Paper-based material with high lignin content and preparation method thereof
By using alkali lignin as a filler in paper-based materials and subjecting them to hot pressing, the problems of weakened inter-fiber bonding and unutilized lignin are solved, improving the mechanical properties and barrier properties of the materials, and realizing the high-value utilization of lignin and environmentally friendly production.
Patent Information
- Application Number
- CN202410827297.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-06-25
Smart Images

Figure CN118880651A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of papermaking, and particularly relates to a paper-based material with a high lignin content and a preparation method thereof. Background Art
[0002] Paper-based materials are one of the most widely used materials at present. Usually, plant fibers are used as the main material in the preparation of paper-based materials, and paper is made by papermaking machines. Fillers are the largest component besides fibers, and the amount added accounts for 1%-60% of the paper material components, which can significantly reduce production costs. The fillers usually used in papermaking are mainly inorganic minerals, such as titanium dioxide, calcined kaolin, synthetic silica, talcum powder, ground calcium carbonate, precipitated calcium carbonate, etc. Compared with plant fibers, fillers are usually lower in cost. Adding fillers can not only reduce the production cost of paper-based materials, but also improve the whiteness, opacity, smoothness, etc. of paper. However, with the addition of fillers in paper-based materials, filler particles will occupy fiber gaps and fiber spaces, hinder the combination of plant fibers and fibers, and reduce the strength of the finished paper.
[0003] Lignin is a macromolecule with a phenylpropane structure. It is the second largest component of plant raw materials besides cellulose. It exists in the cell wall and cell wall of plant fibers. As a binder, it gives plants a certain strength. However, in the extraction of papermaking raw materials and papermaking processes, lignin is usually removed as a foreign matter and exists in pulping black liquor. At present, most lignin is used as fuel and burned in the alkali recovery process, and the high-value utilization rate of lignin is low. However, the special structural characteristics and physical and chemical properties of lignin make it hydrophobic, thermoplastic and adhesive. It comes from natural wood and is applied to the preparation of paper-based materials. Compared with its use as fuel, it effectively promotes the high-value utilization of lignin, reduces production costs and environmental pollution, and saves energy and is environmentally friendly. Its thermoplasticity, adhesiveness and hydrophobicity can make the structure of the prepared paper-based materials more compact, improving the shortcomings of poor mechanical strength and poor barrier properties of traditional paper-based materials. In addition, no harmful chemicals are added during the preparation process, which is highly safe. It can be used in packaging materials and food packaging, replace traditional plastics, make paper cups, medical materials, etc., and replace traditional petroleum-based materials and plastics. Therefore, the application of lignin and the preparation of environmentally friendly paper-based materials have become the focus of current research. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a paper-based material with a high lignin content and a preparation method thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A high lignin content paper-based material using alkali lignin as filler.
[0007] The alkali lignin is prepared by the following method: the alkali lignin raw material pulp is subjected to sulphate method, caustic soda method, alkali anthraquinone method, lime method, oxygen alkali method or ammonia method to obtain black liquor which is subjected to precipitation separation;
[0008] Preferably, the alkali lignin raw material pulp is at least one of coniferous wood pulp, broadleaf wood pulp, hemp pulp, straw pulp, bamboo pulp, sugarcane pulp, cotton pulp and reed pulp.
[0009] The particle size of the alkali lignin is 200nm-40μm, the purity is higher than 85%, and the particle size D50 is greater than 300 meshes.
[0010] The paper-based material comprises the following components in relative weight: 100 parts of absolute dry pulp, 0.5-60 parts of alkali lignin, and 0.1-5 parts of retention and drainage aids. Preferably, the weight of alkali lignin accounts for 5-40% of the air-dried pulp of the absolute dry pulp; more preferably, 5-20%; preferably, the weight of retention and drainage aids accounts for 0.8%-1% of the air-dried pulp of the absolute dry pulp.
[0011] The bone-dry pulp is prepared in the following manner: the paperboard pulp is beaten to 15°SR-80°SR, preferably 35°SR.
[0012] The paperboard pulp board is at least one of natural color coniferous wood pulp board, natural color broadleaf wood pulp board and natural color straw pulp board.
[0013] The retention and drainage aid is at least one of polyaluminium chloride, alum, cationic starch, amphoteric starch, chitosan, polyethyleneimine, polyethylene oxide, polydiallyldimethylammonium chloride, polyamide polyamine-epichlorohydrin and cationic polyacrylamide.
[0014] The present invention also includes a method for preparing the paper-based material, comprising the following steps: 1) adding alkali lignin and retention and drainage aids to absolute dry pulp, dispersing and then making sheets to quantitatively obtain a sheet base; 2) subjecting the sheet base obtained in step 1) to surface sizing treatment; 3) subjecting the sheet base obtained in step 2) to hot pressing treatment.
[0015] The specific steps of step 2) are: prepare a starch solution with a concentration of 6%-8%, apply sizing on the surface with a stick type, and the sizing amount is 6g / m 2 The sizing temperature is 18-45°C; the starch is at least one of native starch, oxidized starch, dialdehyde starch, baked dextrin, esterified starch, etherified starch, and grafted starch; the native starch is at least one of corn starch, potato starch, and sweet potato starch.
[0016] The quantitative requirement in step 1) is 20g / m 2 -160 g / m 2; Preferably, the parameters of the hot pressing treatment in step 3) are: the hot pressing temperature is 110℃-250℃, preferably 160-180℃; the line pressure during hot pressing is 2-80N / mm; preferably 20N / mm-50N / mm; the creeping speed is 0.5m / min-5m / min.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. Alkali lignin comes from natural wood. Compared with traditional inorganic mineral fillers, it has significant advantages in renewability, degradability, energy saving and environmental protection;
[0019] 2. After high temperature hot pressing, the paper base is made by utilizing the thermoplasticity, adhesion, hydrophobicity, etc. of lignin, which makes the paper structure denser, enhances its barrier properties and maintains good mechanical properties;
[0020] 3. Rationally utilize the waste alkali lignin removed from papermaking to overcome the problem that most of it is used as fuel and burned in the alkali recovery process, resulting in low high-value utilization rate;
[0021] 4. No harmful chemicals are added during the preparation of paper-based materials, which are highly safe and can be used in packaging materials and food packaging, making paper cups, medical materials, etc., replacing traditional petroleum-based materials and plastics. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The effect diagram of the withstand voltage index of Examples 1-5;
[0023] Figure 2 This is a rendering of the longitudinal tensile index of Examples 1-5;
[0024] Figure 3 This is a rendering of the transverse tensile index of Examples 1-5;
[0025] Figure 4 This is a rendering of the longitudinal folding times of Examples 1-5;
[0026] Figure 5 This is a rendering of the number of transverse folding endurances of Examples 1-5;
[0027] Figure 6 This is the effect diagram of the contact angle of paper when blank sample 1 is not hot pressed;
[0028] Figure 7 This is a rendering of the contact angle of paper in Example 5 without heat pressing;
[0029] Figure 8 This is a diagram showing the effect of the contact angle of paper when the blank sample 1 of the embodiment is hot pressed at 160°C;
[0030] Fig. 9This is a diagram showing the contact angle of paper during hot pressing at 160°C in Example 5. DETAILED DESCRIPTION
[0031] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiment. The percentages used in this application are all mass percentages unless otherwise specified.
[0032] Unless otherwise specified, all materials used in this application were purchased from Tianjin Wood Elf Biotechnology Co., Ltd.; the alkali lignin in this application was also purchased from Tianjin Wood Elf Biotechnology Co., Ltd., and its particle size distribution is as follows Figure 1 It is shown that the particle size is 200nm-40μm, the purity is higher than 85%; the particle size D50>300 mesh; the alkali lignin can be obtained by evaporating and concentrating the black liquor obtained after pulping by sulfate method, caustic soda method, alkali anthraquinone method, lime method, oxygen alkali method or ammonia method to 3-30 degrees Baume, filtering and then entering the centrifugal atomizer for high-temperature atomization treatment, and then entering the drying tower for drying, and then separating the alkali lignin dry powder by the cyclone separator.
[0033] Example 1
[0034] In this embodiment, alkali lignin is applied to papermaking filler to obtain a paper-based material with a high lignin content. The paper-based material is prepared in the following manner:
[0035] 1) Select the natural dry pulp of softwood, beat it to 35°SR with a Wally beater, sieve out 300-mesh alkali lignin particles, add 5% of the air-dried pulp, and add the retention and drainage aid PE I to 0.8% of the air-dried pulp. After debonding, make sheets with a quantitative of 60 g / m 2 .
[0036] 2) The film base obtained in step 1) is subjected to surface sizing treatment with aldehyde starch; specifically, a 3%-8% aldehyde starch solution is prepared, gelatinized at 90°C for 30 minutes, and the surface is sizing with a rod, with a sizing amount of 6g / m 2 , the gluing temperature is 30℃;
[0037] 3) The film base obtained in step 2) is subjected to hot pressing treatment using a roller hot press at a temperature of 160° C., a line pressure of 50 N / mm, and a creeping speed of 0.5 m / min. The prepared film base is then placed in an international standard constant temperature and humidity environment (temperature of 23±0.5° C., humidity of 50±5% rh) for 24 hours before relevant testing.
[0038] Example 2
[0039] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 1 is that in step 1), the alkali lignin particles are added at 10% of the absolute dry pulp amount, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be repeated here.
[0040] Example 3
[0041] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 1 is that in step 1), the alkali lignin particles are added at 20% of the absolute dry pulp amount, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be repeated here.
[0042] Example 4
[0043] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 1 is that in step 1), the alkali lignin particles are added at 30% of the amount of the air-dried pulp, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be repeated here.
[0044] Example 5
[0045] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 1), the alkali lignin particles are added at 40% of the amount of the air-dried pulp, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be repeated here.
[0046] Blank sample 1: Blank sample 1 is the absolute dry pulp obtained at 35°SR;
[0047] Blank sample 2: The difference between Blank sample 2 and Example 1 is that no lignin particles are added.
[0048] Examples 1-5 show the effects of different amounts of alkali lignin added on paper-based materials. The results show that compared with blank sample 1 and blank sample 2, Figure 1 Before hot pressing, the bursting index gradually decreased with the increase of alkali lignin addition, and the bursting index increased from 8.23 Kpa.m of blank sample 1 to 2 / g to 40% addition and then it drops to 4.12Kpa.m 2 / g, because lignin particles occupy the fiber gaps and fiber space, hindering the combination of plant fibers and fibers, and reducing their strength. After hot pressing, the bursting index is higher than that before pressing, and it can still maintain a good bursting index when the addition amount is 5%-20%. This shows that the partial melting of lignin during hot pressing has a positive effect on the mechanical properties and strength of paper.
[0049] Figure 2Comparing the longitudinal tensile index before and after hot pressing, the tensile index gradually decreased with the increase of alkali lignin addition before hot pressing, and its tensile index dropped from 179.05Nm / g of blank sample 1 to 91.20Nm / g when the addition amount was 40%. When the addition amount was 5-30%, more than 60% of the original tensile strength could be maintained. Although the strength was significantly reduced when the addition amount was 20%-40%, the adhesion of lignin after hot pressing restored some of its strength, and the tensile index after hot pressing increased compared with that before pressing. Figure 3 Comparing the transverse tensile index before and after hot pressing, the tensile index gradually decreased with the addition of alkali lignin before hot pressing, and the tensile index did not change much before and after hot pressing, and slightly increased after hot pressing. The transverse tensile index after hot pressing was the best when the addition amount was 5%-10%. And the original strength level was basically maintained when the addition amount was 10%-30%. This shows that through hot pressing, the melting of lignin during hot pressing has a good effect on improving the mechanical properties of paper.
[0050] Figure 4 Comparing the longitudinal folding resistance before and after hot pressing, the number of folding resistances gradually decreased with the addition of alkali lignin before hot pressing, but it could still reach 517 times at an addition of 40%. After hot pressing, the number of folding resistances increased with the addition of alkali lignin compared with that before hot pressing, and it could still be increased to 891 times at an addition of 40%, which is equivalent to traditional plastic film. ( Figure 5 ) Comparing the transverse folding resistance before and after hot pressing, the folding times before hot pressing gradually decreased with the addition of alkali lignin at 20%-40%, but was better than the blank sample at 5-10%. Although the folding times after hot pressing decreased, the transverse folding resistance could still reach 70 times at the addition of 40%, which was significantly higher than the 30 times before hot pressing. The folding times were higher at the addition of 5%-20%.
[0051] Example 6
[0052] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that the amount of the retention and drainage aid selected in step 1) is 0.1% of the air-dried pulp. The remaining raw materials and methods are the same as those in Embodiment 3 and will not be repeated here.
[0053] Example 7
[0054] This embodiment provides a method for preparing a paper-based material. The difference from Example 3 is that the amount of the retention and drainage aid selected in step 1) is 1% of the air-dried pulp. The remaining raw materials and methods are the same as those in Example 3 and will not be repeated here.
[0055] Example 8
[0056] This embodiment provides a method for preparing a paper-based material. The difference from Example 3 is that the amount of the retention and drainage aid selected in step 1) is 2% of the air-dried pulp. The remaining raw materials and methods are the same as those in Example 3 and will not be repeated here.
[0057] Examples 6-8 show the effects of different retention and drainage aid addition amounts on paper-based materials. The results show that because lignin particles are negatively charged, adding too little retention and drainage aid will cause less fine lignin particles to remain in the paper (retention <30%), while adding too much will cause pulp flocculation, affecting the uniformity of the finished paper, and further having an adverse effect on its mechanical properties, etc. Therefore, 0.8%-1% is selected as its preferred form.
[0058] Example 9
[0059] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 3), the paper hot pressing temperature is 80° C., and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0060] Example 10
[0061] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 3), the paper hot pressing temperature is 180° C., and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0062] Embodiment 11
[0063] This embodiment provides a method for preparing a paper-based material. The difference from the embodiment 3 is that the paper hot pressing temperature in step 3) is 260° C., and the other raw materials and methods are the same as those in the embodiment 3, which will not be described in detail here.
[0064] Examples 9-11 show the effects of different hot pressing temperatures on paper-based materials. The results show that when the temperature is too low, the glass transition temperature of lignin cannot be reached, thereby affecting its mechanical properties, while when the temperature is too high, the stability of the starch coating is destroyed, affecting the barrier properties of the paper after hot pressing. Therefore, a hot pressing temperature of 160-180°C is preferred.
[0065] Example 12
[0066] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 3), the linear pressure of the paper hot pressing roller is 5 N / mm, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0067] Embodiment 13
[0068] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 3), the linear pressure of the paper hot pressing roller is 20 N / mm, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0069] Embodiment 14
[0070] This embodiment provides a method for preparing a paper-based material. The difference from Embodiment 3 is that in step 3), the linear pressure of the paper hot pressing roller is 60 N / mm, and the remaining raw materials and methods are the same as those in Embodiment 3, which will not be described again.
[0071] Examples 12-14 show the effects of different roller pressures on paper-based materials. The results show that when the pressure is too low, the lignin cannot be squeezed into sheets to fill the fiber gaps in coordination with the temperature, thereby affecting its mechanical properties. Excessive pressure destroys the fiber lumen and causes crushing, which affects the mechanical properties of the paper after hot pressing. Therefore, 20N / mm-50N / mm is the preferred form.
[0072] Evaluation of the properties of the paper-based material
[0073] Various physical property tests were performed on the bases of Examples 1 to 5 and the control bases without adding alkali lignin particles (blanks 1 and 2) and without heat pressing.
[0074] 1. Determination of mechanical strength before and after hot pressing
[0075] The mechanical properties of the film bases prepared in Examples 1 to 5 and blank samples 1 and 2 were tested before and after calendering. The film bases were placed in an international standard constant temperature and humidity environment (temperature 23±0.5°C, humidity 50±5% rh) for 24 hours before relevant tests. The tensile strength was measured using a tensile strength meter (B0660005, Lorentzen & Wettre, Sweden); the number of folding times was measured using a folding endurance meter; the bursting endurance was measured using a bursting endurance meter (Lorentzen & Wettre, Sweden); each sample was tested three times, and the average value was recorded. Figures 1 to 5 The figure is a data chart of the bursting index, tensile index and folding times of the paper of Examples 1-5 and blank samples 1 and 2 before and after hot pressing.
[0076] 2. Determination of water resistance before and after hot pressing of sheets
[0077] The water resistance of the sheets prepared in Examples 1-5 and Blank Sample 2 was tested before and after calendering. The static water contact angle of the paper before and after calendering was measured at room temperature using a PGX contact angle meter (AST Products, Inc, USA).
[0078] By measuring the effect of different alkali lignin additions on the barrier properties of paper-based materials before and after hot pressing, Figure 6 This is the effect diagram of the contact angle of paper when blank sample 1 is not hot pressed; Figure 7 This is a rendering of the contact angle of paper in Example 5 without heat pressing; Figure 8 This is a diagram showing the effect of the contact angle of paper when the blank sample 1 of the embodiment is hot pressed at 160°C; Fig. 9This is a diagram showing the contact angle of paper during hot pressing at 160°C in Example 5.
[0079] The contact angle results show that the blank sample (blank sample 1) before hot pressing has an initial contact angle of 40°, and the water absorption time is 5s. The sample with 40% added (Example 5) has an initial contact angle of 58.10°, and the water absorption time is 16s. The blank sample (blank sample 1) after hot pressing has an initial contact angle of 91.19°, and the contact angle is 80.53° after 10 minutes. The sample with 40% added has an initial contact angle of 112.49°, and the contact angle is maintained at 104.36° after 10 minutes. Similarly, the addition amount is 5%, 10%, 20%, and 30%, whether it is the initial contact angle or the water absorption time, there are different degrees of improvement. The results show that the addition of lignin can play a positive role in the barrier properties of paper-based materials.
[0080] In summary, compared with the prior art, the technical solution of the present invention:
[0081] 1. Alkali lignin comes from natural wood. Compared with traditional inorganic mineral fillers, it has significant advantages in renewability, degradability, energy saving and environmental protection;
[0082] 2. After high temperature hot pressing, the paper base is made by utilizing the thermoplasticity, adhesion, hydrophobicity, etc. of lignin, which makes the paper structure denser, enhances its barrier properties and maintains good mechanical properties;
[0083] 3. Rationally utilize the waste alkali lignin removed from papermaking to overcome the problem that most of it is used as fuel and burned in the alkali recovery process, resulting in low high-value utilization rate;
[0084] 4. No harmful chemicals are added during the preparation of paper-based materials, which are highly safe and can be used in packaging materials and food packaging, making paper cups, medical materials, etc., replacing traditional petroleum-based materials and plastics.
[0085] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A paper-based material with a high lignin content, characterized in that: Alkali lignin was used as filler.
2. The paper-based material with high lignin content according to claim 1, characterized in that: The alkali lignin is prepared by the following method: the alkali lignin raw material pulp is subjected to sulphate method, caustic soda method, alkali anthraquinone method, lime method, oxygen alkali method or ammonia method to obtain black liquor which is subjected to precipitation separation; Preferably, the alkali lignin raw material pulp is at least one of coniferous wood pulp, broadleaf wood pulp, hemp pulp, straw pulp, bamboo pulp, sugarcane pulp, cotton pulp and reed pulp.
3. The paper-based material with high lignin content according to claim 1, characterized in that: The particle size of the alkali lignin is 200nm-40μm, the purity is higher than 85%, and the particle size D50 is greater than 300 meshes.
4. The paper-based material with high lignin content according to claim 1, characterized in that: The invention comprises the following components in relative weight proportions: 100 parts of absolute dry pulp, 0.5-60 parts of alkali lignin, and 0.1-5 parts of retention and filtering aids; preferably, the weight proportion of alkali lignin is 5-40% of the air-dried pulp of the absolute dry pulp; more preferably, it is 5-20%; preferably, the weight proportion of retention and filtering aids is 0.8%-1% of the air-dried pulp of the absolute dry pulp.
5. The paper-based material with high lignin content according to claim 4, characterized in that: The bone-dry pulp is prepared in the following manner: the paperboard pulp is beaten to 15°SR-80°SR, preferably 35°SR.
6. The paper-based material according to claim 5, characterized in that: The paperboard pulp board is at least one of natural color coniferous wood pulp board, natural color broadleaf wood pulp board and natural color straw pulp board.
7. The paper-based material with high lignin content according to claim 4, characterized in that: The retention and drainage aid is at least one of polyaluminium chloride, alum, cationic starch, amphoteric starch, chitosan, polyethyleneimine, polyethylene oxide, polydiallyldimethylammonium chloride, polyamide polyamine-epichlorohydrin and cationic polyacrylamide.
8. A method for preparing a paper-based material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: 1) adding alkali lignin and retention and drainage aids into the absolute dry pulp, dispersing and then making sheets to quantitatively obtain sheet base; 2) performing surface sizing treatment on the sheet base obtained in step 1); 3) performing hot pressing treatment on the sheet base obtained in step 2).
9. The method for preparing a paper-based material according to claim 8, characterized in that: The specific steps of step 2) are: prepare starch solution, apply sizing agent on the surface with a sizing amount of 6g / m 2 The sizing temperature is 18-45°C; the starch is at least one of native starch, oxidized starch, dialdehyde starch, baked dextrin, esterified starch, etherified starch, and grafted starch; the native starch is at least one of corn starch, potato starch, and sweet potato starch.
10. The method for preparing a paper-based material according to claim 8, characterized in that: The quantitative requirement in step 1) is 20g / m 2 -160 g / m 2 ; Preferably, the parameters of the hot pressing treatment in step 3) are: hot pressing temperature is 110℃-250℃; preferably 160-180℃; line pressure during hot pressing is 2-80N / mm; preferably 20N / mm-50N / mm; creeping speed is 0.5m / min-5m / min.
Citation Information
Patent Citations
Method for producing non-formaldehyde environment-friendly particle boards by utilizing alkali lignin as binder
CN103358385A
Method for making high-strength paper by adding compound lignin
CN110067146A
Preparation method and application of biodegradable cellulose paper taking lignin as adhesive
CN114016323A
Process for producing a flat, printed component
DE102007013133A1
Compound board material has a matrix of cellulose fibers with a lignin solution as a bonding agent and the material is impregnated with a natural polymer for strength and impact force resistance
DE19852029A1
Cited By
Preparation process of environment-friendly degradable thermo-sensitive paper for food
CN119194915A
Preparation process of environment-friendly degradable heat-sensitive paper for food
CN119194915B
Preparation method and application of quaternary ammonium salt type lignin waterproof and oil-proof agent
CN119372952A