Platinum modified aluminide coating resistant to high-temperature molten salt corrosion as well as preparation method and application of platinum modified aluminide coating
Through the platinum modified aluminum coating, the service life of nickel-based high-temperature alloy in a high-temperature molten salt corrosion environment is solved, and efficient protection of nickel-based high-temperature alloy is achieved, which extends its service life and improves thermal cycling performance.
Patent Information
- Application Number
- CN202410836167.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-01
AI Technical Summary
Nickel-based high-temperature alloys are susceptible to high-temperature molten salt corrosion in marine environments, resulting in the peeling and cracking of turbine blades. The prior art is difficult to effectively protect its mechanical properties in a high-temperature molten salt thermal corrosion environment.
Using platinum modified aluminide coating, platinum is platinum platinum and vacuum diffusion annealing, combined with solid powder embedding and aluminium penetration technology, PtAl2 and (Ni,Pt)Al phase coatings with high aluminium content and platinum elements are formed to enhance the balance. Protection capability of nickel-based high-temperature alloys.
It significantly improves the service life and thermal cycling performance of nickel-based high-temperature alloys in high-temperature molten salt corrosion environments, slows down the decline in the mechanical properties of the matrix, prevents the corrosion failure of molten salt entering the matrix, and extends the service life of the coating.
Smart Images

Figure CN118880326A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of high temperature molten salt corrosion protection for gas turbine engine turbine blades, and in particular to a platinum-modified aluminide coating resistant to high temperature molten salt corrosion, and a preparation method and application thereof. Background Art
[0002] As the speed and load-carrying capacity of ships and warships continue to increase, gas turbines are gradually replacing traditional steam turbines and less efficient diesel engines due to their advantages of high power and small size. Because nickel-based high-temperature alloys have high endurance strength, fatigue strength and long-lasting plasticity, and their structure and mechanical properties are highly stable at the operating temperature of gas turbines (900°C), nickel-based high-temperature alloys are currently used as the main structural material for hot end components such as turbine blades, combustion chambers, and turbine disks in gas turbines.
[0003] When the marine gas turbine operates in the marine environment, the Na + , Cl - Sulfur impurities in the fuel will enter the engine, and mixed salts (mainly Na2SO4 and NaCl) will be deposited on the surface of the turbine blades. Although nickel-based high-temperature alloys have good high-temperature oxidation resistance, in order to maintain high mechanical properties, the alloys have low Al and Cr contents with good corrosion resistance, which makes the alloys prone to spalling and cracking. Therefore, a single nickel-based high-temperature alloy cannot serve for a long time in a high-temperature molten salt thermal corrosion environment.
[0004] In order to maintain the excellent mechanical properties of nickel-based high-temperature alloys and improve their resistance to high-temperature molten salt corrosion, it is necessary to prepare a protective coating on the surface of nickel-based high-temperature alloys to increase the service life of the blades. Although Cr and Al can form a dense oxide film to protect nickel-based high-temperature alloys, Cr is prone to form volatile substances as corrosion products in a high-temperature molten salt corrosion environment and does not have a high protective ability. A single Al-infiltrated coating is extremely easy to interdiffuse with the matrix elements in a high-temperature molten salt corrosion environment, resulting in wrinkling and peeling of the oxide film. Summary of the invention
[0005] In order to improve the ability of nickel-based high-temperature alloys to resist molten salt corrosion at high temperatures, the purpose of the present invention is to provide a platinum-modified aluminide coating resistant to high-temperature molten salt corrosion and its preparation method and application. The present invention uses Pt to modify the traditional Al-infiltrated coating to enhance the ability of gas turbine blades to resist molten salt corrosion. The addition of Pt can prevent the refractory elements in the nickel-based high-temperature alloy from diffusing to the outside through the Al2O3 film, slow down the rate of decline in the mechanical properties of the substrate, and enhance the bonding force between the Al2O3 film and the substrate, reduce the corrosion failure caused by the molten salt entering the interior of the substrate, and thus extend the service life of the Al-infiltrated coating. In addition, the platinum-modified aluminide coating of the present invention has a sufficient aluminum content. At the same time, because the surface contains a high level of platinum, the mutual diffusion of elements between the substrate and the coating can be suppressed, and the service life of the nickel-based high-temperature alloy in a high-temperature molten salt corrosion environment can be greatly improved.
[0006] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:
[0007] A method for preparing a platinum-modified aluminide coating resistant to high-temperature molten salt corrosion, first electroplating platinum on the surface of an alloy, then performing vacuum diffusion annealing, and then performing solid powder embedding and aluminum infiltration on the alloy to obtain a coating resistant to high-temperature molten salt corrosion; the method comprises the following steps:
[0008] Step 1: Substrate surface pretreatment
[0009] The surface of the base alloy is polished with 180# coarse sandpaper until the alloy surface presents a silvery white metallic luster, followed by sandblasting, and then ultrasonic cleaning in anhydrous ethanol for degreasing; after cleaning, the base alloy is taken out and activated with a mixed acid solution, and finally the alloy surface is cleaned with deionized water until no acid remains;
[0010] Step 2: Prepare a platinum electroplating solution and prepare a platinum layer on the substrate surface by electroplating
[0011] Prepare electroplating solution, suspend the pretreated base alloy in the heated electroplating solution, use the titanium plate or platinum-coated titanium mesh as the anode, use the alloy base as the cathode, turn on the magnetic stirrer, turn on the power switch, and perform electroplating;
[0012] Step 3: After the electroplating is completed, vacuum diffusion annealing is performed to reduce the platinum concentration on the substrate surface, so that the platinum element diffuses downward into the substrate and enhances the bonding force between the coating and the substrate;
[0013] Step 4, performing "two-step" solid powder embedding and aluminizing on the sample after step 3.
[0014] Preferably, the volume ratio of hydrochloric acid to nitric acid in the mixed acid solution in step 1 is 1:3, and the activation treatment is performed for 1-5 minutes.
[0015] Preferably, the preparation method of the electroplating solution in step 2 is to take 5-8 g / L of dinitrosodiammineplatinum, 10-40 g / L of aminosulfonic acid, 0.002-0.01 g / L of sodium dodecyl sulfate, 5-10 g / L of sodium nitrite, 40-60 g / L of ammonium nitrate, and the balance is deionized water; add the raw materials taken into a beaker, stir and dissolve them, then dissolve them by ultrasound for 30 minutes, and adjust the pH value to 2-6 with ammonia water.
[0016] Preferably, the temperature of the electroplating solution in step 2 is 60-80°C and the current density is 4-8A / dm 2 The electroplating time is 20min-60min, the area ratio of the anode to the cathode is 1-3:1, the distance between the anode and the cathode is 10-20cm, the magnetic stirrer is turned on, the power switch is turned on for electroplating, and the thickness of the platinum layer formed by electroplating is 3-8μm.
[0017] Preferably, during the vacuum diffusion annealing in step 3, the vacuum degree in the vacuum tube furnace is less than 5×10 -3 Pa, temperature is 700-1000℃, heating rate is less than 10℃ / min, and holding time is 1-3h.
[0018] Preferably, the steps of solid powder embedding aluminizing in step 4 are as follows:
[0019] (1) Prepare aluminizing agent
[0020] The aluminizing agent comprises the following components by mass fraction: 40%-50% iron aluminum powder, 3-6% ammonium chloride, and the balance is aluminum oxide powder, wherein the aluminum content in the iron aluminum powder is 50%;
[0021] (2) Two-step heating and aluminizing
[0022] First, wrap the platinum-plated annealed alloy in a work box of aluminizing agent, and weld and seal the work box; then place the work box in a resistance furnace and start heating it. After heating to 450°C, keep it warm for 1 hour, then continue to heat it to 1000°C and keep it warm for 4-6 hours. When the furnace cools to 400°C, take it out and cool it to room temperature. The whole heating / cooling rate is less than 5°C / min.
[0023] Preferably, after step 4, the method further includes continuing vacuum heat treatment at 1000-1100° C. and keeping the temperature for 2-4 hours to effectively increase the proportion of the (Ni, Pt)Al phase.
[0024] The platinum-modified aluminide coating prepared by the above preparation method forms a coating having a dual phase of PtAl2 and (Ni,Pt)Al on the surface of the base alloy, wherein the aluminum content is 40-50%, the platinum content is 20-30%, the nickel content is 10-20%, and the coating thickness is 40-80μm.
[0025] Preferably, after 100 hours of high-temperature molten salt thermal corrosion, the platinum-modified aluminide coating is well bonded to the substrate, the surface is covered with a dense oxide film and no weight loss occurs; the obtained platinum-modified aluminide coating not only improves the high-temperature molten salt corrosion resistance of the nickel-based high-temperature alloy and prolongs its service life, but also has excellent thermal cycling performance and reliability.
[0026] The above-mentioned platinum-modified aluminide coating is used in the field of protection of hot end components of gas turbines or in the protective coating of turbine blades of aircraft engines.
[0027] The platinum-modified aluminide coating of the present invention has a simple preparation process, and the production technology system of electroplating and aluminizing involved is mature and complete, and has a wide range of applications. The platinum-modified aluminide coating prepared by the present invention not only improves the high-temperature molten salt corrosion resistance of nickel-based high-temperature alloys and prolongs the service life, but also has excellent anti-stripping and functional stability, excellent thermal cycle performance and reliability. After 100 hours of high-temperature molten salt thermal corrosion, the coating is well combined with the substrate, the surface is still covered with a dense oxide film, and no weight loss occurs. Therefore, the coating of the present invention can not only be used in the field of protection of hot end components of gas turbines in ships, but also can be used as a protective coating for components such as aircraft engine turbine blades to improve their corrosion resistance and high-temperature oxidation resistance.
[0028] Beneficial Effects
[0029] Compared with the prior art, the platinum-modified aluminide coating resistant to high-temperature molten salt corrosion and its preparation method and application in the present invention have the following advantages:
[0030] 1. The electroplating solution of the present invention can not only prepare a platinum layer with a thickness of 3-8 μm on the surface of the nickel-based high-temperature alloy, but also the surface of the platinum layer prepared by the electroplating solution has no large pores and burrs and has high stability. It only needs to supplement the main salt concentration while ensuring the pH of the solution.
[0031] 2. The electroplating solution of the present invention uses aminosulfonic acid, sodium dodecyl sulfate, sodium nitrite and ammonium nitrate as auxiliary salts. By controlling the concentration of the auxiliary salts, the electroplating solution can reduce the phenomenon of decreased electroplating quality due to changes in component content, and the electroplating solution is non-toxic and harmless and does not pollute the environment.
[0032] 3. The surface aluminum content of the platinum-modified aluminide coating of the present invention is above 40%, and the main phases PtAl2 and (Ni, Pt)Al phases are both resistant to high-temperature oxidation and corrosion. In particular, PtAl2, as a phase with a high melting point and excellent thermal stability, can resist high-temperature molten salt thermal corrosion for a long time.
[0033] 4. The solid powder embedding aluminizing technology adopted in the present invention can prepare a platinum-modified aluminide coating with a thickness of 40-80 μm on the surface of the nickel-based high-temperature alloy after platinum plating using a two-step method. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The XRD results of Example 1-3 after platinum plating;
[0035] Figure 2 The surface morphology, cross-sectional morphology and elemental analysis of Example 1 after platinum plating, (a), (b), (c) are all surfaces, (d), (e), (f) are all cross-sectional views;
[0036] Figure 3 (a) and Figure 3 (b) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 1 before corrosion;
[0037] Figure 3 (c) and Figure 3 (d) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 1 after being subjected to high-temperature molten salt hot corrosion for 100 h;
[0038] Figure 4 The surface morphology, cross-sectional morphology and elemental analysis of Example 2 after platinum plating, (a), (b), (c) are all surfaces, (d), (e), (f) are all cross-sectional views;
[0039] Figure 5 (a) and Figure 5 (b) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 2 before corrosion;
[0040] Figure 5 (c) and Figure 5 (d) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 2 after being subjected to high-temperature molten salt hot corrosion for 100 h;
[0041] Figure 6 The surface morphology, cross-sectional morphology and elemental analysis of Example 3 after platinum plating, (a), (b), (c) are all surfaces, (d), (e), (f) are all cross-sectional views;
[0042] Figure 7 (a) and Figure 7 (b) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 3 before corrosion;
[0043] Figure 7 (c) and Figure 7 (d) are the surface and cross-sectional morphologies of the platinum-modified aluminide coating of Example 3 after being subjected to high-temperature molten salt thermal corrosion for 100 h.
[0044] Figure 8 The XRD results of the platinum-modified aluminide coating prepared in Example 1-3 after being subjected to high-temperature molten salt hot corrosion for 100 hours;
[0045] Fig. 9 The surface morphology after platinum plating in Comparative Example 1 is shown, wherein (a) is a morphology of the platinum-plated peeling area; (b) is a morphology of the platinum-plated flat area;
[0046] Fig.10 The surface (a) and cross-sectional morphology (b) of the platinum-modified aluminide coating of comparative example 2 after high-temperature molten salt thermal corrosion for 100 hours. DETAILED DESCRIPTION
[0047] The present invention is described in detail below in combination with specific embodiments through the accompanying drawings.
[0048] The base alloy of each embodiment of the present invention is GH4169 alloy, and the chemical composition (mass fraction) is: Cr: 15.8%, Fe: 14.1%, Mo: 2.8%, Ti: 0.84%, Al: 0.47%, C: 0.04%, and Ni is the balance.
[0049] The GH4169 alloy sheet was cut into small metal blocks of 20×15×3 mm in size, and a small hole with a diameter of 2 mm was punched in the upper left corner so that it could be subsequently suspended in the electroplating solution for electroplating.
[0050] Example 1
[0051] (1) Pretreatment of the substrate: Use #180 coarse sandpaper to polish the surface of the GH4169 alloy until the alloy surface presents a silvery white metallic luster, then perform sandblasting (60psi), and then place it in anhydrous ethanol for ultrasonic cleaning for 20 minutes to remove oil. After cleaning, take it out and use a mixed acid (hydrochloric acid: nitric acid, volume ratio 1:3) solution for activation treatment for 2 minutes. After taking it out, rinse the alloy surface with deionized water until there is no residual acid solution, and place it in an 80℃ drying oven for 4 hours.
[0052] (2) The raw materials of the electroplating solution used are shown in the table below. They were added into deionized water, heated at 60°C and stirred until dissolved, and then ultrasonically diffused for 30 minutes to make the solution ions diffuse evenly.
[0053] The formula of the plating solution is as follows:
[0054] raw material Content (g / L) Dinitrosodiammineplatinum (calculated as platinum) 5 Sulfamic acid 20 Sodium Lauryl Sulfate 0.004 Sodium Nitrite 6 Ammonium Nitrate 45 Deionized water Add to 1L
[0055] (3) Specific process of electroplating: put the electroplating solution into the electroplating tank, and then place it in a water bath and heat it to 65°C. Use the platinum-plated titanium mesh as the anode and the GH4169 alloy sample as the cathode. The area ratio of the anode to the cathode is 2:1, and the distance between the anode and the cathode is 10 cm. Use a magnetic stirrer to stir the electroplating solution during the electroplating process to make the ions in the electroplating solution more evenly distributed. The electroplating current is a direct current with an average current density of 5A / dm 2 , pH is 3, electroplating time is 30min, and the XRD results after platinum electroplating are as follows Figure 1 As shown, the surface and cross-sectional morphology of the platinum layer are Figure 2 shown.
[0056] (4) Vacuum diffusion annealing: Place the electroplated sample in a vacuum furnace and evacuate the tube three times, each time for no more than 3 minutes, until the vacuum degree in the tube is less than 5×10 -3 Pa, the temperature was set to 800°C, the heating rate was less than 10°C / min, and the holding time was 2h;
[0057] (5) "Two-stage method" solid powder embedding aluminization: 40% of iron aluminum powder (50% Al) (aluminum source), 4% of ammonium chloride (infiltration promoter) and the remaining alumina powder (inert agent) are mixed and placed in a tooling box, and then the tooling box is welded and sealed. The tooling box is placed in a resistance furnace and heated. After the temperature reaches 450°C, it is kept warm for 1 hour, and then the temperature is continued to rise to 1000°C and kept warm for 4 hours. When the furnace cools to 400°C, it is taken out and cooled to room temperature. The whole heating / cooling rate is less than 5°C / min.
[0058] After the preparation of the platinum-modified aluminide coating, the coating surface is visually smooth without any roughness, and the coating is tightly bonded to the substrate. The surface morphology and cross-sectional morphology of the platinum-modified aluminide coating are shown in Figure 2. Figure 3 As shown, the overall thickness of the coating reaches 73.8 μm.
[0059] The experiment was carried out according to the HB 20401-2016 salt coating hot corrosion test method shown in my country's aviation industry standard. The results are as follows Figure 3 After 100 hours of corrosion, there is no obvious damage on the coating surface, and a dense Al2O3 film is formed. The platinum-modified aluminide coating prepared by the present invention effectively improves the high-temperature molten salt corrosion resistance of the GH4169 alloy.
[0060] Example 2
[0061] (1) Pretreatment of substrate:
[0062] Except that the activation treatment time was changed to 1 min, the rest was the same as step (1) of Example 1.
[0063] (2) The raw materials of the electroplating solution used are shown in the table below. They were added into deionized water, heated at 60°C and stirred until dissolved, and then ultrasonically diffused for 30 minutes to make the solution ions diffuse evenly.
[0064] The formula of the plating solution is as follows:
[0065] raw material Content (g / L) Dinitrosodiammineplatinum (calculated as platinum) 6 Sulfamic acid 25 Sodium Lauryl Sulfate 0.006 Sodium Nitrite 8 Ammonium Nitrate 50 Deionized water Add to 1L
[0066] (3) Specific process of electroplating: put the electroplating solution into the electroplating tank, and then place it in a water bath and heat it to 75°C. Use the titanium plate as the anode and the GH4169 alloy sample as the cathode. The area ratio of the anode to the cathode is 3:1, and the distance between the anode and the cathode is 13 cm. Use a magnetic stirrer to stir the electroplating solution during the electroplating process to make the ions in the electroplating solution more evenly distributed. The electroplating current is a direct current with an average current density of 6A / dm 2 , pH is 4, electroplating time is 20min, and the XRD results after platinum electroplating are as follows Figure 1 As shown, the surface and cross-sectional morphology of the platinum layer are Figure 4 shown.
[0067] (4) Vacuum diffusion annealing: Place the electroplated sample in a vacuum furnace and evacuate the tube three times, each time for no more than 3 minutes, until the vacuum degree in the tube is less than 5×10 -3 Pa, the temperature is set to 900℃, the heating rate is less than 10℃ / min, and the holding time is 1.5h
[0068] (5) "Two-stage method" solid powder embedding aluminization: 45% iron aluminum powder (50% Al), 5% ammonium chloride and the remaining alumina powder are mixed and placed in a tooling box, and then the tooling box is welded and sealed. The tooling box is placed in a resistance furnace and heated. After heating to 450°C, it is kept warm for 1 hour, and then continued to heat to 1000°C and kept warm for 4 hours. When the furnace cools to 400°C, it is taken out and cooled to room temperature. The whole heating / cooling rate is less than 5°C / min.
[0069] After the preparation of the platinum-modified aluminide coating, the surface and cross-sectional morphology after 100 hours of corrosion showed that the coating surface was covered with a dense oxide film, and the element interdiffusion between the coating and the substrate was relatively light. Figure 5 From the cross-sectional morphology, the oxygen element did not reach the surface of the substrate, and the coating was tightly bonded to the substrate, effectively preventing the invasion of molten salt.
[0070] Example 3
[0071] (1) Pretreatment of substrate:
[0072] Except that the activation treatment time was changed to 3 min, the rest was the same as step (1) of Example 1.
[0073] (2) The platinum plating solution used is the plating solution after the main salt concentration is reduced in Example 1 (in this example, electroplating is performed for 3 days, and the sample weight can be weighed. When the sample weight does not change and the sample surface turns black, it means that the main salt concentration is exhausted), the concentration of dinitrosodiammine platinum salt is supplemented to 5 g / L, and the other ingredients are the same as in Example 1.
[0074] The formula of the plating solution is as follows:
[0075] raw material Content (g / L) Dinitrosodiammineplatinum (calculated as platinum) 5 Sulfamic acid 20 Sodium Lauryl Sulfate 0.004 Sodium Nitrite 6 Ammonium Nitrate 45 Deionized water Add to 1L
[0076] (3) Specific process of electroplating: put the electroplating solution into the electroplating tank, and then place it in a water bath and heat it to 80°C. Use the platinum-plated titanium mesh as the anode and the GH4133 alloy sample as the cathode. The area ratio of the anode to the cathode is 2.5:1, and the distance between the anode and the cathode is 15 cm. Use a magnetic stirrer to stir the electroplating solution during the electroplating process to make the ions in the electroplating solution more evenly distributed. The electroplating current is a direct current with an average current density of 8A / dm 2 , pH is 5, electroplating time is 35min, and the XRD results after platinum electroplating are as follows Figure 1 As shown, the surface and cross-sectional morphology of the platinum layer are Figure 6 shown.
[0077] (4) Vacuum diffusion annealing: Place the electroplated sample in a vacuum furnace and evacuate the tube three times, each time for no more than 3 minutes, until the vacuum degree in the tube is less than 5×10 -3 Pa, the temperature was set to 1000°C, the heating rate was less than 10°C / min, and the holding time was 1h.
[0078] (5) "Two-stage method" solid powder embedding aluminization: 50% iron aluminum powder (50% Al), 3% ammonium chloride and the rest of alumina powder are mixed and placed in a tooling box, and then the tooling box is welded and sealed. The tooling box is placed in a resistance furnace and heated. After heating to 450°C, it is kept warm for 1 hour, and then continued to heat to 1000°C and kept warm for 4 hours. When the furnace cools to 400°C, it is taken out and cooled to room temperature. The whole heating / cooling rate is less than 5°C / min.
[0079] This embodiment uses the electroplating solution that is replenished twice after the main salt concentration decreases for electroplating. Figure 6 The platinum plating results show that the platinum layer is dense and still has high surface quality. The surface and cross-sectional morphology of the platinum-modified aluminide coating prepared in Example 3 are as follows: Figure 7 As shown in the figure, the coating thickness is 68.6μm, and there are no obvious pores on the coating surface. The coating surface quality is high. After 100h of molten salt thermal corrosion, there is no obvious damage on the surface. Figure 8The XRD results after 100h of hot corrosion show that the surface is still dense Al2O3 film and PtAl2 phase. Figure 7 The cross-sectional morphology after hot corrosion also shows that there is less TCP precipitation phase and the platinum-modified aluminide coating plays an ideal protective role.
[0080] Comparative Example 1
[0081] When preparing the platinum electroplating solution, only 6 g / L of dinitrosodiammine platinum (calculated as platinum) and 20 g / L of aminosulfonic acid were added, and no other auxiliary salts were added. In addition, the other process parameters were the same as those in Example 1.
[0082] from Fig. 9 The surface morphology of the electroplated platinum shows that the coating surface has obvious peeling phenomenon, and the thickness of the platinum layer is relatively thin, which cannot meet the preparation requirements of the subsequent platinum-modified aluminide coating. The coating prepared by the present invention was subjected to a thermal corrosion test, and the coating began to partially peel off and fail after 60 hours. From the results of scanning electron microscopy, the coating surface is not dense enough and has obvious pores.
[0083] Comparative Example 2
[0084] The electroplating process and vacuum diffusion annealing process parameters are the same as those in Case 1, but the "two-stage method" is not used for embedded aluminizing. Instead, the temperature is directly raised to 1000°C and kept for 4 hours. When the furnace is cooled to 400°C, it is taken out and cooled to room temperature. The whole heating / cooling rate is less than 5°C / min.
[0085] from Fig.10 It can be seen that the surface roughness after corrosion is relatively high, and the thickness of the prepared platinum-aluminum coating is significantly reduced. After 100 hours of high-temperature molten salt thermal corrosion, the overall weight loss is obvious, and the surface oxide film also partially peels off. The ability to resist molten salt thermal corrosion is lower than that of the platinum-modified aluminide coating prepared in Example 1.
[0086] Table 1 Comparison of properties of coatings obtained under different preparation processes
[0087]
[0088] As can be seen from Table 1, the platinum-modified aluminide coating prepared by the present invention not only has a high surface quality, but also can well inhibit the serious element interdiffusion phenomenon between the nickel-aluminum coating and the substrate during high-temperature molten salt thermal corrosion, effectively improving the ability of the nickel-based high-temperature alloy to resist molten salt thermal corrosion, and also points out the direction for further improving the service life of gas turbine blades in the later stage, and has good application prospects.
Claims
1. A method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion, characterized in that: First, platinum is electroplated on the surface of the alloy, and then vacuum diffusion annealing is performed, and then the alloy is solid powder embedded and aluminum is infiltrated to obtain a coating with high temperature molten salt corrosion resistance; the steps include: Step 1: Substrate surface pretreatment The surface of the base alloy is polished with 180# coarse sandpaper until the alloy surface presents a silvery white metallic luster, followed by sandblasting, and then ultrasonic cleaning in anhydrous ethanol for degreasing; after cleaning, the base alloy is taken out and activated with a mixed acid solution, and finally the alloy surface is cleaned with deionized water until no acid remains; Step 2: Prepare a platinum electroplating solution and prepare a platinum layer on the substrate surface by electroplating. Prepare electroplating solution, suspend the pretreated base alloy in the heated electroplating solution, use the titanium plate or platinum-coated titanium mesh as the anode, use the alloy base as the cathode, turn on the magnetic stirrer, turn on the power switch, and perform electroplating; Step 3: After the electroplating is completed, vacuum diffusion annealing is performed to reduce the platinum concentration on the substrate surface, so that the platinum element diffuses downward into the substrate and enhances the bonding strength between the coating and the substrate; Step 4, the sample after step 3 is subjected to "two-step" solid powder embedding and aluminizing.
2. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: In step 1, the volume ratio of hydrochloric acid to nitric acid in the mixed acid solution is 1:3, and the activation treatment is performed for 1-5 minutes.
3. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: The preparation method of the electroplating solution in step 2 is as follows: 5-8 g / L of dinitrodiammineplatinum, 10-40 g / L of aminosulfonic acid, 0.002-0.01 g / L of sodium dodecyl sulfate, 5-10 g / L of sodium nitrite, 40-60 g / L of ammonium nitrate, and the remainder is deionized water; the raw materials are added into a beaker and stirred to dissolve, then ultrasonically dissolved for 30 minutes, and the pH value is adjusted to 2-6 with ammonia water.
4. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: The temperature of the plating solution in step 2 is 60-80°C and the current density is 4-8A / dm 2 The electroplating time is 20min-60min, the area ratio of the anode to the cathode is 1-3:1, the distance between the anode and the cathode is 10-20cm, the magnetic stirrer is turned on, the power switch is turned on for electroplating, and the thickness of the platinum layer formed by electroplating is 3-8μm.
5. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: During the vacuum diffusion annealing in step 3, the vacuum degree in the vacuum tube furnace is less than 5×10 -3 Pa, temperature is 700-1000℃, heating rate is less than 10℃ / min, and holding time is 1-3h.
6. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: The steps of solid powder embedding aluminizing in step 4 are as follows: (1) Prepare aluminizing agent The aluminizing agent comprises the following components by mass fraction: 40%-50% iron aluminum powder, 3-6% ammonium chloride, and the balance is aluminum oxide powder, wherein the aluminum content in the iron aluminum powder is 50%; (2) Two-step heating and aluminizing First, wrap the platinum-plated annealed alloy in a work box of aluminizing agent, and weld and seal the work box; then place the work box in a resistance furnace and start heating it. After heating to 450°C, keep it warm for 1 hour, then continue to heat it to 1000°C and keep it warm for 4-6 hours. When the furnace cools to 400°C, take it out and cool it to room temperature. The whole heating / cooling rate is less than 5°C / min.
7. The method for preparing a platinum-modified aluminide coating resistant to high temperature molten salt corrosion according to claim 1, characterized in that: The method also includes continuing vacuum heat treatment at 1000-1100° C. and keeping the temperature for 2-4 hours after step 4, so as to effectively increase the proportion of the (Ni, Pt)Al phase.
8. The platinum-modified aluminide coating prepared by the preparation method according to claims 1-7, characterized in that: A coating having a dual phase of PtAl2 and (Ni, Pt)Al is formed on the surface of the base alloy, wherein the content of aluminum is 40-50%, the content of platinum is 20-30%, the content of nickel is 10-20%, and the thickness of the coating is 40-80 μm.
9. The platinum-modified aluminide coating according to claim 8, characterized in that After 100 hours of high-temperature molten salt thermal corrosion, the platinum-modified aluminide coating is well bonded to the substrate, the surface is covered with a dense oxide film, and no weight loss occurs.
10. Use of the platinum-modified aluminide coating according to claim 8 in the field of protection of hot end components of gas turbines or protective coating of turbine blades of aircraft engines.
Citation Information
Cited By
High-temperature hot corrosion resistant PtAl coating designed by means of machine learning and preparation method of high-temperature hot corrosion resistant PtAl coating
CN120400656A
Preparation method of PtAl coating
CN121428470A