 2000 s. After the treatment, a dark yellow TiO coating was obtained on the surface of the sample.
[0081] Step 3: Forming a Ti-TiO-C composite coating on a metal substrate
[0082] The TiO-coated metal substrate was transferred into a vacuum furnace and the vacuum was first drawn to 3×10 -3 Pa, then hydrogen and methane are introduced in a ratio of 2:1, the vacuum tube is heated to 700°C, the plasma generator is turned on, the plasma generator power is set to 450W, the gas is ionized and produces an obvious glow, the processing time is 3600s; after the treatment is completed, a black coating is produced on the surface of the metal substrate.
[0083] After the heating is completed, 100 sccm nitrogen is introduced and the temperature is lowered. After the furnace is cooled, the sample is taken out to obtain a metal substrate with a Ti-OC bonding composite coating.
[0084] Comparative Example 1
[0085] The metal substrate of this embodiment is selected as titanium, and a conventional carbon coating is deposited on the metal substrate. The specific steps are as follows:
[0086] Step 1: Forming a Ti layer on a metal substrate
[0087] (1) The selected metal substrate was ultrasonically cleaned with anhydrous ethanol and deionized water for 10 min and 5 min, respectively. The metal substrate was purged with clean nitrogen before use and stored in a vacuum drying oven for later use;
[0088] (2) Place the sample in a vacuum container and evacuate the vacuum container to 6×10 -4 Pa. Argon gas was introduced to keep the vacuum degree of the chamber at 0.3 Pa, the temperature was 220°C, the power was 300W, the target material used was pure titanium target, the physical vapor deposition time was 300s, and after the treatment, a pure Ti base layer with metallic luster was obtained.
[0089] Step 2: Forming a Ti / C mixed coating on a metal substrate
[0090] Argon gas was introduced into the vacuum container where the metal substrate with the pure Ti base layer was located, the vacuum degree of the cavity was maintained at 0.3 Pa, the temperature was 220°C, the power supply was 300 W, the target materials used were pure titanium target and graphite target, the physical vapor deposition time was 300 s, and after the treatment, a light gray mixed coating was obtained on the surface of the sample.
[0091] Step 3: Forming a carbon coating on a metal substrate
[0092] Argon gas was introduced into the vacuum container where the metal substrate with the mixed coating was located, the vacuum degree of the cavity was maintained at 1Pa, the temperature was 250°C, the power supply was 350W, the target material used was a graphite target, and the physical vapor deposition time was 1200s. After the treatment, a gray-black carbon coating was obtained on the surface of the sample.
[0093] Experimental Section
[0094] (I) Corrosion resistance test
[0095] The present invention takes Examples 1 to 3 and Comparative Example 1 as examples, and tests the potentiodynamic polarization thereof in a simulated fuel cell environment, respectively, and the test method is as follows:
[0096] Polarization curve tests were conducted in a simulated environment consisting of 0.5 mM H2S04 and 5 ppm HF. The test samples were metal substrates with Ti-OC bonding composite coatings and metal substrates with traditional carbon coatings.
[0097] The corrosion current density of the metal substrate with Ti-OC bonding composite coating in the simulated fuel cell environment given in Example 2 is 0.01 μA / cm 2 The corrosion current density of the metal substrate with a traditional carbon coating in the simulated fuel cell environment given in Comparative Example 1 is 0.3 μA / cm 2 , it is found by comparison that the corrosion current density of Example 1 is reduced by more than 10 times compared with the corrosion current density of Comparative Example 1;
[0098] The corrosion current density of the metal substrate with the Ti-OC bonding composite coating in the simulated fuel cell environment given in Example 3 is 0.03 μA / cm 2 The corrosion current density of the metal substrate with a traditional carbon coating in the simulated fuel cell environment given in Comparative Example 1 is 0.3 μA / cm 2 , it was found by comparison that the corrosion current density of Example 1 was reduced by nearly 10 times compared with the corrosion current density of Comparative Example 1.
[0099] like Figure 1 As shown in the figure, the corrosion current density of the metal substrate with the Ti-OC bonding composite coating in the simulated fuel cell environment given in Example 1 is 0.004 μA / cm 2 The corrosion current density of the metal substrate with a traditional carbon coating in the simulated fuel cell environment given in Comparative Example 1 is 0.3 μA / cm 2 By comparison, it was found that the corrosion current density of Example 1 was nearly 100 times lower than that of Comparative Example 1; the Raman test results showed that the I(D) / I(G) value of the carbon-rich layer on the surface of the composite coating was 1.83, while the I(D) / I(G) value of the traditional carbon coating was 2.25. The smaller the ratio, the fewer carbon crystal defects. This result shows that the carbon-rich layer on the surface of the composite coating has fewer defects than the traditional carbon coating, the coating is denser, and the corrosion resistance is better, thereby greatly reducing the corrosion current density.
[0100] (II) Morphology test
[0101] In the present invention, Example 1 and Comparative Example 1 are taken as examples. The metal substrate with a Ti-OC bonding composite coating given in Example 1 and the metal substrate with a traditional carbon coating given in Comparative Example 1 are respectively subjected to constant potential polarization at 80°C, 0.5 mM sulfuric acid + 5 ppm hydrofluoric acid for 500 h and 0.8 V. The morphologies of the metal substrates in Example 1 and Comparative Example 1 are respectively measured. By comparing the macroscopic morphologies of the coating surfaces, it is found that the surface coating of the metal substrate with a traditional carbon coating given in Comparative Example 1 has completely fallen off and severe signs of oxidation corrosion have occurred.
[0102] (III) Contact resistance test
[0103] The present invention takes Example 1 and Comparative Example 1 as examples, and tests the contact resistance of the metal substrate with the Ti-OC bonding composite coating given in Example 1 and the metal substrate with the traditional carbon coating given in Comparative Example 1, respectively, and summarizes the test results of Example 1 and Comparative Example 1, as shown in FIG. Figure 3 The results are as follows:
[0104] After accelerated corrosion, the contact resistance of the metal substrate with a conventional carbon coating given in Comparative Example 1 is as high as 10000 mΩ·cm 2 The above; however, the surface of the metal substrate with the Ti-OC bonding composite coating given in Example 1 only undergoes slight oxidation corrosion, and the contact resistance of the metal substrate with the Ti-OC bonding composite coating given in Example 1 is only 150mΩ·cm 2 .
[0105] The contact resistance test results show that after the accelerated corrosion test, the contact resistance of the composite coating obtained by the method is at least 100 times lower than that of the ordinary carbon coating (such as Figure 3 As shown in the figure, the expected service life of the composite coating is much higher than that of the traditional carbon coating. The composite coating replaces the physical deposition bonding of the traditional coating by Ti-OC chemical bonding, which greatly improves the bonding strength between the carbon-rich layer and the substrate. In long-term service, the traditional carbon coating often completely falls off, resulting in obvious oxidation corrosion of the substrate, causing a significant increase in contact resistance. However, the carbon-rich layer of the composite coating basically does not completely fall off in long-term service, and only a small area of the substrate shows traces of oxidation corrosion, so the increase in contact resistance is greatly reduced.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate, characterized in that: The steps include: forming a Ti layer as a base bonding layer on the surface of the metal substrate; A mixed atmosphere consisting of argon and oxygen is introduced into the environment of the metal substrate containing the Ti layer, and the vacuum degree is maintained at 0.1-1.0 Pa, and then a physical vapor deposition coating process is performed to form a defective TiO layer on the surface of the metal substrate; The metal substrate containing the TiO layer is placed in a vacuum of 3×10 -3 Pa~5×10 -3 Pa, a carbon source gas and a carrier gas are introduced, and then a discharge plasma treatment is performed to excite and crack the carbon source gas to form a high-activity carbon source group, and then the generated high-activity carbon source group reacts with TiO to form a black coating on the surface of the metal substrate, thereby obtaining a metal substrate with a Ti-OC bonding composite coating.
2. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The Ti layer as the base bonding layer is formed on the surface of the metal substrate by placing the cleaned metal substrate in a vacuum of 6×10 -4 In a vacuum environment below Pa, argon gas is introduced, and the vacuum degree is maintained at 0.1-1.0 Pa, and physical vapor deposition coating treatment is performed to obtain the film.
3. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The carbon source gas includes but is not limited to any one of CH4, C2H2 or C3H6.
4. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The carrier gas is argon, and the flow ratio of the carbon source gas to the carrier gas is 1:
2.
5. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The flow ratio of argon gas to oxygen gas is 1:
1.
6. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The physical vapor deposition temperature for forming a Ti layer on the surface of the metal substrate is 200°C to 600°C, the power of the physical vapor deposition power source is 250W to 350W, the physical vapor deposition time is 200s to 600s, and the target material is a pure titanium target. The physical vapor deposition treatment temperature for forming a defective titanium monoxide layer on the surface of the metal substrate is 200°C to 600°C, the power of the physical vapor deposition power source is 250W to 350W, the physical vapor deposition time is 500s to 2000s, and the target material is a pure titanium target. During the discharge plasma treatment, a plasma generator is used for discharge, the power of the plasma generator is set to 400W to 500W, the heating temperature is 500 to 700°C, and the treatment time is 1800s to 5500s.
7. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The cleaned metal substrate is obtained by the following steps: The metal substrate is placed in anhydrous ethanol cleaning solution for ultrasonic cleaning to remove surface contaminants, and then placed in deionized water for surface cleaning again. The above sequence of cleaning is repeated several times until there is no contaminant visible to the naked eye on the surface of the metal substrate.
8. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 7, characterized in that: The ultrasonic power of ultrasonic cleaning is 300W to 500W, the ultrasonic cleaning time in anhydrous ethanol is 5 to 10 minutes, and the ultrasonic cleaning time in deionized water is 3 to 6 minutes.
9. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The metal substrate with the Ti-OC bonding composite coating can also be washed to remove floating carbon in a cleaning solution, wherein the cleaning solution is a citric acid aqueous solution, wherein the citric acid content is 5% to 15%.
10. A method for forming a long-life conductive corrosion-resistant coating on the surface of a metal substrate as claimed in claim 1, characterized in that: The metal matrix is stainless steel or titanium.