Method for testing mechanical property of fiber gridding cloth reinforced concrete composite material
By preparing and loading test pieces in the mechanical properties test of fiber mesh reinforced concrete composite materials and monitoring their deformation values, the problem of difficulty in accurately evaluating the mechanical properties of materials in the prior art is solved, and pulling of different fibers and mortars is achieved Research on the mechanism of extension failure provides an accurate experimental reference for structural reinforcement design.
Patent Information
- Application Number
- CN202410920713.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
In the mechanical properties test of fiber mesh cloth reinforced concrete composite materials, it is difficult for the prior art to accurately evaluate the tensile failure mechanism and component failure model of different fibers, layers and mortars, which affects the accuracy of structural reinforcement design.
By preparing long fiber mesh cloth, reinforced concrete composite specimens and loading them uniformly and continuously on the mechanical testing machine. Combined with the test piece deformation measurement system to monitor deformation values, record load values and deformation data, improve testing accuracy and reliability sex.
The precise test of the mechanical properties of fiber mesh cloth reinforced concrete composite materials is realized, and the tensile failure mechanism of different fibers, layers and mortars is explored, providing experimental reference for structural reinforcement design, and improving the testing accuracy and application reliability.
Smart Images

Figure CN118883202A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of composite material testing, and in particular to a method for testing the mechanical properties of a fiber mesh cloth reinforced concrete composite material. Background Art
[0002] As a new type of fiber-reinforced cement-based composite material, Textile Reinforced Mortar (TRM) composite material has attracted wide attention in recent years due to its high crack resistance, impact resistance, and simple construction process. In the mechanical property test of TRM composite material, tensile test is an important means to evaluate the tensile strength and deformation performance of the material.
[0003] At present, TRM composite materials have achieved remarkable applications in the engineering field, including: using TRM composite materials to reinforce structures in civil engineering, effectively improving the tensile bearing capacity of the structure and delaying structural aging; bridge maintenance, through its high strength and durability, improving the bearing capacity and service life of the bridge structure; providing solutions for different protection needs in coastal protection, slope protection, etc.; therefore, it is necessary to conduct mechanical property testing on it to determine its mechanical properties so that it can be applied to different fields. Summary of the invention
[0004] An embodiment of the present invention provides a method for testing the mechanical properties of a fiber mesh cloth reinforced concrete composite material. When the mechanical properties of the fiber mesh cloth reinforced concrete composite material are tested, corresponding test specimens are prepared in advance according to the test parameters, thereby improving the test accuracy. At the same time, different test specimens can be made according to needs, and the tensile failure mechanism and component failure model of the test specimens with different fibers, different numbers of layers, and different mortars can be explored, providing an experimental reference for structural reinforcement design.
[0005] In a first aspect, the present invention provides a method for testing the mechanical properties of a fiber mesh reinforced concrete composite material, comprising:
[0006] Prepare long strip fiber mesh cloth reinforced concrete composite material specimens;
[0007] The two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine through a clamp respectively;
[0008] Installing a specimen deformation measurement system, wherein the composite specimen is located within a monitoring range of the specimen deformation measurement system to monitor the deformation value of the composite specimen;
[0009] The mechanical testing machine and the specimen deformation measuring system are operated to uniformly and continuously load the composite material specimen, and the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen are recorded.
[0010] Optionally, preparing a long fiber mesh cloth reinforced concrete composite material specimen includes:
[0011] Assembling the mold and applying a concrete isolation agent on the inner surface of the mold;
[0012] pouring a first mortar layer inside the mold, and smoothing the top of the first mortar layer;
[0013] Placing a first galvanized iron mesh on the top surface of the first mortar layer, and pressing the first galvanized iron mesh tightly so that at least a portion of the first mortar layer passes through the first galvanized iron mesh;
[0014] Placing a fiber mesh cloth on the top surface of the first galvanized iron mesh;
[0015] Placing a second galvanized iron mesh sheet on the top surface of the fiber mesh cloth, and pressing the second galvanized iron mesh tightly, so that at least a portion of the first mortar layer passes through the first galvanized iron mesh, the fiber mesh cloth, and the second galvanized iron mesh in sequence;
[0016] pouring a second mortar layer on the top surface of the second galvanized iron mesh, and smoothing the top of the second mortar layer;
[0017] The composite material specimen is demoulded and cured to obtain the composite material specimen.
[0018] Optionally, the first mortar layer and the second mortar layer have the same thickness, both in the range of 4.5-5.5 mm.
[0019] Optionally, after pouring the second mortar layer on the top surface of the second galvanized iron mesh, before demoulding the composite material specimen and curing and solidifying to obtain the composite material specimen, the method further includes:
[0020] Cover the top of the second mortar layer with plastic film.
[0021] Optionally, after demoulding and curing the composite material specimen to obtain the composite material specimen, one end of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction is clamped on the upper crossbeam of the mechanical testing machine through a clamp, and the other end of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction is clamped on the lower crossbeam of the mechanical testing machine through a clamp, the method further includes:
[0022] Aluminum plates are respectively attached to the first side and the second side of the composite material specimen; the first side and the second side are the two opposite sides of the composite material specimen in the thickness direction.
[0023] Optionally, before one end of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction is clamped on the upper crossbeam of the mechanical testing machine by a clamp, and the other end of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction is clamped on the lower crossbeam of the mechanical testing machine by a clamp, the method further includes:
[0024] The fixture is installed on the mechanical testing machine.
[0025] Optionally, the clamp includes a first clamp and a second clamp; the first clamp and the second clamp each include a first side clamp and a second side clamp disposed in parallel, and a plurality of anti-slip grooves are disposed on a surface of the first side clamp and the second side clamp on a side close to each other; a plurality of second bolt holes and a first bolt hole are disposed on a surface of the first side clamp and the second side clamp;
[0026] Install the fixture on the mechanical testing machine, including:
[0027] Extend the upper crossbeam connecting rod of the mechanical testing machine between the first side clamping plate and the second side clamping plate of the first clamping member, and use a bolt to sequentially penetrate the first bolt hole of the first side clamping plate, the bolt hole of the upper crossbeam connecting rod, and the first bolt hole of the second side clamping plate to install the first clamping member on the upper crossbeam of the mechanical testing machine;
[0028] Extend the lower crossbeam connecting rod of the mechanical testing machine between the first side clamping plate and the second side clamping plate of the second clamping member, and use a bolt to sequentially penetrate the first bolt hole of the first side clamping plate, the bolt hole of the lower crossbeam connecting rod and the first bolt hole of the second side clamping plate to install the second clamping member on the lower crossbeam of the mechanical testing machine;
[0029] The two ends of the long fiber mesh cloth reinforced concrete composite material specimen in the extension direction are respectively clamped on a mechanical testing machine by means of a clamp, including:
[0030] Disassembling the clamping plates on the same side of the first clamping member and the second clamping member;
[0031] The first side surfaces of the two ends of the elongated fiber mesh reinforced concrete composite material specimen in the extension direction are respectively pressed against the side surfaces of the clamping plates on the undisassembled side of the first clamping member and the second clamping member, where the anti-slip grooves are arranged;
[0032] installing the clamping plate with the first clamping member and the second clamping member removed;
[0033] The multiple second bolt holes of the first side clamp in the first clamp are bolted to the multiple second bolt holes of the second side clamp, and the multiple second bolt holes of the first side clamp in the second clamp are bolted to the multiple second bolt holes of the second side clamp, so as to fix the long fiber mesh cloth reinforced concrete composite material specimen to the first clamp and the second clamp at both ends of the extension direction, respectively.
[0034] Optionally, the specimen deformation measurement system comprises a contact extensometer and an extensometer bracket; the gauge length of the extensometer bracket is greater than or equal to 300 mm;
[0035] Install the specimen deformation measurement system, including:
[0036] A contact extensometer is installed on both sides of the long fiber mesh cloth reinforced concrete composite material specimen in the thickness direction through the extensometer bracket.
[0037] Optionally, the specimen deformation measurement system comprises a digital image correlation method non-contact extensometer;
[0038] Before operating the mechanical testing machine and the specimen deformation measurement system, the method further includes:
[0039] Speckles are sprayed on the surface of the long strip fiber mesh cloth reinforced concrete composite material specimen.
[0040] Optionally, the mechanical testing machine and the specimen deformation measuring system are operated, and before the mechanical testing machine and the specimen deformation measuring system are operated to uniformly and continuously load the composite material specimen, and record the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen, the method further includes:
[0041] The mechanical testing machine and the specimen deformation measurement system are operated to preload the composite specimen, and when the deformation parameter of the composite specimen exceeds a preset change rate, the position of the fixture holding the composite specimen is adjusted.
[0042] A method for testing the mechanical properties of a fiber mesh cloth reinforced concrete composite material provided by an embodiment of the present invention comprises the following steps: first, preparing a long fiber mesh cloth reinforced concrete composite material specimen; then, clamping the two ends of the long fiber mesh cloth reinforced concrete composite material specimen in the extension direction on the upper beam and the lower beam of a mechanical testing machine through a clamp; installing a specimen deformation measurement system, and the composite material specimen is located within the monitoring range of the specimen deformation measurement system to monitor the deformation value of the composite material specimen; finally, operating the mechanical testing machine and the specimen deformation measurement system to uniformly and continuously load the composite material specimen, and recording the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen; in the above technical scheme, when testing the mechanical properties of the fiber mesh cloth reinforced concrete composite material, the corresponding specimen is prepared in advance according to the test parameters, thereby improving the test accuracy; at the same time, different specimens can be made according to needs, and then the tensile failure mechanism and component failure model of the specimen with different fibers, different numbers of layers, and different mortars can be explored, providing an experimental reference for structural reinforcement design. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0044] Figure 1 It is a schematic flow chart of a method for testing mechanical properties of a fiber mesh cloth reinforced concrete composite material provided by an embodiment of the present invention;
[0045] Figure 2 is a structural schematic diagram of an integrated mold provided by an embodiment of the present invention;
[0046] Figure 3 It is a schematic structural diagram of a fiber mesh cloth reinforced concrete composite material specimen provided by an embodiment of the present invention;
[0047] Figure 4 is a structural schematic diagram of a clamping member provided by an embodiment of the present invention;
[0048] Figure 5 yes Figure 4 A front structural diagram of the clamp shown;
[0049] Figure 6 It is a schematic diagram of the connection between a fixture, a mechanical testing machine and a composite material test piece provided by an embodiment of the present invention;
[0050] Figure 7 It is a schematic diagram of connecting a contact extensometer and a composite material specimen provided by an embodiment of the present invention;
[0051] Figure 8 is a schematic diagram of tensile stress-strain curves of a composite material specimen at different temperatures provided by an embodiment of the present invention;
[0052] Fig. 9 It is a schematic diagram of a non-contact extensometer monitoring a composite material test piece provided by an embodiment of the present invention;
[0053] Fig.10 It is a schematic diagram of a tensile stress-strain curve of a composite material specimen provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0054] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0055] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. It should be noted that the directional words such as "upper", "lower", "left", "right" and the like described in the embodiments of the present invention are described at the angles shown in the accompanying drawings and should not be understood as limitations on the embodiments of the present invention. In addition, in the context, it is also necessary to understand that when it is mentioned that an element is formed "on" or "under" another element, it can not only be directly formed "on" or "under" another element, but also indirectly formed "on" or "under" another element through an intermediate element. The terms "first", "second", etc. are only used for descriptive purposes and do not represent any order, quantity or importance, but are only used to distinguish different components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood in specific circumstances.
[0056] The term “including” and its variations used in the present invention are open inclusions, that is, “including but not limited to.” The term “based on” means “based at least in part on.” The term “one embodiment” means “at least one embodiment.”
[0057] It should be noted that the concepts such as "first" and "second" mentioned in the present invention are only used to distinguish the corresponding contents, and are not used to limit the order or interdependence.
[0058] It should be noted that the modifications of "one" and "plurality" mentioned in the present invention are illustrative rather than restrictive, and those skilled in the art should understand that, unless otherwise clearly indicated in the context, it should be understood as "one or more".
[0059] Figure 1is a flow chart of a method for testing the mechanical properties of a fiber mesh reinforced concrete composite material provided by an embodiment of the present invention, with reference to Figure 1 , the method comprising:
[0060] S110. Prepare long strip fiber mesh cloth reinforced concrete composite material specimens.
[0061] Specifically, fiber mesh cloth reinforced mortar composite material, as a new type of fiber reinforced cement-based composite material, has the advantages of high crack resistance, impact resistance, and simple construction process, and has received widespread attention in various fields. Therefore, it is necessary to measure its mechanical performance parameters, especially tensile properties, in order to apply it to different fields; therefore, it is necessary to first prepare long strips of fiber mesh cloth reinforced concrete composite material specimens in order to perform tensile tests on the composite material to test its tensile properties. In other embodiments of the present invention, the shape of the composite material specimen can be specifically set according to different mechanical property tests, and this is not limited.
[0062] S120, clamping the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction on the upper beam and the lower beam of the mechanical testing machine through a clamp.
[0063] Specifically, in order to test the tensile properties of the fiber mesh cloth reinforced concrete composite material specimen, the two ends of the elongated composite material specimen in the extension direction need to be clamped on the upper beam and the lower beam of the mechanical testing machine through clamps, so as to stretch the composite material specimen by controlling the relative movement of the upper beam and the lower beam.
[0064] S130. Install a specimen deformation measurement system, wherein the composite specimen is located within a monitoring range of the specimen deformation measurement system to monitor a deformation value of the composite specimen.
[0065] Specifically, in order to obtain the deformation parameters of the composite specimen under load, it is also necessary to install a specimen deformation measurement system and place the composite specimen within the monitoring range of the specimen deformation measurement system to monitor the deformation value of the composite specimen.
[0066] S140. Operate the mechanical testing machine and the specimen deformation measurement system to uniformly and continuously load the composite material specimen, and record the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen.
[0067] Specifically, after the composite material specimen is prepared and clamped in the mechanical testing machine, the mechanical testing machine is operated to stretch the two ends of the composite material specimen, and the composite material specimen is uniformly and continuously loaded so that the composite material specimen is deformed in the stretching direction; at the same time, the specimen deformation measurement system is operated to monitor the deformation changes of the composite material specimen under continuous loading.
[0068] A method for testing the mechanical properties of a fiber mesh cloth reinforced concrete composite material provided by an embodiment of the present invention comprises the following steps: first, preparing a long fiber mesh cloth reinforced concrete composite material specimen; then, clamping the two ends of the long fiber mesh cloth reinforced concrete composite material specimen in the extension direction on the upper beam and the lower beam of a mechanical testing machine through a clamp; installing a specimen deformation measurement system, and the composite material specimen is located within the monitoring range of the specimen deformation measurement system to monitor the deformation value of the composite material specimen; finally, operating the mechanical testing machine and the specimen deformation measurement system to uniformly and continuously load the composite material specimen, and recording the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen; in the above technical scheme, when testing the mechanical properties of the fiber mesh cloth reinforced concrete composite material, the corresponding specimen is prepared in advance according to the test parameters, thereby improving the test accuracy; at the same time, different specimens can be made according to needs, and then the tensile failure mechanism and component failure model of the specimen with different fibers, different numbers of layers, and different mortars can be explored, providing an experimental reference for structural reinforcement design.
[0069] It should be noted that after the test, all kinds of instrument equipment need to be dismantled and the composite specimens need to be unloaded from the mechanical testing machine.
[0070] Optionally, the above step S110, preparing a long strip fiber mesh cloth reinforced concrete composite material specimen, comprises:
[0071] Assemble the mold and apply concrete isolation agent to the inner surface of the mold.
[0072] Specifically, Figure 2 is a schematic diagram of the structure of an integrated mold provided by an embodiment of the present invention, with reference to Figure 2 In order to prepare multiple test pieces at the same time, the integrated mold includes multiple identical molds 10, each mold 10 has the same internal shape, and can prepare the same composite material test pieces; that is, using the integrated mold, multiple identical composite material test pieces can be prepared at the same time, thereby improving the test efficiency. The mold bottom plate is made of acrylic material, and the surrounding frames can be made of bamboo so that the frame and the bottom plate fit better. The bolts are nailed to the bottom plate with nails, and the nail spacing is about 150mm. Concrete isolation agent is applied to the inner surface of the mold 10 to prevent the concrete from sticking to the inside of the mold.
[0073] Pour the first mortar layer inside the mold and smooth the top of the first mortar layer.
[0074] Specifically, Figure 3 is a schematic diagram of the structure of a fiber mesh reinforced concrete composite material specimen provided by an embodiment of the present invention, with reference to Figure 3 The mortar is the matrix material of the composite material, so a first mortar layer 20 is poured inside the mold as the base of the specimen.
[0075] A first galvanized iron mesh is placed on the top surface of the first mortar layer, and the first galvanized iron mesh is pressed tightly so that at least a portion of the first mortar layer passes through the first galvanized iron mesh.
[0076] Specifically, in order to prevent inaccurate test results caused by specimen breakage, the method uses galvanized iron mesh to reinforce the inside of the specimen to enhance the strength and rigidity of the clamping end, so that the specimen can still be efficiently and accurately subjected to tensile tests after pretreatment (such as high temperature treatment, alkaline environment corrosion). Therefore, it is necessary to place a first galvanized iron mesh 30 on the top surface of the first mortar layer 20, and to press the first galvanized iron mesh 30 so that at least a portion of the first mortar layer 20 passes through the first galvanized iron mesh 30, so that the next layer of material is fixed to the first galvanized iron mesh 30 through the mortar.
[0077] A fiber mesh cloth is placed on the top surface of the first galvanized iron mesh sheet.
[0078] A second galvanized iron mesh sheet is placed on the top surface of the fiber mesh cloth, and the second galvanized iron mesh is pressed tightly so that at least a portion of the first mortar layer passes through the first galvanized iron mesh, the fiber mesh cloth, and the second galvanized iron mesh in sequence.
[0079] Specifically, a second galvanized iron mesh 50 is placed on the top surface of the fiber mesh cloth 40 and pressed tightly. At this time, at least a portion of the first mortar layer 20 passes through the first galvanized iron mesh 30, the fiber mesh cloth 40 and the second galvanized iron mesh 50 in sequence, that is, the first galvanized iron mesh 30, the fiber mesh cloth 40 and the second galvanized iron mesh 50 are connected through the first mortar layer 20.
[0080] Pour the second mortar layer on the top surface of the second galvanized iron mesh, and smooth the top of the second mortar layer.
[0081] Specifically, a second mortar layer 60 is poured on the top surface of the second galvanized iron mesh 50, and the top of the second mortar layer 60 is smoothed, and the second mortar layer 60 is fixed to the first mortar layer 20 that passes through the second galvanized iron mesh 50, thereby forming a composite material test piece. The first mortar layer 20 and the second mortar layer 60 have the same thickness, both in the range of 4.5-5.5 mm, so that the size of the test piece is appropriate, and it will not be too short to affect the firmness of clamping with the mechanical testing machine, and it will not be too long to cause mismatch with the mechanical testing machine.
[0082] The composite material specimen is demoulded and cured to obtain the composite material specimen.
[0083] Specifically, the prepared specimens were demoulded after about 48 hours and placed in a standard curing room for curing. The specimens were placed sideways during curing. The exact demoulding time should be determined according to the properties of the mortar. Because the specimens were thin, excessive vibration during demoulding could damage the specimens.
[0084] Optionally, after pouring the second mortar layer on the top surface of the second galvanized iron mesh, before demoulding the composite material specimen and curing and solidifying to obtain the composite material specimen, the method further includes:
[0085] A plastic film is covered on the top of the second mortar layer 60. Specifically, the plastic film can prevent the mortar from shrinking due to water loss, thereby affecting the mechanical performance parameters of the test piece in subsequent experiments.
[0086] Optionally, after demoulding and curing the composite material specimen to obtain the composite material specimen, the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine by a clamp, and the method further includes:
[0087] Aluminum plates are respectively attached to the first side and the second side of the composite material specimen; the first side and the second side are two opposite sides of the composite material specimen in the thickness direction.
[0088] Specifically, after the composite material specimen is prepared, both ends of the specimen need to be stretched to test its mechanical properties. Furthermore, in order to improve the stress environment of the composite material specimen and make the composite material specimen evenly stressed during the stretching process, aluminum plates are also pasted on the two opposite surfaces of the composite material specimen in the thickness direction to reinforce the specimen.
[0089] Optionally, before the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine by means of a clamp, the method further includes:
[0090] Install the fixture on the mechanical testing machine.
[0091] Specifically, the clamp includes a first clamp and a second clamp, so as to respectively clamp the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction. Figure 4 is a schematic diagram of the structure of a clamping member provided by an embodiment of the present invention, with reference to Figure 4 The first clamping member and the second clamping member each include a first side clamping plate 01 and a second side clamping plate 02 arranged in parallel, and a plurality of anti-slip grooves 011 are arranged on the surfaces of the first side clamping plate 01 and the second side clamping plate 02 which are close to each other; Figure 5 yes Figure 4 Front view of the clamp shown, see Figure 5 A plurality of second bolt holes 012 and a first bolt hole 013 are provided on the surface of the first side clamping plate 01 and the surface of the second side clamping plate 02 .
[0092] Install the fixture on the mechanical testing machine, including:
[0093] The upper crossbeam connecting rod of the mechanical testing machine is extended between the first side clamp and the second side clamp of the first clamp, and a bolt is used to penetrate the first bolt hole of the first side clamp, the bolt hole of the upper crossbeam connecting rod and the first bolt hole of the second side clamp in sequence to install the first clamp on the upper crossbeam of the mechanical testing machine.
[0094] Specifically, since the first clamping member includes the first side clamping plate 01 and the second side clamping plate 02, that is, the first side clamping plate 01 and the second side clamping plate 02 are used to clamp the top of the test piece. Figure 6 is a schematic diagram of a connection between a fixture, a mechanical testing machine and a composite material specimen provided by an embodiment of the present invention, with reference to Figure 6 , it is necessary to relatively fix the first side clamp 01 and the second side clamp 02 of the first clamp on the upper crossbeam connecting rod 80 of the mechanical testing machine, so the upper crossbeam connecting rod 80 of the mechanical testing machine is inserted between the first side clamp 01 and the second side clamp 02 of the first clamp, and a bolt is used to sequentially penetrate the first bolt hole 013 of the first side clamp 01, the bolt hole 801 of the upper crossbeam connecting rod 80, and the first bolt hole 013 of the second side clamp. Among them, the first bolt hole 013 of the first side clamp 01 is set at the top position of the first side clamp, and the first bolt hole 013 of the second side clamp 02 is set at the top position of the second side clamp 02, so after the top of the first clamp is fixed to the upper crossbeam of the mechanical testing machine, the test piece is supported by the lower half.
[0095] Extend the lower crossbeam connecting rod of the mechanical testing machine between the first side clamping plate and the second side clamping plate of the second clamping member, and use a bolt to pass through the first bolt hole of the first side clamping plate, the bolt hole of the lower crossbeam connecting rod and the first bolt hole of the second side clamping plate in sequence to install the second clamping member on the lower crossbeam of the mechanical testing machine;
[0096] For details, please refer to Figure 6 Since the second clamp needs to support the other end of the test piece, the second clamp is fixed to the lower crossbeam connecting rod 90 of the mechanical testing machine. The first side clamp 01 and the lower half of the second side clamp 02 are provided with a first bolt hole 013. A bolt is used to penetrate the first bolt hole 013 of the first side clamp, the bolt hole 901 of the lower crossbeam connecting rod 90 and the first bolt hole 013 of the second side clamp in sequence to install the second clamp on the lower crossbeam of the mechanical testing machine, so that the test piece is clamped by the upper half of the first side clamp 01 and the second side clamp 02 of the second clamp.
[0097] The two ends of the long fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the mechanical testing machine by clamps, including:
[0098] Remove the clamping plates on the same side of the first and second clamping members.
[0099] Specifically, in order to clamp the specimen on the mechanical testing machine through the clamp, that is, to clamp the two ends of the specimen by the two clamps of the first clamp and the two clamps of the second clamp respectively, it is necessary to first remove the clamps on the same side of the first clamp and the second clamp so as to clamp the two ends of the specimen between the two clamps.
[0100] The first side surfaces of the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are respectively pressed against the side surface of the clamping plate on the undisassembled side in the first clamp and the second clamp, where the anti-slip groove is arranged.
[0101] For details, please refer to Figure 6 Since the anti-slip groove 011 is provided on one side of the two oppositely arranged clamping plates of the clamp, the first side surfaces of the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are respectively pressed against the anti-slip grooves 011 of the first clamp and the second clamp, thereby improving the clamping firmness.
[0102] Install the clamping plate from which the first clamp and the second clamp are removed.
[0103] For details, please refer to Figure 6 , use bolts to connect the first bolt hole 013 of the disassembled plate of the first clamp with the bolt hole 801 of the upper beam connecting rod 80 of the testing machine and the first bolt hole of the clamp on the side that has not been disassembled, and use bolts to connect the first bolt hole 013 of the disassembled plate of the second clamp with the bolt hole 901 of the lower beam connecting rod of the testing machine and the first bolt hole 013 of the clamp on the side that has not been disassembled.
[0104] The multiple second bolt holes of the first side clamp in the first clamp are bolted to the multiple second bolt holes of the second side clamp, and the multiple second bolt holes of the first side clamp in the second clamp are bolted to the multiple second bolt holes of the second side clamp, so as to fix the long fiber mesh cloth reinforced concrete composite material specimen to the first clamp and the second clamp at both ends of the extension direction, respectively.
[0105] Specifically, in order to prevent the specimen from falling off the fixture due to loose clamping when the mechanical testing machine loads the specimen, it is necessary to further fix the first side clamp 01 and the second side clamp 02 in the first clamp, that is, use bolts to connect the multiple second bolt holes 012 of the first side clamp 01 and the multiple second bolt holes 012 of the second side clamp; at the same time, use bolts to connect the multiple second bolt holes 012 of the first side clamp and the multiple second bolt holes 012 of the second side clamp in the second clamp, so as to further increase the firmness of the two ends of the specimen and the clamp; the torque of the bolt accommodated in the second bolt hole 012 can be adjusted to adjust the distance between the two clamps to adapt to composite material specimens of different sizes.
[0106] Optionally, Figure 7 It is a schematic diagram of connecting a contact extensometer and a composite material specimen provided by an embodiment of the present invention. The specimen deformation measurement system includes a contact extensometer 201 and an extensometer bracket 202; the gauge length of the extensometer bracket 202 is greater than or equal to 300 mm.
[0107] Install the specimen deformation measurement system, including:
[0108] A contact extensometer is installed on both sides of the long fiber mesh cloth reinforced concrete composite material specimen in the thickness direction through an extensometer bracket.
[0109] Exemplarily, when conducting a uniaxial tensile test after high-temperature heating of carbon fiber reinforced mortar, a composite material specimen is first prepared, wherein the specimen material is glass fiber mesh cloth, cement mixed mortar, and galvanized iron mesh (100x60 mm); the prepared specimen is cured in the mold for 72 hours, and after demolding, it is placed in a concrete curing room for standard curing. After the curing is completed. The specimen is placed in a high-temperature furnace for heating, with a target temperature of 100°C, 200°C, and 300°C. After the specimen is heated for 8 hours, the heating is stopped, and the specimen is allowed to cool naturally in the furnace. After the specimen is taken out, the aluminum plate is glued with epoxy resin glue and allowed to solidify. Then the specimen is installed for a tensile test. First, the fixture is connected to the testing machine, and then the specimen is installed. Among them, the torque of each screw accommodated in the second bolt hole is 9.5Nm. After the specimen is installed, the extensometer and the large-gauge extensometer bracket are used to measure the deformation, and the test is started after adjusting various parameters. Figure 8 is a schematic diagram of tensile stress-strain curves of a composite material specimen at different temperatures provided by an embodiment of the present invention, with reference to Figure 8 The tensile test uses displacement control to apply load at a speed of 0.2 mm / min until the time failure. Figure 8 The tensile stress-strain curves of the specimens at 20°C, 100°C, 200°C and 300°C are shown, thereby obtaining the mechanical properties parameters of the composite specimens at different temperatures.
[0110] Optionally, the specimen deformation measurement system includes a digital image correlation method non-contact extensometer; Fig. 9 is a schematic diagram of a non-contact extensometer monitoring a composite material specimen provided by an embodiment of the present invention, with reference to Fig. 9 , the composite material specimen is located within the monitoring range of the non-contact extensometer 300.
[0111] Before operating the mechanical testing machine and specimen deformation measurement system, it also includes:
[0112] Spraying on the surface of the long fiber mesh cloth reinforced concrete composite material specimen.
[0113] Specifically, the non-contact extensometer 300 can capture the deformation of the specimen in the test in the entire range, thereby ensuring the accuracy and credibility of the data, and also providing more comprehensive and accurate data and image information for subsequent analysis and research on the failure mode of the specimen. If this method is selected, the composite specimen needs to be sprayed with speckle before the test, where the speckle spray paint can be matte white or black; speckle spraying can provide contrast and produce obvious patterns when the surface of the object is deformed, so that the digital image correlation method non-contact extensometer can track these patterns more accurately, thereby improving the accuracy of deformation and strain measurement. Users can choose two-dimensional or three-dimensional industrial digital image correlation method measurement equipment and software, or they can use a camera to take interval photos, and then use the digital image correlation method algorithm to process the image to obtain data. Among them, the digital image correlation method non-contact extensometer mainly includes three parts: Fuji camera X-H2S, non-stroboscopic light source, and DIC open source algorithm code and software.
[0114] Exemplarily, when conducting a uniaxial tensile test on carbon fiber reinforced mortar, after the specimen is prepared according to the above preparation process, it is cured in the mold for 48 hours, and after demolding, it is placed in a concrete curing room for standard curing. After curing, the aluminum plate is glued with epoxy resin glue and waits for it to solidify, and then the specimen is installed for tensile testing. First connect the fixture to the testing machine, and then install the specimen. In the installation of the specimen, the torque of each screw in the second bolt hole 012 is 12.5Nm. After the specimen is installed, the non-contact extensometer system is installed, and the test is started after adjusting various parameters. The tensile test uses displacement control to apply the load at a speed of 0.2mm / min until the time is broken. Fig.10 is a schematic diagram of a tensile stress-strain curve of a composite material specimen provided by an embodiment of the present invention, with reference to Fig.10 After the tensile test, we can get Fig.10 The tensile stress-strain curve is shown in order to obtain the mechanical properties parameters of the specimen.
[0115] Optionally, the mechanical testing machine and the specimen deformation measurement system are operated to uniformly and continuously load the composite specimen, and the load value and the corresponding deformation value are recorded before preloading, and the following steps are further included:
[0116] The mechanical testing machine and the specimen deformation measurement system are operated to preload the composite specimen, and when the deformation parameter of the composite specimen exceeds a preset change rate, the position of the fixture holding the composite specimen is adjusted.
[0117] Specifically, in order to ensure that the composite specimens are subjected to uniform and stable stress during the experiment, and to prevent large errors or specimen breakage due to uneven stress, the specimens need to be preloaded, that is, a relatively small load is applied to the composite specimens. At the same time, we observe the changes in the instrument readings to determine the uniformity of the stress on the specimens, and adjust the position of the fixture holding the composite specimen according to the uniformity of the stress, so as to further increase the accuracy of the test.
[0118] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments, combinations and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A method for testing the mechanical properties of a fiber mesh reinforced concrete composite material, characterized in that: include: Prepare long strip fiber mesh cloth reinforced concrete composite material specimens; The two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine through a clamp respectively; Installing a specimen deformation measurement system, wherein the composite specimen is located within a monitoring range of the specimen deformation measurement system to monitor the deformation value of the composite specimen; The mechanical testing machine and the specimen deformation measuring system are operated to uniformly and continuously load the composite material specimen, and the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen are recorded.
2. The control method according to claim 1, characterized in that: A long fiber mesh cloth reinforced concrete composite material specimen is prepared, including: Assembling the mold and applying a concrete isolation agent on the inner surface of the mold; pouring a first mortar layer inside the mold, and smoothing the top of the first mortar layer; Placing a first galvanized iron mesh on the top surface of the first mortar layer, and pressing the first galvanized iron mesh tightly so that at least a portion of the first mortar layer passes through the first galvanized iron mesh; Placing a fiber mesh cloth on the top surface of the first galvanized iron mesh; Placing a second galvanized iron mesh sheet on the top surface of the fiber mesh cloth, and pressing the second galvanized iron mesh tightly, so that at least a portion of the first mortar layer passes through the first galvanized iron mesh, the fiber mesh cloth, and the second galvanized iron mesh in sequence; pouring a second mortar layer on the top surface of the second galvanized iron mesh, and smoothing the top of the second mortar layer; The composite material specimen is demoulded and cured to obtain the composite material specimen.
3. The control method according to claim 2, characterized in that: The first mortar layer and the second mortar layer have the same thickness, both in the range of 4.5-5.5 mm.
4. The control method according to claim 2, characterized in that: After pouring the second mortar layer on the top surface of the second galvanized iron mesh, demoulding the composite material specimen and curing and solidifying the composite material specimen to obtain the composite material specimen, the method further includes: Cover the top of the second mortar layer with plastic film.
5. The control method according to claim 2, characterized in that: After demoulding and curing the composite material specimen to obtain the composite material specimen, the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine by a clamp respectively, and the method further includes: Aluminum plates are respectively attached to the first side and the second side of the composite material specimen; the first side and the second side are the two opposite sides of the composite material specimen in the thickness direction.
6. The control method according to claim 1, characterized in that: Before the two ends of the elongated fiber mesh cloth reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine by means of a clamp, the method further comprises: The fixture is installed on the mechanical testing machine.
7. The control method according to claim 6, characterized in that: The clamp comprises a first clamp and a second clamp; the first clamp and the second clamp each comprise a first side clamp plate and a second side clamp plate arranged in parallel, a plurality of anti-slip grooves are arranged on the surfaces of the first side clamp plate and the second side clamp plate adjacent to each other; a plurality of second bolt holes and a first bolt hole are arranged on the surfaces of the first side clamp plate and the second side clamp plate; The fixture is installed on the mechanical testing machine, including: Extend the upper crossbeam connecting rod of the mechanical testing machine between the first side clamping plate and the second side clamping plate of the first clamping member, and use a bolt to pass through the first bolt hole of the first side clamping plate, the bolt hole of the upper crossbeam connecting rod and the first bolt hole of the second side clamping plate in sequence, so as to install the first clamping member on the upper crossbeam of the mechanical testing machine; Extend the lower crossbeam connecting rod of the mechanical testing machine between the first side clamping plate and the second side clamping plate of the second clamping member, and use a bolt to sequentially penetrate the first bolt hole of the first side clamping plate, the bolt hole of the lower crossbeam connecting rod and the first bolt hole of the second side clamping plate to install the second clamping member on the lower crossbeam of the mechanical testing machine; The two ends of the elongated fiber mesh reinforced concrete composite material specimen in the extension direction are clamped on the upper beam and the lower beam of the mechanical testing machine by means of a clamp, including: Disassembling the clamping plates on the same side of the first clamping member and the second clamping member; The first side surfaces of the two ends of the elongated fiber mesh reinforced concrete composite material specimen in the extension direction are respectively pressed against the side surfaces of the clamping plates on the undisassembled side of the first clamping member and the second clamping member, where the anti-slip grooves are arranged; installing the clamping plate with the first clamping member and the second clamping member removed; The multiple second bolt holes of the first side clamp in the first clamp are bolted to the multiple second bolt holes of the second side clamp, and the multiple second bolt holes of the first side clamp in the second clamp are bolted to the multiple second bolt holes of the second side clamp, so as to fix the long fiber mesh cloth reinforced concrete composite material specimen to the first clamp and the second clamp at both ends of the extension direction, respectively.
8. The control method according to claim 1, characterized in that: The specimen deformation measurement system comprises a contact extensometer and an extensometer bracket; the gauge length of the extensometer bracket is greater than or equal to 300 mm; Install the specimen deformation measurement system, including: A contact extensometer is installed on both sides of the long fiber mesh cloth reinforced concrete composite material specimen in the thickness direction through the extensometer bracket.
9. The control method according to claim 1, characterized in that: The specimen deformation measurement system comprises a digital image correlation method non-contact extensometer; Before operating the mechanical testing machine and the specimen deformation measurement system, the method further includes: Speckles are sprayed on the surface of the long strip fiber mesh cloth reinforced concrete composite material specimen.
10. The control method according to claim 1, characterized in that: Before operating the mechanical testing machine and the specimen deformation measuring system, uniformly and continuously loading the composite material specimen, and recording the load value and the deformation value of the fiber mesh cloth reinforced concrete composite material specimen, the method further includes: The mechanical testing machine and the specimen deformation measurement system are operated to preload the composite specimen, and when the deformation parameter of the composite specimen exceeds a preset change rate, the position of the fixture holding the composite specimen is adjusted.