Crystal growth method for crystal growth furnace
By filling the platinum crucible into the alumina crucible and heating it in layers, crystal growth is achieved in a non-vacuum environment, solving the difficulties in observation and high energy consumption caused by vacuum extraction in the prior art, and improving crystal growth reliability and shoulder structural strength.
Patent Information
- Application Number
- CN202410976267.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-01
AI Technical Summary
The existing crystal growth furnaces require vacuum during heating to reduce oxidation, which makes the crystal growth process unobservable and high energy consumption, affecting production costs.
The platinum crucible is loaded into an alumina crucible and heated the platinum crucible through a layered heating coil to achieve crystal growth in a non-vacuum environment, and lift the seed rod in stages to lift and place the shoulders. Ensure the strength of the crystal shoulder structure.
Crystal growth is achieved without vacuum, which is convenient for workers to observe, and improves the reliability of crystal growth and shoulder structure strength, reducing production costs.
Smart Images

Figure CN118880437A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a crystal processing method, in particular to a crystal growing method used in a crystal growing furnace. Background Art
[0002] When currently used, the existing crystal growth furnace needs to be vacuumed to reduce oxidation of the metal crucible during the heating process. This not only makes it impossible to closely observe the crystal growth process, affecting workers' monitoring of the crystal growth process, but also requires additional energy consumption for vacuuming, resulting in relatively high production costs. Summary of the invention
[0003] The purpose of the invention is to provide a crystal growth method for a crystal growth furnace, which can be implemented without vacuuming, making it easier for workers to observe the growth process and improving the reliability of crystal growth.
[0004] Technical solution: The crystal growth method for a crystal growth furnace of the present invention comprises the following steps:
[0005] Step 1, put the platinum crucible into the alumina crucible, fill the space between the platinum crucible and the alumina crucible with zirconium sand, the alumina crucible is located at the center of the heating coil of the crystal growth furnace, first adjust the horizontality of the platinum crucible, and then adjust the concentricity of the platinum crucible and the seed crystal rod;
[0006] Step 2: Use a vacuum cleaner to clean the debris in the platinum crucible, then wipe the inner wall of the platinum crucible with an alcohol cotton ball, and then put the weighed LT polycrystalline powder into the platinum crucible;
[0007] Step 3, clean the alumina inner cover, the inner insulation cover and the outer insulation cover with a vacuum cleaner, and then sequentially cover the alumina inner cover, the inner insulation cover and the outer insulation cover on the alumina crucible;
[0008] Step 4, turn on the electric frequency power supply of the crystal growth furnace, start the temperature rising program, heat the platinum crucible with the heating coil, wait for the LT polycrystalline powder to melt into molten material, then reduce the electric frequency power supply to the inoculation power value, and keep the constant temperature for 40 to 60 minutes;
[0009] Step 5, setting the rotation speed of the seed crystal rod to 8-14 rpm, and then slowly lowering the lower end of the seed crystal rod into the molten material to perform seeding, inoculation and seed melting;
[0010] Step 6, lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder, and entering a rapid growth program when the shoulder diameter is expanded to a preset size;
[0011] Step 7, after entering the rapid growth program, set the lifting speed of the seed crystal rod to 3.5-3.8 mm / hour, end the rapid growth program when the crystal grows to the set length, stop the rotation drive of the seed crystal rod, reduce the power value of the electric frequency power supply to achieve cooling, lift the seed crystal rod so that the crystal is lifted 25-35 mm from the liquid surface, and set the heating power value to zero;
[0012] Step 8, after the crystals are cooled to room temperature, they are taken out and the taken out crystals are initially inspected, numbered, weighed, shape measured, color tested, and put into storage.
[0013] Furthermore, in step 1, when adjusting the concentricity of the platinum crucible and the seed crystal rod, the deviation between the central axis of the inner wall ring of the platinum crucible and the central axis of the seed crystal rod is between 0 and 8 mm.
[0014] Furthermore, in step 2, after wiping the inner wall of the platinum crucible with an alcohol cotton ball, the inside of the platinum crucible is cleaned again with a vacuum cleaner.
[0015] Furthermore, in step 3, when the alumina inner cover, the inner insulation cover and the outer insulation cover are covered on the alumina crucible, it is ensured that the distance between the hole wall of the top center hole and the outer wall of the seed rod is between 2 and 3.5 cm.
[0016] Furthermore, in step 4, the heating coil includes an upper heating coil, a middle heating coil and a lower heating coil; the upper heating coil is used to heat the upper position of the platinum crucible; the middle heating coil is used to heat the middle position of the platinum crucible; and the lower heating coil is used to heat the lower position of the platinum crucible.
[0017] Furthermore, in step 4, the specific steps of heating the platinum crucible by the heating coil are:
[0018] First, the upper layer, the middle layer and the lower layer of the platinum crucible are heated synchronously by the upper layer heating coil, the middle layer heating coil and the lower layer heating coil at the same first heating power, so that the heating temperature reaches a first temperature value, and the heating time is 15 to 20 minutes, so that the LT polycrystalline powder is melted into a molten material;
[0019] Then, the heating power of the upper heating coil is set to 95% of the first heating power, the heating power of the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes;
[0020] Then, the heating power of the middle heating coil is set to 95% of the first heating power, the heating power of the upper heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes;
[0021] Then, the heating power of the lower heating coil is set to 95% of the first heating power, the heating power of the upper heating coil and the middle heating coil is set to the first heating power, and the heating time is 2 to 4 minutes;
[0022] Finally, the heating power of the upper heating coil, the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 1 to 3 minutes.
[0023] Furthermore, in step 5, the rotation speed of the seed rod is set to 10 rpm, and the lower end of the seed rod is slowly lowered to a depth of 8 to 13 mm in the molten material.
[0024] Further, in step 6, the specific steps of lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder are:
[0025] First, the lifting speed of the first lifting stage is set to 3-3.5 mm / hour, and the lifting time of the first lifting stage is set to 1.5-2 hours. The first lifting stage is performed according to the set lifting speed and lifting time.
[0026] Then, after the first lifting stage is completed, the lifting speed of the second lifting stage is set to 2-3 mm / hour, the lifting time of the second lifting stage is set to 1-1.5 hours, and the second lifting stage is performed according to the set lifting speed and lifting time;
[0027] Finally, after the second lifting stage is completed, the lifting speed of the third lifting stage is set to 1-1.5 mm / hour, the lifting time of the third lifting stage is set to 0.5-1 hour, and the third lifting stage is executed according to the set lifting speed and lifting time.
[0028] Further, in step 7, the lifting speed of the seed crystal rod is set to 3.6 mm / hour.
[0029] Furthermore, in step 7, the specific steps of lifting the seed crystal rod to lift the crystal out of the liquid surface are:
[0030] First, the lifting speed of the first lifting stage is set to 2-3 mm / hour, the lifting time of the first lifting stage is set to 2-2.5 hours, and the first lifting stage is performed according to the set lifting speed and lifting time;
[0031] Then, after the first lift-off stage is completed, the lift-off speed of the second lift-off stage is set to 3-5 mm / hour, the lift-off time of the second lift-off stage is set to 1-1.5 hours, and the second lift-off stage is performed according to the set lift-off speed and lift-off time;
[0032] Finally, after the second lift-off stage is completed, the lift-off speed of the third lift-off stage is set to 15 to 20 mm / hour, and the third lift-off stage is executed so that the crystal is lifted 25 to 35 mm from the liquid surface.
[0033] Compared with the prior art, the present invention has the following beneficial effects: a platinum crucible is built into an alumina crucible to load LT polycrystalline powder for heating, which has good oxidation resistance and realizes the crystal growth requirements in a non-vacuum environment, making it convenient for workers to open the furnace door at any time to observe the crystal growth situation and ensure reliable crystal growth; the seed crystal rod is lifted and released in stages to make the shoulder of the crystal have a better transition effect and a stronger structural strength, thereby ensuring reliable crystal suspension growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The present invention is a flow chart of the method. DETAILED DESCRIPTION
[0035] The technical solution of the present invention is described in detail below with reference to the accompanying drawings, but the protection scope of the present invention is not limited to the embodiments.
[0036] Embodiment 1:
[0037] like Figure 1 As shown, the crystal growth method for a crystal growth furnace disclosed in the present invention comprises the following steps:
[0038] Step 1, put the platinum crucible into the alumina crucible, fill the space between the platinum crucible and the alumina crucible with zirconium sand, the alumina crucible is located at the center of the heating coil of the crystal growth furnace, first adjust the horizontality of the platinum crucible, and then adjust the concentricity of the platinum crucible and the seed crystal rod;
[0039] Step 2: Use a vacuum cleaner to clean the debris in the platinum crucible, then wipe the inner wall of the platinum crucible with an alcohol cotton ball, and then put the weighed LT polycrystalline powder into the platinum crucible;
[0040] Step 3, clean the alumina inner cover, the inner insulation cover and the outer insulation cover with a vacuum cleaner, and then sequentially cover the alumina inner cover, the inner insulation cover and the outer insulation cover on the alumina crucible;
[0041] Step 4, turn on the electric frequency power supply of the crystal growth furnace, start the temperature rising program, heat the platinum crucible with the heating coil, wait for the LT polycrystalline powder to melt into molten material, then reduce the electric frequency power supply to the inoculation power value, and keep the constant temperature for 40 to 60 minutes;
[0042] Step 5, setting the rotation speed of the seed crystal rod to 8-14 rpm, and then slowly lowering the lower end of the seed crystal rod into the molten material to perform seeding, inoculation and seed melting;
[0043] Step 6, lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder, and entering a rapid growth program when the shoulder diameter is expanded to a preset size;
[0044] Step 7, after entering the rapid growth program, set the lifting speed of the seed crystal rod to 3.5-3.8 mm / hour, end the rapid growth program when the crystal grows to the set length, stop the rotation drive of the seed crystal rod, reduce the power value of the electric frequency power supply to achieve cooling, lift the seed crystal rod so that the crystal is lifted 25-35 mm from the liquid surface, and set the heating power value to zero;
[0045] Step 8, after the crystals are cooled to room temperature, they are taken out and the taken out crystals are initially inspected, numbered, weighed, shape measured, color tested, and put into storage.
[0046] The platinum crucible is built into the alumina crucible to load the LT polycrystalline powder for heating. It has good oxidation resistance and realizes the crystal growth requirements in a non-vacuum environment. It is convenient for workers to open the furnace door at any time to observe the crystal growth and ensure the reliable growth of the crystal. The seed crystal rod is lifted and lowered in stages to make the shoulder of the crystal have a better transition effect and a stronger structural strength, which ensures the reliable suspension growth of the crystal.
[0047] Furthermore, in step 1, when adjusting the concentricity of the platinum crucible and the seed crystal rod, the deviation between the central axis of the circular ring on the inner wall of the platinum crucible and the central axis of the seed crystal rod is made to be between 0 and 8 mm, preferably between 0 and 3 mm. This can ensure that the crystal grown under the seed crystal rod has better concentricity, reduce center deviation, and ensure the stability of the crystal during rotational growth.
[0048] Furthermore, in step 2, after wiping the inner wall of the platinum crucible with an alcohol cotton ball, the inside of the platinum crucible is vacuumed again with a vacuum cleaner. The cotton threads that may remain after wiping can be sucked out by vacuuming again, ensuring that the crucible is sufficiently clean after cleaning.
[0049] Furthermore, in step 3, when the alumina inner cover, inner insulation cover and outer insulation cover are covered on top of the alumina crucible, it is ensured that the distance between the hole wall of each top center hole and the outer wall of the seed rod is between 2 and 3.5 cm, and the preferred distance is between 2 and 2.5 cm, thereby reducing the heat dissipation at the top center hole and ensuring that the seed rod collides with the hole wall.
[0050] Furthermore, in step 4, the heating coil includes an upper heating coil, a middle heating coil and a lower heating coil; the upper heating coil is used to heat the upper position of the platinum crucible; the middle heating coil is used to heat the middle position of the platinum crucible; and the lower heating coil is used to heat the lower position of the platinum crucible. The upper heating coil, the middle heating coil and the lower heating coil constitute the heating coil, which can achieve layered and fine heating of the upper, middle and lower layers of the platinum crucible, and has a better heating effect.
[0051] Furthermore, in step 4, the specific steps of heating the platinum crucible by the heating coil are:
[0052] First, the upper layer, the middle layer and the lower layer of the platinum crucible are heated synchronously by the upper layer heating coil, the middle layer heating coil and the lower layer heating coil at the same first heating power, so that the heating temperature reaches a first temperature value, and the heating time is 15 to 20 minutes, preferably 18 minutes, so that the LT polycrystalline powder is melted into a molten material;
[0053] Then, the heating power of the upper heating coil is set to 95% of the first heating power, the heating power of the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes, preferably 3 minutes;
[0054] Then, the heating power of the middle heating coil is set to 95% of the first heating power, the heating power of the upper heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes, preferably 3 minutes;
[0055] Then, the heating power of the lower heating coil is set to 95% of the first heating power, and the heating power of the upper heating coil and the middle heating coil is set to the first heating power, and the heating time is 2 to 4 minutes, preferably 3 minutes;
[0056] Finally, the heating power of the upper heating coil, the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 1 to 3 minutes, preferably 2 minutes.
[0057] By heating at the first temperature value for 15 to 20 minutes, the LT polycrystalline powder can be melted into molten material, and then layered fine heating is performed for 2 to 4 minutes. The heating temperatures of each layer are allowed to be inconsistent, so that the molten material can flow under the condition of uneven heating, thereby enhancing the uniformity of the molten material. Finally, heating at the same power for 1 to 3 minutes is used to maintain the molten material after flowing to the set temperature again, so as to facilitate the implementation of subsequent steps.
[0058] Furthermore, in step 5, the rotation speed of the seed rod is set to 10 rpm, and the lower end of the seed rod is slowly lowered into the molten material to a depth of 8 to 13 mm, preferably 10 mm, so as to ensure the reliable implementation of the subsequent shoulder release process.
[0059] Further, in step 6, the specific steps of lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder are:
[0060] First, the lifting speed of the first lifting stage is set to 3-3.5 mm / hour, and the lifting time of the first lifting stage is set to 1.5-2 hours. The first lifting stage is performed according to the set lifting speed and lifting time.
[0061] Then, after the first lifting stage is completed, the lifting speed of the second lifting stage is set to 2-3 mm / hour, the lifting time of the second lifting stage is set to 1-1.5 hours, and the second lifting stage is performed according to the set lifting speed and lifting time;
[0062] Finally, after the second lifting stage is completed, the lifting speed of the third lifting stage is set to 1-1.5 mm / hour, the lifting time of the third lifting stage is set to 0.5-1 hour, and the third lifting stage is executed according to the set lifting speed and lifting time.
[0063] Through the implementation of the first lifting stage, the crystal and the seed rod can have a stronger bonding performance when the shoulder diameter is small, and in the second lifting stage, the diameter expansion speed of the shoulder becomes faster, so it is necessary to slow down the lifting speed and reduce the lifting time, so that the shoulder diameter can be quickly expanded to a larger size, and then to the third lifting stage, the lifting speed and lifting time are further reduced to consolidate the grown shoulder to ensure the quality and structural strength of the shoulder. At the same time, the three-stage lifting can ensure the growth of a crystal shoulder with good bonding effect and high structural strength, providing reliable support for subsequent crystal growth.
[0064] Further, in step 7, the lifting speed of the seed crystal rod is set to 3.6 mm / hour.
[0065] Furthermore, in step 7, the specific steps of lifting the seed crystal rod to lift the crystal out of the liquid surface are:
[0066] First, the lifting speed of the first lifting stage is set to 2-3 mm / hour, the lifting time of the first lifting stage is set to 2-2.5 hours, and the first lifting stage is performed according to the set lifting speed and lifting time;
[0067] Then, after the first lift-off stage is completed, the lift-off speed of the second lift-off stage is set to 3-5 mm / hour, the lift-off time of the second lift-off stage is set to 1-1.5 hours, and the second lift-off stage is performed according to the set lift-off speed and lift-off time;
[0068] Finally, after the second lift-off stage is completed, the lift-off speed of the third lift-off stage is set to 15 to 20 mm / hour, and the third lift-off stage is executed so that the crystal is lifted 25 to 35 mm from the liquid surface.
[0069] Through the low-speed lifting in the first lifting stage, the diameter of the bottom of the crystal can shrink relatively smoothly. After entering the second lifting stage, the lifting speed begins to increase and this stage is completed in a short time, so that the bottom diameter shrinks faster and separates from the molten material surface below to form a tip. Finally, entering the third lifting stage, it is quickly lifted to a specified height, so that the crystal is completely separated from the molten liquid surface and maintains a safe distance. Through three stages of lifting, the bottom of the crystal can shrink smoothly, and there will be no pulling damage caused by bottom separation.
[0070] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. A crystal growth method for a crystal growth furnace, characterized in that: The steps include: Step 1, put the platinum crucible into the alumina crucible, fill the space between the platinum crucible and the alumina crucible with zirconium sand, the alumina crucible is located at the center of the heating coil of the crystal growth furnace, first adjust the horizontality of the platinum crucible, and then adjust the concentricity of the platinum crucible and the seed crystal rod; Step 2: Use a vacuum cleaner to clean the debris in the platinum crucible, then wipe the inner wall of the platinum crucible with an alcohol cotton ball, and then put the weighed LT polycrystalline powder into the platinum crucible; Step 3, clean the alumina inner cover, the inner insulation cover and the outer insulation cover with a vacuum cleaner, and then sequentially cover the alumina inner cover, the inner insulation cover and the outer insulation cover on the alumina crucible; Step 4, turn on the electric frequency power supply of the crystal growth furnace, start the temperature rising program, heat the platinum crucible with the heating coil, wait for the LT polycrystalline powder to melt into molten material, then reduce the electric frequency power supply to the inoculation power value, and keep the constant temperature for 40 to 60 minutes; Step 5, setting the rotation speed of the seed crystal rod to 8-14 rpm, and then slowly lowering the lower end of the seed crystal rod into the molten material to perform seeding, inoculation and seed melting; Step 6, lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder, and entering a rapid growth program when the shoulder diameter is expanded to a preset size; Step 7, after entering the rapid growth program, set the lifting speed of the seed crystal rod to 3.5-3.8 mm / hour, end the rapid growth program when the crystal grows to the set length, stop the rotation drive of the seed crystal rod, reduce the power value of the electric frequency power supply to achieve cooling, lift the seed crystal rod so that the crystal is lifted 25-35 mm from the liquid surface, and set the heating power value to zero; Step 8, after the crystals are cooled to room temperature, they are taken out and the taken out crystals are initially inspected, numbered, weighed, shape measured, color tested, and put into storage.
2. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 1, when adjusting the concentricity of the platinum crucible and the seed crystal rod, the deviation between the central axis of the inner wall ring of the platinum crucible and the central axis of the seed crystal rod is between 0 and 8 mm.
3. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 2, after wiping the inner wall of the platinum crucible with an alcohol cotton ball, the inside of the platinum crucible is cleaned again with a vacuum cleaner.
4. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 3, when the alumina inner cover, the inner insulation cover and the outer insulation cover are covered on the alumina crucible, the distance between the hole wall of the top center hole and the outer wall of the seed crystal rod is ensured to be between 2 and 3.5 cm.
5. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 4, the heating coil includes an upper heating coil, a middle heating coil and a lower heating coil; the upper heating coil is used to heat the upper position of the platinum crucible; the middle heating coil is used to heat the middle position of the platinum crucible; and the lower heating coil is used to heat the lower position of the platinum crucible.
6. The crystal growth method for a crystal growth furnace according to claim 5, characterized in that: In step 4, the specific steps of heating the platinum crucible by the heating coil are: First, the upper layer, the middle layer and the lower layer of the platinum crucible are heated synchronously by the upper layer heating coil, the middle layer heating coil and the lower layer heating coil at the same first heating power, so that the heating temperature reaches a first temperature value, and the heating time is 15 to 20 minutes, so that the LT polycrystalline powder is melted into a molten material; Then, the heating power of the upper heating coil is set to 95% of the first heating power, the heating power of the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes; Then, the heating power of the middle heating coil is set to 95% of the first heating power, the heating power of the upper heating coil and the lower heating coil is set to the first heating power, and the heating time is 2 to 4 minutes; Then, the heating power of the lower heating coil is set to 95% of the first heating power, the heating power of the upper heating coil and the middle heating coil is set to the first heating power, and the heating time is 2 to 4 minutes; Finally, the heating power of the upper heating coil, the middle heating coil and the lower heating coil is set to the first heating power, and the heating time is 1 to 3 minutes.
7. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 5, the rotation speed of the seed crystal rod is set to 10 rpm, and the lower end of the seed crystal rod is slowly lowered to a depth of 8 to 13 mm in the molten material.
8. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 6, the specific steps of lifting the seed crystal rod in stages at a lifting speed of 1.5 to 3.5 mm / hour to lift and release the shoulder are as follows: First, the lifting speed of the first lifting stage is set to 3-3.5 mm / hour, and the lifting time of the first lifting stage is set to 1.5-2 hours. The first lifting stage is performed according to the set lifting speed and lifting time. Then, after the first lifting stage is completed, the lifting speed of the second lifting stage is set to 2-3 mm / hour, the lifting time of the second lifting stage is set to 1-1.5 hours, and the second lifting stage is performed according to the set lifting speed and lifting time; Finally, after the second lifting stage is completed, the lifting speed of the third lifting stage is set to 1-1.5 mm / hour, the lifting time of the third lifting stage is set to 0.5-1 hour, and the third lifting stage is executed according to the set lifting speed and lifting time.
9. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 7, the lifting speed of the seed crystal rod is set to 3.6 mm / hour.
10. The crystal growth method for a crystal growth furnace according to claim 1, characterized in that: In step 7, the specific steps of lifting the seed crystal rod to lift the crystal out of the liquid surface are: First, the lifting speed of the first lifting stage is set to 2-3 mm / hour, the lifting time of the first lifting stage is set to 2-2.5 hours, and the first lifting stage is performed according to the set lifting speed and lifting time; Then, after the first lift-off stage is completed, the lift-off speed of the second lift-off stage is set to 3-5 mm / hour, the lift-off time of the second lift-off stage is set to 1-1.5 hours, and the second lift-off stage is performed according to the set lift-off speed and lift-off time; Finally, after the second lift-off stage is completed, the lift-off speed of the third lift-off stage is set to 15 to 20 mm / hour, and the third lift-off stage is executed so that the crystal is lifted 25 to 35 mm from the liquid surface.