Synthesis method of single crystal with huge abnormal Hall conductivity at room temperature
By burning and sealing quartz tubes in a vacuum environment and performing high-temperature centrifugation, CaTi3Bi4 single crystal with huge abnormal Hall conductivity in room temperature was prepared, which solved the problem of preparing pure single crystals in the prior art and achieved miniaturization of the device and low power detection capability.
Patent Information
- Application Number
- CN202410919840.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to effectively prepare CaTi3Bi4 single crystals with huge abnormal Hall conductivity in room temperature, limiting its development in low-power electronic devices and sensors.
Ti metal, Ca metal and Bi metal are used as raw materials and flux, and sealed quartz tubes are burned and sealed in a vacuum environment, heated and subjected to high-temperature centrifugation to prepare pure layered CaTi3Bi4 single crystals.
The high purity of CaTi3Bi4 single crystal and huge abnormal Hall conductivity in room temperature are achieved, supporting the miniaturization and high integration of devices, and detecting magnetic field changes at extremely low currents, which promotes the development of low-power electronic devices and sensors.
Smart Images

Figure CN118880431A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of condensed matter physics, and in particular to a method for synthesizing a single crystal with huge anomalous Hall conductivity at room temperature. Background Art
[0002] When a magnetic field perpendicular to the direction of current is applied in a thin sheet of carriers, a voltage is generated perpendicular to the direction of current and magnetic field. This phenomenon is called the Hall effect. For the normal Hall effect, its intensity value is linearly related to the external magnetic field, while in some materials with large magnetic properties or Berry curvature, the intensity value of the Hall effect deviates significantly from the linear correlation with the external magnetic field. Compared with the normal Hall effect, the anomalous Hall effect signal is generally at least one order of magnitude larger and does not require a large external magnetic field. Anomalous Hall conductivity is a measure of the intensity of the anomalous Hall effect. It has extensive and important applications in modern physics and materials science. By measuring and analyzing the anomalous Hall conductivity, we can gain a deeper understanding of the magnetism, spin properties and topological properties of materials and promote the development of new electronic devices and materials.
[0003] CaTi3Bi4 single crystal is a layered metal material whose thickness can be dissociated to the nanometer level, which helps in the miniaturization and high integration of devices. Its huge anomalous Hall effect at room temperature makes it have potential application value in low-power electronic devices, sensors, etc. Summary of the Invention
[0004] The present invention aims to provide a method for synthesizing a single crystal with giant anomalous Hall conductivity at room temperature, so as to prepare a relatively pure single crystal with giant anomalous Hall conductivity at room temperature.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature, characterized by comprising the following steps:
[0007] S1. Weighing raw materials and flux: Weigh Ti metal, Ca metal, and Bi metal, wherein Ti metal is the raw material, and Ca metal and Bi metal are both raw materials and flux;
[0008] S2. Mixing of raw materials: Mix the raw materials weighed in S1 and add them into a crucible. Place the crucible into a quartz tube and fill the crucible with quartz wool.
[0009] S3. Sealing the quartz tube: extract the air from the quartz tube to make it a vacuum state, and seal the quartz tube using a melting sealing method under a vacuum environment;
[0010] S4, heating the quartz tube: heating the sealed quartz tube in S3 to raise the temperature inside the quartz tube to 850-1000°C, keeping it at this temperature for 3-5 hours, and then cooling it to 450-550°C to obtain CaTi3Bi4 single crystal, liquid Ca / Bi mixture and solid quartz wool;
[0011] S5, high temperature centrifugation: the quartz tube in S4 is subjected to high temperature centrifugation to separate the CaTi3Bi4 single crystal in the quartz tube from the liquid Ca / Bi mixture;
[0012] S6. Obtaining CaTi3Bi4 single crystals: After the quartz tube subjected to high-temperature centrifugation in S5 is cooled to room temperature, the crucible is taken out to obtain a layered CaTi3Bi4 single crystal having a nearly hexagonal shape and a size of 1 to 2 mm in the crucible.
[0013] Furthermore, in S1, when weighing the metal, it is weighed according to the element ratio of Ca:Ti:Bi=1:1:10-20.
[0014] Furthermore, in S1, the total amount of Ti metal, Ca metal and Bi metal weighed is 3 to 4.5 g.
[0015] Furthermore, in S2, the thickness of the quartz wool filled above the crucible is 2 to 3 cm.
[0016] Furthermore, in S3, when the quartz tube is sealed, the pressure of the vacuum environment is less than 10Pa.
[0017] Furthermore, in S4, the heating rate is 1-3°C / min, and the cooling rate is 1-3°C / h.
[0018] The beneficial effects of the technical solution are:
[0019] 1. The present invention uses Ti metal, Ca metal and Bi metal as raw materials, wherein Ca metal and Bi metal serve as both raw materials and fluxes, effectively ensuring the purity of the prepared CaTi3Bi4 single crystal.
[0020] 2. The CaTi3Bi4 single crystal prepared by the present invention is a layered material that can be easily dissociated to nanometer-level thickness by mechanical exfoliation, which is very beneficial to the miniaturization and high integration of devices.
[0021] 3. The CaTi3Bi4 single crystal prepared by the present invention has huge anomalous Hall conductivity at room temperature, which can detect tiny magnetic field changes at extremely low currents, and is helpful to promote the development of low-power electronic devices, sensors, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is an optical photograph of the layered CaTi3Bi4 single crystal prepared in Example 1 of the present invention;
[0023] Figure 2 The single crystal XRD spectrum of the layered CaTi3Bi4 single crystal prepared in Example 1 of the present invention is shown below:
[0024] Figure 3 This is a Hall conductivity curve of the layered CaTi3Bi4 single crystal prepared in Example 1 of the present invention; DETAILED DESCRIPTION
[0025] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments:
[0026] Example 1 Preparation of CaTi3Bi4 Single Crystal
[0027] S1. Weigh metal elements in a ratio of Ca:Ti:Bi = 1:1:20, with the total amount not exceeding 4.5 g, wherein Ca metal and Bi metal serve as both raw materials and flux;
[0028] S2. Add the weighed raw materials to a 5 mL magnesium oxide crucible, place the crucible in a quartz tube, and fill the crucible with quartz wool about 3 cm high.
[0029] S3, evacuate the quartz tube, and melt and seal the quartz tube under a vacuum state with a pressure less than 10Pa;
[0030] S4. Place the sealed quartz tube in a muffle furnace and heat it to 1000°C within 10 hours. Keep it at this temperature for 5 hours and then slowly cool it down to 500°C at a rate of 3°C / h.
[0031] S5, separating the CaTi3Bi4 single crystal from the liquid Ca / Bi mixture in the quartz tube by rapid high-temperature centrifugation;
[0032] S6. After the quartz tube is cooled to room temperature, the crucible is taken out to obtain a layered CaTi3Bi4 single crystal having a nearly hexagonal shape and a size of 1 to 2 mm in the crucible.
[0033] The layered CaTi3Bi4 single crystals prepared in Example 1 are as follows Figure 1 shown.
[0034] Example 1 The prepared CaTi3Bi4 single crystal was subjected to single crystal X-ray diffraction spectrum testing;
[0035] The test results are as follows Figure 2 As shown in the figure: the diffraction peaks all correspond to the (0 0l) peaks of CaTi3Bi4, and no impurity peaks are observed, indicating that the prepared CaTi3Bi4 single crystal is relatively pure.
[0036] Example 1 The prepared CaTi3Bi4 single crystal was tested for inverse Hall conductivity;
[0037] The test results are as follows Figure 3 As shown in the figure: The curve is the Hall conductivity curve of CaTi3Bi4 single crystal. The system has a huge anomalous Hall conductivity (AHC) at low magnetic field. At 100K, AHC (about 1200Ω -1 cm -1 ) is the largest. As the temperature rises, AHC decreases. At room temperature 300K, there is still AHC (about 300Ω -1 cm -1 ).
[0038] The above is only an embodiment of the present invention, and common knowledge such as the specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several variations and improvements can be made, which should also be regarded as the scope of protection of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the description can be used to interpret the content of the claims.
Claims
1. A method for synthesizing a single crystal having huge anomalous Hall conductivity at room temperature, characterized in that: The following steps are involved: S1. Weighing raw materials and flux: Weigh Ti metal, Ca metal and Bi metal, wherein Ti metal is the raw material, and Ca metal and Bi metal are both raw materials and flux; S2, mixing of raw materials: adding the raw materials weighed in S1 to a crucible, placing the crucible in a quartz tube, and filling the crucible with quartz wool; S3, sealing the quartz tube: extracting the air in the quartz tube to make the quartz tube in a vacuum state, and at the same time using a melting sealing method to seal the quartz tube in a vacuum environment; S4, heating the quartz tube: heating the sealed quartz tube in S3, raising the temperature inside the quartz tube to 850-1000°C, keeping it warm for 3-5h, and then cooling it to 450-550°C to prepare CaTi3Bi4 single crystal, liquid Ca / Bi mixture and solid quartz wool; S5, high temperature centrifugation: subjecting the quartz tube in S4 to high temperature centrifugation to separate the CaTi3Bi4 single crystal in the quartz tube from the liquid Ca / Bi mixture; S6. Obtaining CaTi3Bi4 single crystals: After the quartz tube after high-temperature centrifugation in S5 is cooled to room temperature, the crucible is taken out to obtain a layered CaTi3Bi4 single crystal of approximately hexagonal shape with a size of 1 to 2 mm in the crucible.
2. The method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature according to claim 1, characterized in that: In S1, when weighing the metal, it is weighed according to the element ratio of Ca:Ti:Bi=1:1:10-20.
3. The method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature according to claim 1, characterized in that: In S1, the total amount of Ti metal, Ca metal and Bi metal weighed is 3 to 4.5 g.
4. The method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature according to claim 1, characterized in that: In S2, the thickness of the quartz wool filled above the crucible is 2 to 3 cm.
5. The method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature according to claim 1, characterized in that: In S3, when the quartz tube is sealed, the pressure of the vacuum environment is less than 10Pa.
6. The method for synthesizing a single crystal having giant anomalous Hall conductivity at room temperature according to claim 1, characterized in that: In S4, the heating rate is 1-3°C / min, and the cooling rate is 1-3°C / h.