Composite crystal and preparation method thereof

The mode guide method of growing composite crystals with pure matrix and activated ion-doped crystals solves the problem of thermal effects of traditional laser devices at high power, and achieves high-quality and large-size composite crystal growth, which is suitable for high-power laser devices and reduces the problem of thermal effects of traditional laser devices. Production costs and improve output performance.

CN118880441APending Publication Date: 2024-11-01QINGDAO HUAXIN JINGDIAN TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410936410.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional laser devices are easily affected by thermal effects at high power, resulting in a decrease in the quality and output power of the laser beam. The existing composite crystal preparation methods have problems such as large composite bonding surface loss, low bonding intensity, small crystal size, and large internal stress. It is difficult to meet the needs of high-power laser devices.

Method used

The composite crystals are grown by the mode guide method. By combining pure matrix crystal A and activated ion doped crystal B, the edge-limited film feeding technology of the mode guide method can achieve rapid growth of large-size composite crystals, avoiding multiple surface treatment processes. and defects during bonding improve crystal stability and size.

Benefits of technology

It realizes the growth of large-size composite crystals without scattering and high-quality, can withstand high power density, reduces production costs, and improves the output performance and economic use value of laser devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880441A_ABST
    Figure CN118880441A_ABST
Patent Text Reader

Abstract

The invention relates to a composite crystal and a preparation method thereof, the composite crystal is composed of a crystal A and a crystal B, the crystal A is a pure host crystal, and the crystal B is an active ion doped crystal with the same matrix as the crystal A. The active ions are luminescent transition metal ions or rare earth ions, and the doping concentration is 0-1. The composite crystal grows by an edge-defined film-fed growth method. The preparation method has the advantages that the components and the method are reasonable in design, the composite crystal is grown by utilizing an edge-defined film-fed crystal growth method, the flaky seed crystal is convenient to inoculate and high in growth speed, the scattering-free high-quality composite crystal can be obtained in a relatively short time, and the grown composite crystal is large in size, stable in composite surface, free of defects and capable of bearing high power density, and is an excellent gain medium for a high-power laser; and moreover, multiple crystal surface treatment procedures are omitted, the possibility of generating color center, wrappage, degumming and other defects in the bonding process is avoided, the production cost can be reduced, the working efficiency can be improved, and the method has relatively high economic use value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite crystal and a preparation method thereof, in particular to a composite crystal of a high-power laser device and a guided mode growth method for preparing the composite crystal, belonging to the technical field of crystal material preparation. Background Art

[0002] "One generation of materials, one generation of devices", laser materials (gain media) as the core and foundation of the development of laser devices, have milestone significance and role, especially laser crystals, which are crucial to the development of laser technology.

[0003] Traditional gain media are usually crystals doped with a specific concentration. When the laser is in use, the higher the pump power density, the more susceptible the crystal is to thermal effects, which reduces the output laser beam quality and output power, and even causes the crystal to crack in severe cases. Therefore, how to effectively remove the waste heat generated by the laser is the key to improving the laser beam quality and output power.

[0004] In order to improve the thermal effect of the laser and obtain high-power and high-quality laser output, existing technologies have proposed the use of composite crystals or bonded crystals as gain media, that is, by compounding or bonding undoped crystals with doped crystals, and extracting waste heat from doped crystals through the high thermal conductivity of undoped crystals. This is mainly achieved through the following two ways: (1) Bonding crystals are prepared using bonding technology. Bonding is a commercial preparation method currently available. Commonly used crystal bonding technologies include melt bonding technology, low-temperature vacuum thermal bonding technology, and adhesive bonding technology. Melt bonding technology and low-temperature vacuum thermal bonding technology have high requirements for the flatness and smoothness of the crystal surface, and the production process has high environmental requirements. Adhesive bonding technology has the advantages of simple process and low processing accuracy requirements. However, the composite crystals prepared by this method have excessive composite bonding surface loss and low bonding strength, and are difficult to withstand high power density. (2) Directly grow composite crystals. There are mainly Czochralski method and optical floating zone method. The Czochralski method for growing composite crystals has high requirements for the crystal growth process. The inoculation of the bottom surface of the block crystal is complex and difficult to control, and defects such as polycrystalline and scattering are prone to occur.

[0005] CN102534791A discloses a method for growing and preparing Nd by using a laser-activated ion-doped concentration gradient vanadate composite crystal and a method for preparing the same. 3+ For composite crystals with gradient concentration, this method is fast and has a short cycle. No crucible is required for crystal growth. However, due to the limitations of the growth method, the crystal diameter is generally small and the internal stress is large.

[0006] The guided mold method is one of the methods for artificially producing single crystal materials from the melt, namely the "edge-limited thin film feeding growth" technology. The working principle of the guided mold method is to heat and melt the raw materials in a crucible, and the melt rises to the top of the mold along the capillary feeding seam of the mold under the capillary action. The seed crystal is connected to the liquid surface at the top of the mold to pull the melt, so that the atoms or molecules are constantly rearranged at the interface between the seed crystal and the melt, and gradually solidifies as the temperature drops to grow a single crystal. The guided mold method has the advantages of short growth time, low power consumption, directional / fixed growth, and simple crystal processing. Summary of the invention

[0007] The present invention proposes a composite crystal and a preparation method thereof, the purpose of which is to overcome the above-mentioned shortcomings of the prior art, to achieve a simple and controllable operation method with reduced production costs, to quickly grow high-quality, large-size composite crystals, and to provide an excellent laser gain medium for laser devices.

[0008] The technical solution of the present invention is: a composite crystal, composed of crystal A and crystal B, wherein crystal A is a pure matrix crystal, and crystal B is a crystal doped with activated ions and having the same matrix as crystal A.

[0009] Preferably, the activation ions are luminescent transition metal ions or rare earth ions, and the doping concentration is 0-1.

[0010] Preferably, the method for preparing a composite crystal, wherein the composite crystal is grown using a guided mode method, comprises: 1) Ingredients; 2) Solid phase sintering; 3) Guided mode growth of crystal A; 4) Guided mode growth of composite crystals.

[0011] Preferably, the step 1) specifically comprises calculating and accurately weighing the raw materials according to the stoichiometric ratio of crystal A and crystal B and mixing them respectively.

[0012] Preferably, the step 2) is to isostatically press the mixed raw materials corresponding to the A crystal and the B crystal respectively, and put them into separate crucibles for sintering.

[0013] Preferably, the step 3) specifically comprises: putting the sintered raw material of crystal A into a crucible, placing crystal A grains at the mold mouth for temperature testing; selecting a crystal seed A and fixing it on the chuck of the seed crystal rod; closing the furnace door to evacuate, filling the protective gas to the standard atmospheric pressure; turning on the heating power supply to heat up until the raw material is completely melted; continuing to heat up until the grains at the mold mouth begin to melt, shaking the seed crystal down, keeping the seed crystal at a distance from the top of the mold to bake the seed crystal, immersing the seed crystal in the melt at the edge of the mold, and then seeding, performing equal diameter growth, in-situ annealing after the growth is completed, slowly cooling to room temperature, and opening the furnace to obtain crystal A.

[0014] Preferably, the step 4) specifically includes: replacing another crucible, putting the raw material of the sintered B crystal into the crucible, placing the B crystal grains at the mold mouth to test the temperature; selecting the A crystal obtained by the previous guided mold method as the seed crystal and fixing it on the chuck of the seed crystal rod; closing the furnace door to evacuate, filling the protective gas to the standard atmospheric pressure; turning on the heating power supply to heat up until the raw material is completely melted; continuing to heat up until the grains at the mold mouth begin to melt, shaking the seed crystal down, keeping the seed crystal at a distance from the top of the mold to bake the seed crystal, immersing the seed crystal in the melt at the edge of the mold, and then seeding, and growing with equal diameters. After the growth is completed, annealing is performed in situ, slowly cooling to room temperature, and opening the furnace to obtain a composite crystal.

[0015] Preferably, the crucible, crucible cover and mold in steps 3) and 4) are made of iridium, molybdenum or tungsten.

[0016] Preferably, the vacuuming in steps 3) and 4) is completed when the vacuum degree reaches 3-10Pa.

[0017] Preferably, in steps 3) and 4), the heating power source is turned on to increase the temperature and maintain the temperature constant for 0.5-2 hours to completely melt the raw materials.

[0018] Preferably, after the raw materials are completely melted in steps 3) and 4), the temperature is continued to rise by 20-50° C. and maintained at a constant temperature for 15 minutes until the grains at the mold mouth begin to melt and then the seed crystals are shaken off.

[0019] Preferably, in steps 3) and 4), the seed crystal is baked for 10-30 minutes while maintaining a distance of 2-4 mm between the seed crystal and the top of the mold.

[0020] Preferably, in steps 3) and 4), the seed crystal is immersed in the melt at the edge of the mold for 15-40 minutes.

[0021] Preferably, in steps 3) and 4), the medium diameter growth pulling speed is 3-10 mm / h, and the cooling rate is 5-10° C. / h.

[0022] Preferably, after the growth in steps 3) and 4) is completed, in-situ annealing is performed for 2-10 hours, and the temperature is slowly cooled to room temperature for 20-40 hours.

[0023] The advantages of the present invention are as follows: the components and methods are reasonably designed, the composite crystal is grown by the guided mode method, the flake seed crystal is convenient to inoculate, the growth speed is fast, and a scattering-free high-quality composite crystal can be obtained in a relatively short time. The grown composite crystal is large in size, the composite surface is stable and defect-free, and it can withstand high power density, and is an excellent gain medium for high-power lasers; and multiple crystal surface treatment processes are omitted, and the possibility of defects such as color centers, inclusions, and debonding in the bonding process is avoided, which can reduce production costs, improve work efficiency, and has great economic use value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the composite crystal preparation method of the present invention.

[0025] In the figure, 1 is the seed crystal, 2 is the A crystal, 3 is the B crystal, 4 is the mold, and 5 is the crucible. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below with reference to examples and specific implementation methods.

[0027] A composite crystal is composed of crystal A and crystal B, wherein crystal A is a pure matrix crystal, and crystal B is a crystal with the same matrix as crystal A doped with activated ions, wherein the activated ions refer to luminescent transition metal ions or rare earth ions, and the doping concentration is 0-1.

[0028] like Figure 1 As shown, a method for preparing a composite crystal, wherein the composite crystal is grown by a guided mode method, comprising: Ingredients: Calculate and accurately weigh each raw material (preferably with a purity greater than 99.99%) according to the stoichiometric ratio of crystal A and crystal B and mix them separately; Solid phase sintering: The mixed raw materials corresponding to crystal A and crystal B are isostatically pressed and sintered in separate alumina crucibles; The guided mold growth of crystal A: the sintered raw material of crystal A is put into a crucible (the material of the crucible, crucible cover and mold is preferably high temperature resistant material such as iridium, molybdenum or tungsten), and the crystal A grain is placed at the mold mouth for temperature testing. Select A crystal seed (preferably high-quality crystal, requiring no cracks, no grain boundaries, and no bubbles) and fix it on the seed crystal rod chuck; close the furnace door to evacuate (turn on the mechanical pump until the vacuum reaches 3-10Pa and then turn it off), fill it with protective gas to standard atmospheric pressure; turn on the heating power to increase the temperature (constant temperature for 0.5-2h) until the raw material is completely melted; continue to increase the temperature (20-50℃, and keep the temperature constant for 15min) until the grains at the mold mouth begin to melt, shake the seed crystal down, keep the seed crystal at a distance of 2-4mm from the top of the mold, bake the seed crystal (10-30min), immerse the seed crystal in the melt at the edge of the mold (15-40min), then seed the crystal, and grow it in equal diameters (pulling speed 3-10mm / h, cooling rate 5-10℃ / h), anneal in situ after the growth is completed (2-10h), slowly cool it to room temperature (20-40h), open the furnace to obtain A crystal; Guided mold growth of composite crystals: Replace another crucible, put the sintered B crystal raw material into the crucible (the material of the crucible, crucible cover and mold is preferably iridium, molybdenum or tungsten and other high-temperature resistant materials), and place B crystal grains at the mold mouth to test the temperature. Select the A crystal obtained by the previous guided mold method as the seed crystal (preferably a high-quality crystal with no cracks, no grain boundaries, and no bubbles) and fix it on the seed crystal rod chuck; close the furnace door to evacuate (turn on the mechanical pump until the vacuum reaches 3-10Pa and then turn it off), fill it with protective gas to standard atmospheric pressure; turn on the heating power to increase the temperature (constant temperature for 0.5-2h) until the raw material is completely melted; continue to increase the temperature (20-50℃, and keep the temperature constant for 15min) and shake the seed crystal down after the grains at the mold mouth begin to melt, keep the seed crystal at a distance from the top of the mold (preferably 2-4mm) to bake the seed crystal (10-30min), immerse the seed crystal in the melt at the edge of the mold (15-40min), then seed the crystal, and perform equal diameter growth (pulling speed 3-10mm / h, cooling rate 5-10℃ / h, in-situ annealing after the growth is completed (2-10h), slowly cool to room temperature (20-40h), open the furnace to obtain a composite crystal. Example 1

[0029] Y 3 Al 5 O 12 -3at%Yb:Y 3 Al 5 O 12 The growth process of composite single crystal includes: Yb with a purity of 99.99% 2 O 3 , Y 2 O 3 With Al 2 O 3 The raw materials were prepared according to the stoichiometric ratio (Yb x Y 1-x ) 3 Al 5 O 12 (x=0, 0.03) weigh accurately and mix well.

[0030] It was isostatically pressed at 200 MPa and sintered in an alumina crucible at 1200 °C for 10 h. The sintered Y 3 Al 5 O 12 The raw materials are put into an iridium crucible. Figure 1 As shown, the mold opening is placed Y 3 Al 5 O 12 Grain. Select Y 3 Al 5 O 12The seed crystal is fixed on the chuck of the seed crystal rod; the furnace door is closed, and the mechanical pump is turned on to draw a vacuum. When the vacuum reaches 5Pa, the mechanical pump is turned off, and the protective gas is filled to the standard atmospheric pressure; the heating power is turned on to raise the temperature to 1950℃, and the temperature is kept constant for 1h to completely melt the raw materials; the temperature is continued to rise by 25℃, and the seed crystal is shaken down after the particles at the mold mouth begin to melt, so that the seed crystal and the top of the mold are kept at a distance of 3mm for baking the seed crystal. After 10 minutes, the seed crystal is immersed in the melt at the edge of the mold, and after 20 minutes, the seed is seeded, and isodiametric growth is performed at a pulling speed of 8mm / h and a cooling rate of 5℃ / h; after the growth is completed, it is annealed in situ for 5h, and then slowly cooled to room temperature after 24h.

[0031] Then open the furnace, replace the crucible and 3at%Yb:Y 3 Al 5 O 12 Raw materials, pure Y 3 Al 5 O 12 The crystal is a seed crystal, and the above growth steps are repeated to grow the crystal again. After the crystal growth is completed, it is annealed and cooled to room temperature to obtain the target product Y 3 Al 5 O 12 -3at%Yb:Y 3 Al 5 O 12 Composite crystals. Example 2

[0032] YAlO 3 -5at%Tm:YAlO 3 The growth process of composite single crystal includes: The purity of 99.99% Tm 2 O 3 , Y 2 O 3 With Al 2 O 3 The raw materials were prepared according to the stoichiometric ratio (Tm x Y 1-x )AlO 3 (x=0, 0.05) weigh accurately and mix well.

[0033] The YAlO was isostatically pressed at 200 MPa and sintered in an alumina crucible at 1200 °C for 10 h. 3 The raw materials are put into an iridium crucible. Figure 1 As shown, the mold mouth is placed YAlO 3 Grain. Select YAlO 3The seed crystal is fixed on the chuck of the seed crystal rod; the furnace door is closed, and the mechanical pump is turned on to draw a vacuum. When the vacuum reaches 5Pa, the mechanical pump is turned off, and the protective gas is filled to the standard atmospheric pressure; the heating power is turned on to raise the temperature to 1873℃, and the temperature is kept constant for 1h to completely melt the raw materials; the temperature is continued to rise by 25℃, and the seed crystal is shaken down after the particles at the mold mouth begin to melt, so that the seed crystal and the top of the mold are kept at a distance of 3mm for baking the seed crystal. After 10 minutes, the seed crystal is immersed in the melt at the edge of the mold, and after 20 minutes, the seed is seeded, and equal-diameter growth is performed at a pulling speed of 8mm / h and a cooling rate of 5℃ / h; after the growth is completed, it is annealed in situ for 5h and slowly cooled to room temperature after 24h.

[0034] Then open the furnace, replace the crucible with 5at%Tm:YAlO 3 Raw materials, freshly obtained pure YAlO 3 The crystal is a seed crystal, and the above growth steps are repeated to grow the crystal again. After the growth is completed, it is annealed and cooled to room temperature. The target product YAlO is obtained. 3 -5at%Tm:YAlO 3 Composite crystals. Comparative Example 1

[0035] The difference from Example 1 is that the Y 3 Al 5 O 12 -3at%Yb:Y 3 Al 5 O 12 Composite single crystal.

[0036] Y 3 Al 5 O 12 The crystal is used as a seed crystal to continue growing 3at% Yb:Y 3 Al 5 O 12 When the seed crystal is a large cylindrical crystal with a large contact surface with the melt, the product has more defects on the connection surface than the product in Example 1, and obvious interface changes occur, which is not conducive to the subsequent use of the composite crystal as a laser gain medium. Comparative Example 2

[0037] The difference from Example 1 is that Y 3 Al 5 O 12 -3at%Yb:Y 3 Al 5 O 12 After the composite crystal growth was completed, it was directly cooled to room temperature without annealing and the crystal was taken out.

[0038] Compared with the product of Example 1, it was found that Y 3 Al 5 O12 With 3at%Yb:Y 3 Al 5 O 12 The stress at the crystal interface is relatively large, which is not conducive to the subsequent use of the composite crystal as a laser gain medium.

[0039] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A composite crystal, characterized in that: It is composed of crystal A and crystal B, wherein crystal A is a pure matrix crystal, and crystal B is a crystal with the same matrix as crystal A doped with activated ions.

2. A composite crystal according to claim 1, characterized in that: The activation ions are luminescent transition metal ions or rare earth ions, and the doping concentration is 0-1.

3. A method for preparing a composite crystal according to claim 1 or 2, characterized in that: The composite crystal is grown using the guided mode method, including: 1) Ingredients; 2) Solid phase sintering; 3) Guided mode growth of crystal A; 4) Guided mode growth of composite crystals.

4. A method for preparing a composite crystal according to claim 3, characterized in that: The step 1) specifically comprises calculating and accurately weighing the raw materials according to the stoichiometric ratio of crystal A and crystal B and mixing them respectively.

5. The method for preparing a composite crystal according to claim 3, characterized in that: The step 2) specifically comprises isostatically pressing the mixed raw materials corresponding to the A crystal and the B crystal into shapes, and placing the mixed raw materials into separate crucibles for sintering.

6. The method for preparing a composite crystal according to claim 3, characterized in that: The step 3) specifically includes: putting the sintered A crystal raw material into a crucible, placing A crystal grains at the mold mouth for temperature testing; selecting A crystal seed crystals and fixing them on the seed crystal rod chuck; closing the furnace door to evacuate, filling the protective gas to the standard atmospheric pressure; turning on the heating power supply to heat up until the raw material is completely melted; continuing to heat up until the grains at the mold mouth begin to melt, shaking the seed crystal down, keeping the seed crystal at a distance from the top of the mold to bake the seed crystal, immersing the seed crystal in the melt at the mold edge, and then seeding, performing equal diameter growth, in-situ annealing after the growth is completed, slowly cooling to room temperature, and opening the furnace to obtain A crystal.

7. A method for preparing a composite crystal according to claim 6, characterized in that: The step 4) specifically includes: replacing another crucible, putting the raw material of the sintered B crystal into the crucible, placing the B crystal grains at the mold mouth for temperature testing; selecting the A crystal grown by the previous guided mold method as the seed crystal and fixing it on the seed crystal rod chuck; closing the furnace door to evacuate, filling the protective gas to the standard atmospheric pressure; turning on the heating power supply to heat up until the raw material is completely melted; continuing to heat up until the grains at the mold mouth begin to melt, shaking the seed crystal down, keeping the seed crystal at a distance from the top of the mold to bake the seed crystal, immersing the seed crystal in the melt at the edge of the mold, and then seeding, performing equal diameter growth, in-situ annealing after the growth is completed, slowly cooling to room temperature, and opening the furnace to obtain a composite crystal.

8. A method for preparing a composite crystal according to claim 7, characterized in that: The vacuuming in steps 3) and 4) is completed when the vacuum degree reaches 3-10 Pa; the heating power is turned on to increase the temperature and keep the temperature constant for 0.5-2 hours to completely melt the raw materials.

9. The method for preparing a composite crystal according to claim 7, characterized in that: After the raw materials in steps 3) and 4) are completely melted, the temperature is continued to rise by 20-50°C and kept constant for 15 minutes. After the grains at the mold mouth begin to melt, the seed crystal is shaken down; the seed crystal is kept 2-4mm away from the top of the mold and baked for 10-30 minutes; the seed crystal is immersed in the melt at the mold edge for 15-40 minutes.

10. The method for preparing a composite crystal according to claim 7, characterized in that: In the steps 3) and 4), the pulling speed of the medium diameter growth is 3-10 mm / h, and the cooling rate is 5-10°C / h; after the growth is completed, in-situ annealing is performed for 2-10 hours, and the temperature is slowly cooled to room temperature for 20-40 hours.

Citation Information

Cited By

  • Method for realizing bonding growth of rare earth doped fluoride and pure fluoride crystal

    CN121321229A