Redispersible or resoluble aqueous ethylenically unsaturated aqueous polyurethane composition with improved water resistance

By using a polyurethane composition with a specific ratio and composition, the problem of insufficient water resistance and redispersibility of waterborne olefinic unsaturated polyurethane compositions after drying is solved, and a dry layer that can be redispersible or redissolved in water is formed on the substrate, which has high water resistance and good application performance.

CN118891300APending Publication Date: 2024-11-01BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027978.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing waterborne olefinic unsaturated polyurethane compositions cannot simultaneously possess good water resistance and redispersibility when dried, making it difficult to meet the requirement of forming a redispersible or water-soluble dried layer on a substrate.

Method used

A polyurethane composition with a specific ratio and composition, comprising polyurethane carrying olefinic unsaturated groups and COOH groups, is formed by the reaction of polyols, polyisocyanates and compounds, ensuring redispersibility or resolubility in water at ambient temperature and exhibiting high water resistance after crosslinking.

Benefits of technology

It achieves redispersibility and high water resistance of the dried layer at ambient temperature, meets the requirements for forming a redispersible or water-soluble dried layer on the substrate, and improves the application flexibility and durability of the composition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044509860000491
    Figure BDA0005044509860000491
  • Figure BDA0005044509860000501
    Figure BDA0005044509860000501
  • Figure BDA0005044509860000531
    Figure BDA0005044509860000531
Patent Text Reader

Abstract

The invention relates to a composition comprising (i) at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, which are at least partially in the form of their salt groups, the polyurethane can be obtained by reacting at least one polyol (B1) carrying at least one COOH group, at least one monohydric alcohol (B2) carrying at least one ethylenically unsaturated group, optionally at least one polyol (B3) carrying at least one ethylenically unsaturated group and not carrying a COOH group, the invention relates to a polyurethane composition comprising at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group, at least one polyol (B4) not carrying ethylenically unsaturated groups and COOH groups, at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group, optionally at least one polyisocyanate (A2) not carrying ethylenically unsaturated groups, and optionally at least one compound (C1) carrying at least one NH2 group and not carrying OH groups, wherein the equivalence ratio of ethylenically unsaturated groups of the polyisocyanates (A1) to ethylenically unsaturated groups of components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.20 / 1.00 to 0.95 / 1.00, and wherein the equivalence ratio of NCO groups of the polyisocyanates (A1) and (A2) to OH groups of components (B1), (B2), (B3) and (B4) is in the range of 1.00 / 1.00 to 1.50 / 1.00, (ii) water, and (iii) optionally at least one compound (2) carrying at least one ethylenically unsaturated group and not carrying a COOH group; and to an aqueous coating composition comprising the composition, a layer formed from the aqueous coating composition, and a substrate coated with the layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to waterborne ethylenically unsaturated polyurethane compositions, waterborne coating compositions comprising these compositions, layers formed from these coating compositions, and substrates coated with these layers.

[0002] Aqueous polyurethane compositions are used as binders in many applications such as coating compositions (eg, primer compositions and wood stain compositions), ink compositions, and adhesive compositions.

[0003] It is desirable that the dried residues formed by the composition on the machinery and equipment used to apply the composition to the substrate be redispersible or redissolvable in water. This allows the dried residues to be removed by simply treating the machinery and equipment with water or even with the aqueous composition itself, which can reduce or shorten interruptions in the process of applying the composition to the substrate.

[0004] When these compositions form a dried residue that is redispersible or redissolvable in water, the compositions generally form dried layers that do not exhibit good water resistance. Therefore, if good water resistance is desired for the final layer, compositions comprising a polyurethane carrying at least one ethylenically unsaturated group are generally preferred, since the layer formed from these compositions on the substrate can be crosslinked (or cured) in a second step.

[0005] Aqueous ethylenically unsaturated polyurethane compositions which form a dried layer which is redispersible or redissolvable in water are known in the art.

[0006] WO 2014111349 describes an aqueous resin composition comprising at least one polymerizable ethylenically unsaturated polyurethane polymer (A), wherein the polyurethane has a weight average molecular weight of less than 15000 g / mol and is obtained by reacting at least one polyisocyanate (i), at least one hydrophilic compound (ii) containing at least one group capable of reacting with isocyanate groups and at least one group capable of making the polyurethane polymer dispersible or soluble in an aqueous medium directly or after neutralization with a neutralizing agent (C) to provide a salt, at least one compound containing at least one group capable of reacting with isocyanate groups and at least one copolymerizable unsaturated group (iii), at least one compound containing at least two groups capable of reacting with isocyanate groups (iv), and optionally at least one chain extender containing at least two groups capable of reacting with isocyanate groups (the chain extender being different from (iv)), and wherein the non-volatile components of the resin composition (i) are redispersible or redispersible in water at 25°C after drying. Example 1 of WO 2014111349 describes an aqueous ethylenically unsaturated polyurethane composition prepared from hexamethylene diisocyanate, 2,2-dimethylolpropionic acid, propoxylated trimethylolpropane diacrylate having an average of 3 propylene oxide units, and EB113 (monofunctional epoxy acrylate).

[0007] Aqueous ethylenically unsaturated polyurethane compositions are also known in the art, wherein the polyurethane comprises units derived from at least one polyisocyanate carrying at least one ethylenically unsaturated group.

[0008] WO 2006089935 describes aqueous ethylenically unsaturated polyurethane compositions, wherein the polyurethane comprises units derived from polyisocyanates carrying at least one ethylenically unsaturated group. WO 2006089935 indicates that these compositions form crosslinked layers of high hardness, but does not mention the redispersibility or resolubility in water of dried layers formed from these compositions.

[0009] It is an object of the present invention to provide aqueous ethylenically unsaturated polyurethane compositions and coating compositions comprising these compositions which form dried layers which are redispersible or redissolvable in water at ambient temperature within a certain period of time and which, after crosslinking, exhibit high water resistance.

[0010] This object is achieved by a composition according to claim 1 , a coating composition according to claim 14 , a layer according to claim 15 and a substrate according to claim 16 .

[0011] The composition of the present invention is a composition comprising:

[0012] (i) at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, obtainable by reaction of:

[0013] at least one polyol (B1) carrying at least one COOH group,

[0014] at least one monool (B2) carrying at least one ethylenically unsaturated group,

[0015] optionally at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0016] at least one polyol (B4) which carries no ethylenically unsaturated groups and no COOH groups,

[0017] at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group,

[0018] optionally at least one polyisocyanate (A2) not carrying ethylenically unsaturated groups, and

[0019] optionally at least one compound (C1) carrying at least one NH2 group and no OH groups,

[0020] wherein the equivalent ratio of the ethylenically unsaturated groups of the polyisocyanate (A1) to the ethylenically unsaturated groups of the components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.20 / 1.00 to 0.95 / 1.00, and

[0021] wherein the equivalent ratio of NCO groups of the polyisocyanates (A1) and (A2) / OH groups of the components (B1), (B2), (B3) and (B4) is in the range of 1.00 / 1.00 to 1.50 / 1.00,

[0022] (ii) water, and

[0023] (iii) optionally at least one compound (2) which carries at least one ethylenically unsaturated group and no COOH group.

[0024] The equivalent ratio of ethylenically unsaturated groups provided by polyisocyanate (A1) / ethylenically unsaturated groups of components (B1), (B2), (B3), (A1) and (C1) is preferably in the range of 0.30 / 1.00 to 0.90 / 1.00, more preferably in the range of 0.40 / 1.00 to 0.80 / 1.00, even more preferably in the range of 0.50 / 1.00 to 0.70 / 1.00, and most preferably in the range of 0.55 / 1.00 to 0.65 / 1.00.

[0025] The polyols have an OH functionality of at least 1.5.

[0026] The OH functionality of a polyol is (hydroxyl number of the polyol [g KOH / g] x molecular weight of the polyol) / molecular weight of KOH. If the polyol is an oligomer or polymer, the number average molecular weight of the polyol is used, which can be determined using gel permeation chromatography calibrated with polystyrene standards. The molecular weight of KOH is 56 g / mol. The hydroxyl number of a polyol can be determined according to DIN 53240, 2016.

[0027] The polyols may be aliphatic, cycloaliphatic or aromatic polyols.

[0028] Aromatic polyols are polyols in which at least one OH functional group is directly attached to an aromatic ring. Cycloaliphatic polyols contain at least one cycloaliphatic ring, and each OH functional group is not directly attached to an aromatic ring. Aliphatic polyols do not contain cycloaliphatic rings, and each OH functional group is not directly attached to an aromatic ring. Preferred aliphatic and cycloaliphatic polyols do not contain aromatic rings.

[0029] Monohydric alcohols have an OH functionality of less than 1.5.

[0030] The OH functionality of a monool is (hydroxyl number of the monool [g KOH / g] x molecular weight of the monool) / molecular weight of KOH. If the monool is an oligomer or polymer, the number average molecular weight of the monool is used, which can be determined using gel permeation chromatography calibrated with polystyrene standards. The molecular weight of KOH is 56 g / mol. The hydroxyl number of the monool can be determined according to DIN 53240, 2016.

[0031] The monohydric alcohol may be an aliphatic, cycloaliphatic or aromatic monohydric alcohol.

[0032] Aromatic monoalcohols are monoalcohols in which the OH functional group is directly attached to an aromatic ring. Cycloaliphatic monoalcohols contain at least one cycloaliphatic ring, and each OH functional group is not directly attached to an aromatic ring. Aliphatic monoalcohols do not contain cycloaliphatic rings, and the OH functional group is not directly attached to an aromatic ring. Preferred aliphatic and cycloaliphatic monoalcohols do not contain aromatic rings.

[0033] The ethylenically unsaturated group can be any ethylenically unsaturated group that can polymerize by a free radical mechanism under heating, radiation treatment (usually UV radiation treatment), in the presence of a suitable initiator, or under electron beam treatment. Examples of ethylenically unsaturated groups are acryloyl, methacryloyl, vinyl and allyl. Preferred ethylenically unsaturated groups are selected from the group of acryloyl and methacryloyl. More preferred ethylenically unsaturated groups are acryloyl.

[0034] Polyisocyanates include polyisocyanates carrying blocked NCO groups and polyisocyanates carrying free NCO groups. Polyisocyanates carrying blocked NCO groups can be deblocked under certain conditions (e.g., at high temperatures, such as at a temperature higher than 110° C.) to obtain the corresponding polyisocyanates carrying free NCO groups. The polyisocyanates carrying blocked NCO groups are characterized as follows via their corresponding polyisocyanates carrying free NCO groups. Preferably, the polyisocyanates only include polyisocyanates carrying free NCO groups.

[0035] The polyisocyanates have an NCO functionality of at least 1.5.

[0036] The NCO functionality of a polyisocyanate is the NCO content x (molecular weight of polyisocyanate / molecular weight of NCO). If the polyisocyanate is a polymeric polyisocyanate, the weight average molecular weight of the polyisocyanate is used. The weight average molecular weight of the polymeric polyisocyanate can be determined using gel permeation chromatography calibrated with polystyrene standards. The NCO content of the polyisocyanate is the weight of NCO / weight of the polyisocyanate. The molecular weight of NCO is 42 g / mol.

[0037] The NCO content of a polyisocyanate can be determined as follows:

[0038] 10mL of 1N solution of di-n-butylamine in xylene is added to 1g of polyisocyanate dissolved in 100mL of N-methylpyrrolidone. The resulting mixture is stirred at room temperature for five minutes. Then, 1N hydrochloric acid is used to back-titrate the resulting reaction mixture to measure the volume of hydrochloric acid required for neutralizing unreacted di-n-butylamine. This reveals how many mol of di-n-butylamine reacts with NCO groups. NCO content is the weight of ("mol of di-n-butylamine reacted" x molecular weight of NCO) / polyisocyanate. The weight of polyisocyanate is 1g.

[0039] The polyisocyanate may be an aliphatic, cycloaliphatic or aromatic polyisocyanate.

[0040] Aromatic polyisocyanates are polyisocyanates in which at least one NCO functional group is directly attached to an aromatic ring. Cycloaliphatic polyisocyanates contain at least one cycloaliphatic ring, and each NCO functional group is not directly attached to an aromatic ring. Aliphatic polyisocyanates do not contain cycloaliphatic rings, and each NCO functional group is not directly attached to an aromatic ring. Preferred aliphatic and cycloaliphatic polyisocyanates do not contain aromatic rings.

[0041] The polyisocyanate may be a monomeric polyisocyanate or a polymeric polyisocyanate.

[0042] Examples of monomeric aliphatic polyisocyanates which carry no ethylenically unsaturated groups are tetramethylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, hexamethylene 1,6-diisocyanate, heptamethylene 1,7-diisocyanate, octamethylene 1,8-diisocyanate, decamethylene 1,10-diisocyanate, dodecamethylene 1,12-diisocyanate, tetradecamethylene 1,14-diisocyanate, methyl 2,6-diisocyanatohexanoate, ethyl 2,6-diisocyanatohexanoate, 2,2,4-trimethylhexane 1,6-diisocyanate and 2,4,4-trimethylhexane 1,6-diisocyanate.

[0043] Further examples of monomeric aliphatic polyisocyanates carrying no ethylenically unsaturated groups are 1,4,8-triisocyanatononane and 2′-isocyanatoethyl 2,6-diisocyanatohexanoate.

[0044] Examples of monomeric alicyclic polyisocyanates which do not carry ethylenically unsaturated groups are 1,4-diisocyanatocyclohexane, 1,3-diisocyanatocyclohexane, 1,2-diisocyanatocyclohexane, 4,4′-di(isocyanatocyclohexyl)methane, 2,4′-di(isocyanatocyclohexyl)methane, 1-isocyanato-3,3,5-trimethyl-5-(isocyanatomethyl)cyclohexane (isophorone diisocyanate), 1,3-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, 2,4-diisocyanato-1-methylcyclohexane, 2,6-diisocyanato-1-methylcyclohexane and 3(or 4),8(or 9)-bis(isocyanatomethyl)tricyclo[5.2.1.0(2,6)]decane.

[0045] Examples of monomeric aromatic polyisocyanates which carry no ethylenically unsaturated groups are 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, 2,4′-diisocyanatodiphenylmethane, 4,4′-diisocyanatodiphenylmethane, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 1-chloro-2,4-phenylene diisocyanate, 1,5-naphthylene diisocyanate, diphenylene 4,4′-diisocyanate, 4,4′-diisocyanato-3,3′-dimethylbiphenyl, 3-methyldiphenylmethane 4,4′-diisocyanate, tetramethylxylylene diisocyanate, 1,4-diisocyanatobenzene and diphenyl ether 4,4′-diisocyanate.

[0046] Further examples of monomeric aromatic polyisocyanates carrying no ethylenically unsaturated groups are 2,4,6-triisocyanatotoluene, triphenylmethane triisocyanate and 2,4,4′-triisocyanatodiphenyl ether.

[0047] Monomeric polyisocyanates carrying no ethylenically unsaturated groups can be prepared by methods known in the art, for example by treating the corresponding amines with phosgene.

[0048] The polymeric polyisocyanate comprises at least two units derived from monomeric polyisocyanates. The polymeric polyisocyanate generally further comprises at least one structural unit selected from the group consisting of uretdione, isocyanurate, biuret, urea, carbodiimide, uretonimine, urethane, allophanate, oxadiazinetrione and iminooxadiazinedione.

[0049] The polyol (B1) carrying at least one COOH group may be any aliphatic, cycloaliphatic or aromatic polyol (B1) carrying at least one COOH group.

[0050] The OH functionality of the polyol (B1) carrying at least one COOH group is generally in the range of 1.7 to 6.0, more preferably in the range of 1.8 to 5.4, even more preferably in the range of 1.8 to 3.4, most preferably in the range of 1.8 to 2.4 and in particular in the range of 1.9 to 2.2.

[0051] The polyol (B1) carrying at least one COOH group preferably has a number average molecular weight below 750 g / mol, more preferably below 500 g / mol and most preferably below 250 g / mol.

[0052] An example of a polyol (B1) carrying one COOH group is 2,2-bis(hydroxymethyl)C 2-10 - Alkanoic acids, such as 2,2-bis(hydroxymethyl)propionic acid (dimethylolpropionic acid), 2,2-bis(hydroxymethyl)butanoic acid and 2,2-bis(hydroxymethyl)valeric acid.

[0053] The polyol (B1) carrying at least one COOH group is preferably a polyol carrying one COOH group, more preferably an aliphatic or cycloaliphatic polyol (B1) carrying one COOH group, even more preferably an aliphatic polyol (B1) carrying one COOH group, most preferably selected from the group consisting of 2,2-bis(hydroxymethyl)propionic acid and 2,2-bis(hydroxymethyl)butanoic acid, and in particular 2,2-bis(hydroxymethyl)propionic acid.

[0054] The monoalcohol (B2) carrying at least one ethylenically unsaturated group may be any aliphatic, cycloaliphatic or aromatic monoalcohol carrying at least one ethylenically unsaturated group.

[0055] The monoalcohols (B2) preferably have an OH functionality in the range from 0.8 to 1.4, preferably in the range from 0.9 to 1.2.

[0056] Examples of monoalcohols (B2) carrying at least one ethylenically unsaturated group, wherein the ethylenically unsaturated group is an acryloyl group or a methacryloyl group, are monoesters of diols with acrylic acid or methacrylic acid, diesters of triols with acrylic acid or methacrylic acid, and triesters of tetraols with acrylic acid or methacrylic acid and pentaesters of hexaols with acrylic acid or methacrylic acid.

[0057] Examples of monoesters of diols with acrylic acid or methacrylic acid are C 1-10 - aliphatic diol, preferably C 1-6 - Monoesters of aliphatic diols with acrylic acid or methacrylic acid.

[0058] C 1-6 Examples of monoesters of aliphatic diols with acrylic acid or methacrylic acid are 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl methacrylate and 4-hydroxybutyl acrylate.

[0059] Further examples of monoalcohols (B2) carrying at least one ethylenically unsaturated group are ethoxylated or propoxylated diesters of 1,1,1-trimethylolpropane with acrylic acid or methacrylic acid, triesters of pentaerythritol with acrylic acid or methacrylic acid, triesters of ethoxylated or propoxylated di(1,1,1-trimethylol)propane with acrylic acid or methacrylic acid and pentaesters of dipentaerythritol.

[0060] Examples of monoalcohols (B2) carrying at least one allyl group are 2-allyloxyethanol and 2,2-bis(allyloxymethyl)butan-1-ol.

[0061] The monool (B2) carrying at least one ethylenically unsaturated group is preferably a monool carrying at least one acryloyl or methacryloyl group, more preferably a monool carrying one acryloyl or methacryloyl group. Even more preferably, the monool (B2) carrying at least one ethylenically unsaturated group is an aliphatic or alicyclic monool (B2) carrying one acryloyl or methacryloyl group, most preferably C 1-6 - Monoesters of aliphatic diols with acrylic acid or methacrylic acid, and in particular 2-hydroxyethyl acrylate.

[0062] The polyol (B3) carrying at least one ethylenically unsaturated group and no COOH group may be any aliphatic, cycloaliphatic or aromatic polyol (B3) carrying at least one ethylenically unsaturated group and no COOH group.

[0063] The OH functionality of the polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups is generally in the range from 1.7 to 6.4, more preferably in the range from 1.8 to 5.4, even more preferably in the range from 1.8 to 3.4, most preferably in the range from 1.8 to 2.4 and in particular in the range from 1.9 to 2.2.

[0064] The polyol (B3) carrying at least one ethylenically unsaturated group and no COOH group may be a polyol carrying at least one acryloyl group or methacryloyl group and no COOH group.

[0065] Examples of polyols (B3) carrying at least one acryloyl or methacryloyl group and no COOH group

[0066] The monoesters are triols not carrying a COOH group and acrylic acid or methacrylic acid, the diesters are tetraols not carrying a COOH group and acrylic acid or methacrylic acid, and the diesters, triesters or tetraesters are hexaols not carrying a COOH group and acrylic acid or methacrylic acid.

[0067] Further examples of polyols (B3) carrying at least one acryloyl or methacryloyl group and no COOH groups are the monoesters of ethoxylated or polyethoxylated 1,1,1-trimethylolpropane with acrylic acid or methacrylic acid, and the triesters or tetraesters of dipentaerythritol with acrylic acid or methacrylic acid.

[0068] A further example of polyol (B3) is bisphenol A diglycidyl ether diacrylate.

[0069] An example of the polyol (B3) in which the ethylenically unsaturated group is an allyl group is allyl pentaerythritol.

[0070] The polyol (B3) carrying at least one ethylenically unsaturated group and no COOH group is preferably a polyol carrying at least one acryloyl or methacryloyl group and no COOH group, more preferably a polyol carrying one to four acryloyl or methacryloyl groups and no COOH group, even more preferably a polyol carrying one to four acryloyl or methacryloyl groups and no COOH group, and most preferably an aliphatic or cycloaliphatic polyol carrying one to four acryloyl or methacryloyl groups and no COOH group.

[0071] Preferably, the polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups at least partly in the form of their salt groups, contains no units derived from polyols (B3) carrying at least one ethylenically unsaturated group and no COOH groups.

[0072] The polyol (B4) not carrying ethylenically unsaturated groups and COOH groups may be any aliphatic, cycloaliphatic or aromatic polyol (B3) not carrying ethylenically unsaturated groups and COOH groups.

[0073] The OH functionality of the polyol (B4) carrying no ethylenically unsaturated groups and no COOH groups is preferably in the range of 1.6 to 8.0, more preferably in the range of 1.8 to 5.4, even more preferably in the range of 1.8 to 3.4, most preferably in the range of 1.8 to 2.4 and in particular in the range of 1.9 to 2.2.

[0074] The polyol (B4) not carrying ethylenically unsaturated groups and COOH groups may be a polyol having a number average molecular weight of less than 500 g / mol or a polyol having a number average molecular weight of at least 500 g / mol.

[0075] Examples of aliphatic polyols (B4) which do not carry ethylenically unsaturated groups and COOH groups are ethylene glycol, propane-1,2-diol, propane-1,3-diol, butane-1,2-diol, butane-1,3-diol, butane-1,4-diol, butane-2,3-diol, pentane-1,2-diol, pentane-1,3-diol, pentane-1,4-diol, pentane-1,5-diol, pentane-2,3-diol, pentane-2,4-diol, hexane-1,2-diol, hexane-1,3-diol, hexane-1,4-diol, hexane-1,5-diol, hexane-1,6-diol, hexane-2,5-diol. , heptane-1,2-diol, heptane-1,7-diol, octane-1,8-diol, octane-1,2-diol, nonane-1,9-diol, decane-1,2-diol, decane-1,10-diol, dodecane-1,2-diol, dodecane-1,12-diol, hexane-1,5-diene-3,4-diol, neopentyl glycol, 2-methyl-pentane-2,4-diol, 2,4-dimethyl-pentane-2,4-diol, 2-ethyl-hexane-1,3-diol, 2,5-dimethyl-hexane-2,5-diol, 2,2,4-trimethyl-pentane-1,3-diol, pinacol and hydroxypivalic acid neopentyl glycol ester.

[0076] Further examples of aliphatic polyols (B4) which carry no ethylenically unsaturated groups and no COOH groups are di(ethylene glycol), tri(ethylene glycol), di(propylene glycol) and tri(propylene glycol).

[0077] Examples of aliphatic polyols (B4) which do not carry ethylenically unsaturated groups and COOH groups are glycerol, trimethylolmethane, 1,1,1-trimethylolethane, 1,1,1-trimethylolpropane, 1,2,4-butanetriol and 1,3,5-tris(2-hydroxyethyl)isocyanurate, and condensates thereof with ethylene oxide, propylene oxide and / or butylene oxide.

[0078] Examples of aliphatic polyols (B4) which do not carry ethylenically unsaturated groups and COOH groups are pentaerythritol, diglycerol, triglycerol, condensates of at least four glycerols, di(trimethylolpropane), di(pentaerythritol), and condensates thereof with ethylene oxide, propylene oxide and / or butylene oxide.

[0079] Examples of cycloaliphatic polyols (B4) which do not carry ethylenically unsaturated groups and COOH groups are 1,1-bis(hydroxymethyl)-cyclohexane, 1,2-bis(hydroxymethyl)-cyclohexane, 1,3-bis(hydroxymethyl)-cyclohexane, 1,4-bis(hydroxymethyl)-cyclohexane, 1,1-bis(hydroxyethyl)-cyclohexane, 1,2-bis(hydroxyethyl)-cyclohexane, 1,3-bis(hydroxyethyl)-cyclohexane, 1,4-bis(hydroxymethyl)-cyclohexane, ethyl)-cyclohexane, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, cyclopentane-1,2-diol, cyclopentane-1,3-diol, 1,2-bis(hydroxymethyl)cyclopentane, 1,3-bis(hydroxymethyl)cyclopentane, cyclohexane-1,2-diol, cyclohexane-1,3-diol, cyclohexane-1,4-diol, cycloheptane-1,3-diol and cycloheptane-1,4-diol and cycloheptane-1,2-diol.

[0080] Further examples of cycloaliphatic polyols (B4) which do not carry ethylenically unsaturated groups and COOH groups are inositol, sugars such as glucose, fructose and sucrose, sugar alcohols such as sorbitol, mannitol, threitol, erythritol, adonitol (ribitol), arabitol (lyxitol), xylitol, dulcitol (galactitol), maltitol and isomalt, and also tris(hydroxymethyl)amine, tris(hydroxyethyl)amine and tris(hydroxypropyl)amine.

[0081] Examples of the polyol (B4) not carrying ethylenically unsaturated groups and COOH groups are also polyester polyols not carrying ethylenically unsaturated groups and COOH groups, polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups, polyether polyols not carrying ethylenically unsaturated groups and COOH groups, polythioether polyols not carrying ethylenically unsaturated groups and COOH groups, and polyacrylate polyols not carrying ethylenically unsaturated groups and COOH groups.

[0082] The polyester polyols not carrying ethylenically unsaturated groups and COOH groups are polymeric polyols not carrying ethylenically unsaturated groups and COOH groups and comprising ester groups as linking groups between two monomer units, wherein the equivalent ratio of ester linking groups / all linking groups is at least 50 / 50, preferably at least 70 / 100, more preferably at least 80 / 100. The polyester polyols not carrying ethylenically unsaturated groups and COOH groups may contain additional linking groups, such as carbonate, ether, thioether or urethane groups.

[0083] The polyester polyols carrying no ethylenically unsaturated groups and no COOH groups can be prepared by methods known in the art, for example by reacting at least one polyacid having a COOH functionality in the range of 1.8 to 2.4 and carrying no ethylenically unsaturated groups with a polyol having an OH functionality in the range of 1.8 to 2.4 and carrying no ethylenically unsaturated groups and no COOH groups. Examples of polyacids having a COOH functionality of 2 and carrying no ethylenically unsaturated groups are aliphatic polyacids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 2-methylmalonic acid, 2-ethylmalonic acid, 2-methylsuccinic acid, 2-ethylsuccinic acid, 3,3-dimethylglutaric acid, 2-phenylmalonic acid, 2-phenylsuccinic acid, alicyclic polyacids such as cyclopentanecarboxylic acid, 1,12-dodecanedi ... Examples of polyols having an OH functionality in the range of 1.8 to 2.4 and carrying no ethylenically unsaturated groups and no COOH groups are given above.

[0084] Also exemplified as polyester polyols are polycaprolactone diols.

[0085] The polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups are polymeric polyols not carrying ethylenically unsaturated groups and COOH groups and comprising at least two carbonate groups in the polymer backbone. The polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups can include additional linking groups in the backbone whose number is less than the number of carbonate groups, such as ester, ether, thioether or urethane linking groups. Examples of polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups are polycarbonates not carrying COOH groups, comprising units derived from the group consisting of butane-1,4-diol, pentane-1,5-diol and hexane-1,6-diol. Preferred polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups are polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups, wherein the equivalent ratio of carbonate groups / all linking groups is at least 70 / 100, more preferably at least 80 / 100.

[0086] The polyether polyols not carrying ethylenically unsaturated groups and COOH groups are polymeric polyols not carrying ethylenically unsaturated groups and COOH groups and containing at least two ether groups in the polymer backbone. The polyether polyols not carrying ethylenically unsaturated groups and COOH groups may contain additional connecting groups in the backbone whose number is less than the number of ether groups, such as ester, carbonate, thioether or urethane groups.

[0087] Preferred polyether polyols carrying no ethylenically unsaturated groups and no COOH groups are polyether polyols carrying no ethylenically unsaturated groups and no COOH groups, wherein the equivalent ratio of ether groups / all connecting groups is at least 70 / 100, more preferably at least 80 / 100.

[0088] Examples of polyether polyols which do not carry ethylenically unsaturated groups and COOH groups are polyethylene glycol, polypropylene glycol, polyethylene glycol-polypropylene glycol, polytetramethylene glycol and polytetrahydrofuran diol. The polyethylene glycol-polypropylene glycol may be a random copolymer or a block copolymer.

[0089] The polythioether polyols not carrying ethylenically unsaturated groups and COOH groups are polymeric polyols not carrying ethylenically unsaturated groups and COOH groups and having at least two thioether groups in the polymer backbone. The polythioether polyols not carrying ethylenically unsaturated groups and COOH groups may contain additional connecting groups in the backbone whose number is less than the number of ether groups, such as ester, carbonate, ether or urethane groups.

[0090] The poly(meth)acrylate polyols not carrying ethylenically unsaturated groups and COOH groups are polymeric polyols not carrying ethylenically unsaturated groups and COOH groups, which comprise at least two units derived from (meth)acrylate monomers carrying at least one OH group, such as 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate.

[0091] The polyol (B4) carrying no ethylenically unsaturated groups and no COOH groups preferably has a number average molecular weight of at least 500 g / mol, more preferably at least 750 g / mol, even more preferably in the range of 800 to 3000 g / mol, most preferably in the range of 800 to 2000 g / mol.

[0092] The polyol (B4) not carrying ethylenically unsaturated groups and COOH groups is preferably selected from the group consisting of polyester polyols not carrying ethylenically unsaturated groups and COOH groups, polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups, and polyether polyols not carrying ethylenically unsaturated groups and COOH groups. More preferably, the polyol (B4) not carrying ethylenically unsaturated groups and COOH groups is a polyester polyol not carrying ethylenically unsaturated groups and COOH groups or a polyether polyol not carrying ethylenically unsaturated groups and COOH groups.

[0093] The polyisocyanate (A1) carrying at least one ethylenically unsaturated group may be any aliphatic, cycloaliphatic or aromatic polyisocyanate carrying at least one ethylenically unsaturated group.

[0094] The NCO functionality of the polyisocyanate (A1) carrying at least one ethylenically unsaturated group is generally in the range of 1.6 to 10.0, preferably in the range of 1.7 to 5.4, more preferably in the range of 1.8 to 3.4, and most preferably in the range of 1.8 to 2.4.

[0095] The polyisocyanate (A1) carrying at least one ethylenically unsaturated group preferably has an ethylenically unsaturated group density in the range of 0.10 to 10.00 milliequivalents of ethylenically unsaturated groups / g (A1), more preferably 0.50 to 5.00 milliequivalents of ethylenically unsaturated groups / g (A1), even more preferably 1.00 to 3.00 milliequivalents of ethylenically unsaturated groups / g (A1), and most preferably 1.50 to 2.50 milliequivalents of ethylenically unsaturated groups / g (A1).

[0096] The ethylenically unsaturated group density of the polyisocyanate (A1) is determined by methods known in the art from 1 The ethylenically unsaturated group density of the polyisocyanate (A1) can be determined, for example, by 1H-NMR was determined using 1,4-dimethyl terephthalate as an internal standard: 1 H-NMR is acquired from a mixture of a specific amount of a polyisocyanate (A1) carrying at least one ethylenically unsaturated group (= weight of polyisocyanate) and a specific amount of 1,4-dimethyl terephthalate (= weight of 1,4-dimethyl terephthalate) in a suitable solvent such as deuterated chloroform, deuterated dimethyl sulfoxide or deuterated methanol. The ratio of the integrated intensity of the signal of the selected protons of the ethylenically unsaturated groups of the polyisocyanate (A1) to the integrated intensity of the signal of the aromatic protons of 1,4-dimethyl terephthalate is determined. The ethylenically unsaturated group density of the polyisocyanate (A1) carrying at least one ethylenically unsaturated group [mmol ethylenically unsaturated group / g polyisocyanate (A1)] is (weight of 1,4-dimethyl terephthalate x number of aromatic protons of 1,4-dimethyl terephthalate x ratio of signal integrated intensity of selected protons of ethylenically unsaturated groups of polyisocyanate (A1) to signal integrated intensity of aromatic protons of 1,4-dimethyl terephthalate) / (molecular weight of 1,4-dimethyl terephthalate x number of selected protons of ethylenically unsaturated groups of polyisocyanate (A1) x weight of polyisocyanate). The molecular weight of 1,4-dimethyl terephthalate is 194 g / mol. The number of aromatic protons of 1,4-dimethyl terephthalate is 4. It should be understood that, depending on the type of ethylenically unsaturated group, a person skilled in the art knows which protons of the ethylenically unsaturated group to select in order to determine the ratio of the signal integrated intensity of the selected protons of the ethylenically unsaturated group of polyisocyanate (A1) to the signal integrated intensity of the aromatic protons of 1,4-dimethyl terephthalate. If the ethylenically unsaturated group is, for example, an acryloyl group, a person skilled in the art typically selects the two protons at the end of the acryloyl group.

[0097] The polyisocyanate (A1) preferably also comprises at least one allophanate group.

[0098] The polyisocyanate (A1) preferably has an allophanate group density in the range of 0.10 to 100.00 milliequivalent allophanate groups / g (A1), more preferably 0.50 to 50.00 milliequivalent allophanate groups / g (A1), even more preferably 0.50 to 10.00 milliequivalent allophanate groups / g (A1), most preferably 1.00 to 5.00 milliequivalent allophanate groups / g (A1), and in particular 1.00 to 3.00 milliequivalent allophanate groups / g (A1).

[0099] The allophanate group density of the polyisocyanate (A1) can be determined by NMR by methods known in the art.

[0100] The polyisocyanate (A1) carrying at least one ethylenically unsaturated group is preferably an aliphatic or cycloaliphatic polyisocyanate.

[0101] The polyisocyanate (A1) carrying at least one ethylenically unsaturated group is preferably a polymeric polyisocyanate obtainable by reaction of at least one polyisocyanate (A3) carrying no ethylenically unsaturated group with at least one monool (B5) carrying one ethylenically unsaturated group.

[0102] The weight ratio of polyisocyanate (A3) / monool (B5) is generally in the range of 95 / 5 to 50 / 50, preferably in the range of 90 / 10 to 70 / 30, most preferably in the range of 85 / 15 to 75 / 25.

[0103] A catalyst is usually used in the reaction, for example N,N,N-trimethyl-N-(2-hydroxypropyl)ammonium 2-ethylhexanoate. The catalyst can be used in an amount of 10 to 500 ppm, preferably 100 to 300 ppm, based on the weight of the polyisocyanate (A3).

[0104] Typically, the reaction is carried out at elevated temperatures, preferably at temperatures in the range from 80° C. to 150° C. When the desired NCO content is reached, the reaction can be stopped by distilling off the unreacted polyisocyanate (A3) not carrying ethylenically unsaturated groups.

[0105] The monool (B5) carrying at least one ethylenically unsaturated group may be any monool carrying at least one ethylenically unsaturated group.

[0106] The monoalcohol (B5) has an OH functionality in the range from 0.8 to 1.4, preferably in the range from 0.9 to 1.2.

[0107] The ethylenically unsaturated group of the monool (B5) is preferably an acryloyl group or a methacryloyl group.

[0108] Examples of monools (B5) carrying at least one acryloyl or methacryloyl group are monoesters of diol groups with acrylic acid or methacrylic acid, diesters of triols with acrylic acid or methacrylic acid, and triesters of tetraols with acrylic acid or methacrylic acid and pentaesters of hexaols with acrylic acid or methacrylic acid.

[0109] Examples of monoesters of diols with acrylic acid or methacrylic acid are C 1-10 - aliphatic diol, preferably C 1-6 - Monoesters of aliphatic diols with acrylic acid or methacrylic acid.

[0110] C 1-6Examples of monoesters of aliphatic diols with acrylic acid or methacrylic acid are 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl methacrylate and 4-hydroxybutyl acrylate.

[0111] Further examples of monoalcohols (B5) carrying at least one ethylenically unsaturated group are ethoxylated or propoxylated diesters of 1,1,1-trimethylolpropane with acrylic acid or methacrylic acid, triesters of pentaerythritol with acrylic acid or methacrylic acid, triesters of ethoxylated or propoxylated di(1,1,1-trimethylol)propane with acrylic acid or methacrylic acid and pentaesters of dipentaerythritol.

[0112] Examples of monoalcohols (B5) which carry at least one allyl group and no COOH groups are 2-allyloxyethanol and 2,2-bis(allyloxymethyl)butan-1-ol.

[0113] The monool (B5) carrying at least one ethylenically unsaturated group is preferably a monool carrying at least one acryloyl or methacryloyl group, more preferably a monool carrying one acryloyl or methacryloyl group. Even more preferably, the monool (B5) carrying at least one ethylenically unsaturated group is an aliphatic or cycloaliphatic monool (B5) carrying one acryloyl or methacryloyl group and no COOH group, most preferably C 1-6 - Monoesters of aliphatic diols with acrylic acid or methacrylic acid, and in particular 2-hydroxyethyl acrylate.

[0114] The polyisocyanate (A3) not carrying ethylenically unsaturated groups may be any aliphatic, alicyclic or aromatic polyisocyanate not carrying ethylenically unsaturated groups, and the polyisocyanate may be a monomeric or polymeric polyisocyanate.

[0115] The NCO functionality of the polyisocyanate (A3) is generally in the range of 1.6 to 8.0, preferably in the range of 1.7 to 5.4, more preferably in the range of 1.8 to 3.4, and most preferably in the range of 1.8 to 2.4.

[0116] The polyisocyanate (A3) not carrying ethylenically unsaturated groups is preferably an aliphatic or cycloaliphatic polyisocyanate not carrying ethylenically unsaturated groups, more preferably an aliphatic polyisocyanate, and even more preferably an aliphatic polyisocyanate selected from the group consisting of tetramethylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, hexamethylene 1,6-diisocyanate, heptamethylene 1,7-diisocyanate, octamethylene 1,8-diisocyanate, and a polymeric polyisocyanate not carrying ethylenically unsaturated groups, having an NCO functionality in the range of 1.8 to 3.4 and comprising at least two units derived from tetramethylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, hexamethylene 1,6-diisocyanate, heptamethylene 1,7-diisocyanate or octamethylene 1,8-diisocyanate.

[0117] Most preferably, the polyisocyanate (A3) not carrying ethylenically unsaturated groups is chosen from the group consisting of hexamethylene 1,6-diisocyanate, and polymeric polyisocyanates not carrying ethylenically unsaturated groups having an NCO functionality in the range of 1.8 to 3.4 and comprising at least two units derived from hexamethylene 1,6-diisocyanate.

[0118] In particular, the polyisocyanate (A3) not carrying ethylenically unsaturated groups is hexamethylene 1,6-diisocyanate or a hexamethylene 1,6-diisocyanate trimer.

[0119] The polyisocyanate (A2) not carrying ethylenically unsaturated groups may be any aliphatic, alicyclic or aromatic polyisocyanate not carrying ethylenically unsaturated groups, and the polyisocyanate may be a monomeric or polymeric polyisocyanate.

[0120] The NCO functionality of the polyisocyanates (A2) not carrying ethylenically unsaturated groups is generally in the range from 1.6 to 8.0, preferably in the range from 1.7 to 5.4, more preferably in the range from 1.8 to 3.4.

[0121] Examples of polymeric aliphatic polyisocyanates are hexamethylene 1,6-diisocyanate trimer, isophorone diisocyanate trimer, and pentamethylene diisocyanate trimer.

[0122] The polymeric polyisocyanates can be prepared by methods known in the art.

[0123] The polyisocyanate (A2) not carrying ethylenically unsaturated groups is preferably an aliphatic or alicyclic polyisocyanate not carrying ethylenically unsaturated groups, more preferably an aliphatic polyisocyanate, and even more preferably an aliphatic polyisocyanate selected from the group consisting of tetramethylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, hexamethylene 1,6-diisocyanate, heptamethylene 1,7-diisocyanate, octamethylene 1,8-diisocyanate, and a polymeric polyisocyanate not carrying ethylenically unsaturated groups, which has an NCO functionality in the range of 1.8 to 3.4 and contains at least two units derived from tetramethylene 1,4-diisocyanate, pentamethylene 1,5-diisocyanate, hexamethylene 1,6-diisocyanate, heptamethylene 1,7-diisocyanate or octamethylene 1,8-diisocyanate.

[0124] In particular, the polyisocyanate (A2) not carrying ethylenically unsaturated groups is selected from the group consisting of hexamethylene 1,6-diisocyanate and polymeric polyisocyanates not carrying ethylenically unsaturated groups having an NCO functionality in the range from 1.8 to 3.4 and comprising at least two units derived from hexamethylene 1,6-diisocyanate.

[0125] The polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, preferably comprises no units derived from polyisocyanates (A2).

[0126] The compound (C1) carrying at least one NH2 group and no OH group may be any aliphatic, cycloaliphatic or aromatic compound carrying at least one NH2 group and no OH group.

[0127] Aromatic compounds (C1) are compounds (C1) in which at least one NH2 functional group is directly attached to an aromatic ring. Cycloaliphatic compounds (C1) contain at least one cycloaliphatic ring, and each NH2 functional group is not directly attached to an aromatic ring. Aliphatic compounds (C1) do not contain cycloaliphatic rings, and each NH2 functional group is not directly attached to an aromatic ring. Preferred aliphatic and cycloaliphatic compounds (C1) do not contain aromatic rings.

[0128] The compound (C1) carrying at least one NH2 group and no OH group may also carry other functional groups such as NH or acidic groups such as SO3H, PO3H, or COOH or salt groups thereof.

[0129] Examples of the compound (C1) are N-aminoethyl-2-aminoethanesulfonic acid sodium salt, N-aminoethyl-2-aminoethanecarboxylic acid sodium salt, and lysine sodium salt.

[0130] The compound (C1) carrying at least one NH2 group and no OH group is preferably an aliphatic or alicyclic compound carrying one NH2 group and no OH group, more preferably an aliphatic compound carrying one NH2 group and no OH group and carrying at least one acidic group selected from the group consisting of SO3H, PO3H, or COOH or a salt group thereof, and most preferably an aliphatic compound carrying one NH2 group and no OH group and carrying one SO3H or SO3Na group, and in particular an aliphatic compound carrying one NH2 group, one NH group, no OH group and carrying one SO3H or SO3Na group.

[0131] Components (B1), (B2), (B3), (B4), (B5), (A1), (A2), (A3) and (C1) can be derived from fossil resources or renewable resources such as plants. Whether a component is derived from a renewable resource can be determined by the C-14 / C-12 isotope ratio.

[0132] The polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, preferably has a number average molecular weight Mn in the range of 750 g / mol to 30000 g / mol, more preferably in the range of 1000 g / mol to 15000 g / mol, even more preferably in the range of 1500 g / mol to 15000 g / mol.

[0133] The polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, preferably has a weight average molecular weight Mw in the range of 3000 g / mol to 50000 g / mol, more preferably in the range of 5000 g / mol to 30000 g / mol, even more preferably in the range of 6000 g / mol to 20000 g / mol, most preferably in the range of 7000 g / mol to 15000 g / mol.

[0134] The number average molecular weight, Mn, and the weight average molecular weight, Mw, are determined using gel permeation chromatography calibrated with polystyrene standards.

[0135] The salt group of the COOH group may be any salt group of the COOH group formed by reacting the COOH group with a base.

[0136] The base may be an inorganic base or a compound carrying at least one tertiary amino group.

[0137] Examples of inorganic bases are alkali metal and alkaline earth metal hydroxides, alkali metal and alkaline earth metal carbonates and alkali metal and alkaline earth metal bicarbonates. Preferred inorganic bases are alkali metal hydroxides such as sodium hydroxide or potassium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, and alkali metal bicarbonates such as sodium bicarbonate and potassium bicarbonate.

[0138] Examples of compounds carrying at least one tertiary amino group are triethanolamine, tripropanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, triethylamine, ethyldiisopropylamine, tripropylamine, triisopropylamine and tri-n-butylamine.

[0139] The salt group of the COOH group is preferably an alkali metal salt of the COOH group, more preferably a sodium or potassium salt of the COOH group, and most preferably a sodium salt of the COOH group.

[0140] The equivalent ratio of the salt group of the COOH group / (COOH group and its salt group) of the polyurethane (1) is preferably in the range of 40 / 100 to 100 / 100, and more preferably in the range of 60 / 100 to 100 / 100.

[0141] The COOH group and its salt group density of the polyurethane (1) is preferably at least 0.20 milliequivalent COOH group and its salt group / g polyurethane (1), and more preferably at least 0.30 milliequivalent COOH group and its salt group / g polyurethane (1), and most preferably in the range of 0.35 to 0.50 milliequivalent COOH group and its salt group / g solid of polyurethane (1).

[0142] The COOH group and its salt group density of polyurethane (1) is the sum of the following terms:

[0143] [weight ratio (B1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1)] multiplied by the COOH group density of (B1), and

[0144] [weight ratio (B2) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1)] multiplied by the COOH group density of (B2), and

[0145] [Weight ratio (C1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1)] multiplied by the COOH group density of (C1).

[0146] The ethylenically unsaturated group density of the polyurethane (1) is preferably at least 0.50 milliequivalent ethylenically unsaturated group / g polyurethane (1), and more preferably at least 1.00 milliequivalent ethylenically unsaturated group / g polyurethane (1), and even more preferably in the range of 1.50 to 5.00 milliequivalent ethylenically unsaturated group / g polyurethane (1), and most preferably in the range of 2.00 to 3.00 milliequivalent ethylenically unsaturated group / g polyurethane (1).

[0147] The ethylenically unsaturated group density of the polyurethane (1) is determined by calculation. The ethylenically unsaturated group density of the polyurethane (1) is the sum of the following terms:

[0148] [weight ratio (B1) / ((A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the ethylenically unsaturated group density of (B1)],

[0149] [weight ratio (B2) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the ethylenically unsaturated group density of (B2)],

[0150] [weight ratio (B3) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the ethylenically unsaturated group density of (B3)],

[0151] [weight ratio (A1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the ethylenically unsaturated group density of (A1)], and

[0152] [Weight ratio (C1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the ethylenically unsaturated group density of (C1).

[0153] The ethylenically unsaturated group density of (B1), (B2), (B3), (A1) and (C1) can be obtained by methods known in the art from 1 Confirmed by H-NMR.

[0154] The polyurethane (1) preferably also comprises allophanate groups.

[0155] If allophanate groups are present, the allophanate group density of the polyurethane (1) is preferably in the range of at least 0.10 to 200.00 milliequivalent allophanate groups / g polyurethane (1), and more preferably in the range of 0.50 to 60.00 milliequivalent allophanate groups / g polyurethane (1), and even more preferably in the range of 0.70 to 10.00 milliequivalent allophanate groups / g polyurethane (1), and most preferably in the range of 0.80 to 5.00 milliequivalent allophanate groups / g polyurethane (1).

[0156] The allophanate group density of the polyurethane (1) was determined by calculation.

[0157] The allophanate group density of the polyurethane (1) is the sum of:

[0158] [weight ratio (A1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the allophanate group density of (A1), and

[0159] [Weight ratio (A2) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1)] multiplied by the allophanate group density of (A2).

[0160] The allophanate group density of (A1) and (A2) can be determined by NMR by methods known in the art.

[0161] The at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, is preferably obtainable by reaction of

[0162] 0.5 to 30% by weight of at least one polyol (B1) carrying at least one COOH group,

[0163] 1 to 60% by weight of at least one monoalcohol (B2) carrying at least one ethylenically unsaturated group and no COOH group,

[0164] 0 to 40% by weight of at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0165] 5 to 80% by weight of at least one polyol (B4) carrying no ethylenically unsaturated groups and no COOH groups,

[0166] 5 to 90% by weight of at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group,

[0167] 0 to 50% by weight of at least one polyisocyanate (A2) carrying no ethylenically unsaturated groups, and

[0168] 0 to 30% by weight of at least one compound (C1) carrying at least one NH2 group and no OH groups,

[0169] In each case based on the sum by weight of (B1), (B2), (B3), (B4), (A1), (A2) and (C1).

[0170] The at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, is more preferably obtainable by reaction of

[0171] 1 to 20% by weight of at least one polyol (B1) carrying at least one COOH group,

[0172] 5 to 50% by weight of at least one monoalcohol (B2) carrying at least one ethylenically unsaturated group and no COOH group,

[0173] 0 to 30% by weight of at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0174] 5 to 60% by weight of at least one polyol (B4) carrying no ethylenically unsaturated groups and no COOH groups,

[0175] 15 to 85% by weight of at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group,

[0176] 0 to 40% by weight of at least one polyisocyanate (A2) carrying no ethylenically unsaturated groups, and

[0177] 0 to 15% by weight of at least one compound (C1) carrying at least one NH2 group and no OH groups,

[0178] In each case based on the sum by weight of (B1), (B2), (B3), (B4), (A1), (A2) and (C1).

[0179] The at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, is even more preferably obtainable by reaction of

[0180] 1 to 10% by weight of at least one polyol (B1) carrying at least one COOH group,

[0181] 5 to 25% by weight of at least one monoalcohol (B2) carrying at least one ethylenically unsaturated group and no COOH group,

[0182] 0 to 5% by weight of at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0183] 10 to 40% by weight of at least one polyol (B4) not carrying ethylenically unsaturated groups and COOH groups,

[0184] 30 to 80% by weight of at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group,

[0185] 0 to 10% by weight of at least one polyisocyanate (A2) carrying no ethylenically unsaturated groups, and

[0186] 0 to 5% by weight of at least one compound (C1) carrying at least one NH2 group and no OH group

[0187] In each case based on the sum by weight of (B1), (B2), (B3), (B4), (A1), (A2) and (C1).

[0188] The at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, is most preferably obtainable by reaction of

[0189] 1 to 10% by weight of at least one polyol (B1) carrying at least one COOH group,

[0190] 5 to 25% by weight of at least one monoalcohol (B2) carrying at least one ethylenically unsaturated group and no COOH group,

[0191] 0% by weight of at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0192] 10 to 40% by weight of at least one polyol (B4) not carrying ethylenically unsaturated groups and COOH groups,

[0193] 40 to 80% by weight of at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group,

[0194] 0 to 10% by weight of at least one polyisocyanate (A2) carrying no ethylenically unsaturated groups, and

[0195] 0 to 3% by weight of at least one compound (C1) carrying at least one NH2 group and no OH groups,

[0196] In each case based on the sum by weight of (B1), (B2), (B3), (B4), (A1), (A2) and (C1).

[0197] The equivalent ratio of NCO groups of polyisocyanates (A1) and (A2) / OH groups of components (B1), (B2), (B3) and (B4) is preferably in the range of 1.01 / 1.00 to 1.30 / 1.00, most preferably in the range of 1.02 / 1.00 to 1.20 / 1.00.

[0198] The equivalent ratio of NCO groups of polyisocyanates (A1) and (A2) / OH groups of components (B1), (B2), (B3) and (B4) and NCO-reactive groups other than OH provided by component (C1) is generally in the range of 1.00 / 1.00 to 1.50 / 1.00, preferably in the range of 1.01 / 1.00 to 1.30 / 1.00, more preferably in the range of 1.02 / 1.00 to 1.20 / 1.00.

[0199] Examples of NCO-reactive groups other than OH provided by component (C1) are NH2, NH and SH.

[0200] Compounds (2) which carry at least one ethylenically unsaturated group and no COOH group generally also carry no NCO group or a group reactive toward NCO. Examples of groups reactive toward NCO groups are OH, SH, NH2 and NH groups.

[0201] Compound (2) preferably has a number average molecular weight below 1000 g / mol. The number average molecular weight can be determined using gel permeation chromatography calibrated with polystyrene standards.

[0202] Compound (2) preferably has a boiling point greater than 200° C. at 101325 Pa (standard pressure).

[0203] Compound (2) preferably has a melting point of less than 0° C. at 101325 Pa (standard pressure).

[0204] The ethylenically unsaturated group functionality of compound (2) is generally in the range of 0.8 to 6.5, preferably in the range of 0.8 to 4.4, and more preferably in the range of 1.8 to 4.4.

[0205] The ethylenically unsaturated group functionality of compound (2) can be calculated by multiplying the ethylenically unsaturated group density of compound (2) by the number average molecular weight of compound (2). The ethylenically unsaturated group density of compound (2) can be calculated by methods known in the art from 1 HNMR confirmed.

[0206] Examples of compound (2) are styrene, p-tert-butylstyrene, p-methylstyrene, o-methylstyrene, 2-vinylnaphthalene, divinylstyrene, butadiene, isoprene, chloroprene, ethylene, propylene, 1-butene, 2-butene, isobutylene, cyclopentene, cyclohexene, cyclododecene, vinyl acetate, vinyl propionate, vinyl chloride and vinylidene chloride, N-vinylformamide, N-vinylacetamide, N-vinyl-N-methylformamide, N-vinyl-N-methyl-acetamide, N-vinylpyrrolidone, N-vinylcaprolactam , ethylene glycol divinyl ether, di(ethylene glycol) divinyl ether, tri(ethylene glycol) divinyl ether, trimethylolpropane trivinyl ether, 1,4-cyclohexanedimethanol divinyl ether, methyl vinyl ether, ethyl vinyl ether, isopropyl vinyl ether, isobutyl vinyl ether, tert-amyl vinyl ether, dodecyl vinyl ether, 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether, cyclohexyl vinyl ether, allyl acetate, diallyl phthalate, triallyl cyanurate, trimethylolpropane triallyl ether, α,β-unsaturated C 4-10 -Dicarboxylic acids (such as maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid and 2-methyleneglutaric acid) and their salts, α, β-unsaturated C 4-10 -esters of dicarboxylic acids (such as dimethyl maleate, ethyl methyl maleate, diethyl maleate, dimethyl fumarate, ethyl methyl fumarate and diethyl fumarate), α,β-unsaturated nitriles (such as (meth)acrylonitrile) and α,β-unsaturated aldehydes (such as (meth)acrolein) and α,β-unsaturated amides (such as (meth)acrylamide), α,β-unsaturated C 3-8 - Carboxylic acids (such as acrylic acid, methacrylic acid and 3,3-dimethylacrylic acid) and their salts.

[0207] Another example of compound (2) is a compound carrying at least one (meth)acryloyl group is (meth)acrylic acid C 1-20-alkyl esters, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, 2-methylbutyl (meth)acrylate, amyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-propylheptyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate and dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate and nonadecyl (meth)acrylate, C (meth)acrylate 5-12 - cycloalkyl esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate and cycloheptyl (meth)acrylate, acetoacetoxy (meth)acrylate (C 2-6 -alkyl) esters such as acetoacetoxyethyl (meth)acrylate, acetoacetoxypropyl (meth)acrylate and acetoacetoxybutyl (meth)acrylate, (meth)acrylate [C 1-10 -alkoxy (C 1-10 -alkoxy) 0-5 ]C 1-10 -alkyl esters such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 2-(2'-methoxyethoxy)ethyl (meth)acrylate and 2-(2'-ethoxyethoxy)ethyl (meth)acrylate, 2-norbornyl (meth)acrylate, dihydrodicyclopentadienyl (meth)acrylate, 4-tetrahydropyranyl (meth)acrylate, 2-tetrahydropyranyl (meth)acrylate, tetrahydrofuranyl (meth)acrylate, C 1-20- Diesters of diols with (meth)acrylic acid, such as 1,2-ethylene glycol di(meth)acrylate, 1,2-propylene glycol di(meth)acrylate, 1,3-propylene glycol di(meth)acrylate, 1,2-butylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,2-bis(hydroxymethyl)-cyclohexane di(meth)acrylate, 1,4-bis(hydroxymethyl)-cyclohexane di(meth)acrylate and cyclohexane-1,4-diol di(meth)acrylate, ethoxylated and / or propoxylated C 1-20 - diesters of diols with (meth)acrylic acid such as ethoxylated and / or propoxylated 1,2-butanediol di(meth)acrylate, ethoxylated and / or propoxylated 1,4-butanediol di(meth)acrylate, ethoxylated and / or propoxylated neopentyl glycol di(meth)acrylate, ethoxylated and / or propoxylated 1,4-bis(hydroxymethyl)-cyclohexane di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate and polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polyethylene glycol-polypropylene glycol di(meth)acrylate - the sequence of ethylene oxide or propylene oxide units is block or random, polytetramethylene glycol di(meth)acrylate )acrylate, polytetramethylene dimethacrylate, and ethoxylated or propoxylated bisphenol A dimethacrylate, glycerol trimethacrylate, 1,1,1-trimethylolpropane trimethacrylate, 1,1,1-trimethylolethane trimethacrylate, pentaerythritol tetramethacrylate, di(1,1,1-trimethylolpropane) tetramethacrylate and dipentaerythritol hexamethacrylate, ethoxylated and / or propoxylated glycerol trimethacrylate, ethoxylated and / or propoxylated 1,1,1-trimethylolpropane trimethacrylate, ethoxylated and / or propoxylated pentaerythritol tetramethacrylate, ethoxylated and / or propoxylated di(1,1,1-trimethylolpropane) tetramethacrylate and ethoxylated and / or propoxylated dipentaerythritol hexamethacrylate.

[0208] The term "(meth)acryloyl" includes acryloyl and methacryloyl.

[0209] The composition of the present invention may also contain a polymerization inhibitor.

[0210] Examples of polymerization inhibitors are 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPOL), 4-benzoyloxy-2,2,6,6-tetramethylpiperidin-1-oxyl, 4-benzyloxy-2,2,6,6-tetramethylpiperidin-1-oxyl, 2,2-diphenyl-1-picrylhydrazyl (DPPH), tris(p-nitrophenyl)methane, p-phenylenediamines such as N,N'-diphenyl-p-phenylenediamine, phenothiazine, hydroxylamines such as N,N-diethylhydroxy Amines (DEHA), quinones such as hydroquinone (HQ), hydroquinone monomethyl ether, 1,4-benzoquinone, tert-butyl hydroquinone, 2,5-bis(1,1,3,3-tetramethylbutyl)hydroquinone, 2,5-bis(1,1-dimethylbutyl)hydroquinone, p-tert-butylcatechol (TBC) and 4-methoxyphenol (MEHQ), alkylated phenols such as 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2,4,6-tri-tert-butylphenol, 2-tert-butyl-4,6-dimethylphenol and 2,6-di-tert-butyl-4-methylphenol.

[0211] The composition of the present invention typically comprises polyurethane (1) in the range of 10 to 70% by weight based on the weight of the composition, more preferably in the range of 20 to 60% by weight based on the weight of the composition, even more preferably in the range of 30 to 50% by weight based on the weight of the composition, and most preferably in the range of 35 to 45% by weight based on the weight of the composition.

[0212] The composition of the present invention typically comprises water in the range of 30% to 90% by weight based on the weight of the composition, more preferably in the range of 80% to 40% by weight based on the weight of the composition, even more preferably in the range of 70% to 50% by weight based on the weight of the composition, and most preferably in the range of 65% to 55% by weight based on the weight of the composition.

[0213] The compositions of the present invention typically comprise less than 10% by weight, more preferably less than 5% by weight, of organic solvents based on the weight of the composition.

[0214] The composition of the present invention may comprise compound (2) in the range of 0 to 50% by weight based on the weight of the composition, more preferably in the range of 0 to 30% by weight based on the weight of the composition, and even more preferably in the range of 0 to 20% by weight based on the weight of the composition. Most preferably, compound (2) is absent from the composition of the present invention.

[0215] The composition of the present invention may comprise a polymerization inhibitor in an amount ranging from 0.001% to 5.000% by weight based on the weight of the polyurethane (1), more preferably in an amount ranging from 0.005% to 2.000% by weight based on the weight of the polyurethane (1), and even more preferably in an amount ranging from 0.010% to 1.000% by weight based on the weight of the polyurethane (1).

[0216] The composition of the invention may be a dispersion or a solution. Examples of dispersions are emulsions (a liquid phase dispersed in a liquid phase) and suspensions (a solid phase dispersed in a liquid phase).

[0217] The composition of the present invention is preferably a dispersion, more preferably a dispersion having an average particle size in the range of 1 to 200 nm, more preferably in the range of 5 to 150 nm, and most preferably in the range of 10 to 100 nm. The average particle size is determined using dynamic light scattering (DLS) ISO 22412, 2017.

[0218] Another aspect of the present invention is a method for preparing the composition of the present invention, the method comprising the following steps

[0219] (i) at least one polyol (B1) carrying at least one COOH group,

[0220] at least one monool (B2) carrying at least one ethylenically unsaturated group,

[0221] optionally at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups,

[0222] at least one polyol (B4) which carries no ethylenically unsaturated groups and no COOH groups,

[0223] at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group, and

[0224] optionally at least one polyisocyanate (A2) not carrying ethylenically unsaturated groups,

[0225] reacting in at least one organic solvent to form a polyurethane prepolymer (3) carrying ethylenically unsaturated groups and COOH groups,

[0226] (ii) optionally reacting a composition comprising the polyurethane prepolymer (3) of step (i) with at least one compound (C1) carrying at least one NH2 group and no OH groups to form a composition comprising a polyurethane prepolymer (4) carrying ethylenically unsaturated groups and COOH groups,

[0227] (iii) reacting at least a portion of the COOH groups of the polyurethane prepolymer (3) of the composition of step (i) or the polyurethane prepolymer (4) of the composition of step (ii) with a base to form a composition comprising a polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, and

[0228] (iv) adding water to the composition of the polyurethane (1) of step (iii) and removing the at least one organic solvent to obtain the composition of the present invention,

[0229] The equivalent ratio of the ethylenically unsaturated groups provided by the polyisocyanate (A1) / the ethylenically unsaturated groups provided by the components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.20 / 1.00 to 0.95 / 1.00.

[0230] The organic solvent of step (i) may be an aliphatic ketone such as acetone, ethyl methyl ketone (2-butanone) or isobutyl methyl ketone, an aliphatic amide such as N-methylpyrrolidone or N-ethylpyrrolidone, an ether such as tetrahydrofuran, dipropylene glycol dimethyl ether or dioxane, a hydrocarbon such as n-heptane, cyclohexane, toluene, o-xylene, m-xylene, p-xylene and a mixture of xylene isomers, an ester such as butyl acetate, an acid such as acetic acid, or a nitrile such as acetonitrile, or a mixture thereof.

[0231] The at least one organic solvent is preferably an aliphatic ketone, and more preferably an aliphatic ketone selected from the group consisting of acetone and ethyl methyl ketone (2-butanone).

[0232] Step (i) is usually carried out in the presence of a polymerization inhibitor.

[0233] Step (i) may be carried out in the presence of at least one catalyst. Preferably, no catalyst is used in step (i).

[0234] Examples of the catalyst are amine catalysts carrying at least one tertiary amino group and organometallic catalysts.

[0235] Examples of amine catalysts carrying at least one tertiary amino group are 1,4-diazabicyclo[2.2.2]octane, N-methylmorpholine, N-methylimidazole, bis[2-(N,N-dimethylamino)ethyl]ether, 2,2′-dimorpholinodiethylether and also tetramethylethylenediamine, dimethylcyclohexylamine, dimethylbenzylamine, dimethylethanolamine and dimethylaminopropylamine.

[0236] Examples of the organometallic catalyst are an organotitanium catalyst, an organotin catalyst, an organozinc catalyst, an organobismuth catalyst, an organozirconium catalyst, an organoiron catalyst, an organoaluminum catalyst, an organomanganese catalyst, an organonickel catalyst, an organocobalt catalyst, an organomolybdenum catalyst, an organotungsten catalyst, and an organovanadium catalyst.

[0237] Examples of organic titanium catalysts are tetra(isopropoxide)titanium(IV) and tetra(butoxide)titanium(IV). Examples of organic tin catalysts are tin diacetate(II), tin di(2-ethylhexanoate)(II), tin dilaurate(II), dimethyltin diacetate(IV), dibutyltin diacetate(IV), dibutyltin dibutyrate(IV), dibutyltin di(2-ethylhexanoate), dibutyltin dilaurate(IV), dioctyltin dilaurate(IV), dioctyltin diacetate(IV), dibutyltin oxide(IV), diphenyltin oxide(IV), dibutyltin dichloride(IV) and dibutyltin maleate(IV). Examples of organic zinc catalysts are zinc diacetate(II), zinc di(2-ethylhexanoate)(II) and zinc dineodecanoate(II). Examples of organic bismuth catalysts are bismuth diacetate(II), bismuth dipivalate(II), bismuth di(2-ethylhexanoate)(II) and bismuth dineodecanoate(II). Examples of organozirconium catalysts are zirconium(IV)tetrakis(acetylacetonate) and zirconium(IV)tetrakis(2,2,6,6-tetramethyl-3,5-heptanedione).

[0238] Step (i) is typically carried out at elevated temperature, such as in the range of 70 to 150°C, preferably in the range of 70 to 100°C, more preferably in the range of 75 to 90°C.

[0239] Typically, step (i) is stopped when an NCO content of less than 2% by weight, preferably less than 1% by weight, based on the weight of the reaction mixture is reached, by adding at least one organic solvent which may be the same as or different from the organic solvent of step (i).

[0240] The equivalent ratio of NCO groups of the polyisocyanates (A1) and (A2) / OH groups of the components (B1), (B2), (B3) and (B4) in step (i) is generally in the range of 1.00 / 1.00 to 1.50 / 1.00, preferably in the range of 1.01 / 1.00 to 1.30 / 1.00, most preferably in the range of 1.02 / 1.00 to 1.20 / 1.00.

[0241] Step (ii), if performed, is typically carried out at a temperature below 80°C.

[0242] If step (ii) is carried out, the equivalent ratio of OH groups of (B1), (B2), (B3) and (B4)) / isocyanate-reactive groups of component (C1) is generally in the range from 50 / 1 to 2 / 1, preferably in the range from 30 / 1 to 5 / 1.

[0243] The base used in step (iii) may be any base. Examples of bases are given above. The base is preferably an alkali metal hydroxide, more preferably sodium hydroxide or potassium hydroxide, and most preferably sodium hydroxide.

[0244] The equivalent ratio of the alkali metal hydroxide / COOH group of the polyurethane prepolymer (3) or (4) is preferably in the range of 40 / 100 to 100 / 100, and most preferably in the range of 60 / 100 to 100 / 100.

[0245] Step (iv) is typically carried out with rapid stirring of the composition.

[0246] If compound (2) is present in the composition of the present invention, step (i) may be carried out in the presence of compound (2). Compound (2) may also be added after step (i), for example, between step (i) or step (ii), or between step (iii) and step (iv). It is also possible to add a portion of compound (2) in step (i) and add another portion of compound (2) later.

[0247] Another part of the present invention is an aqueous coating composition comprising the composition of the present invention, the coating composition comprising a polyurethane (1), at least one additive, optionally at least one initiator and optionally at least one polymer (5) different from the polyurethane (1), wherein the coating composition comprises the polyurethane (1) in the range of 10 to 70% by weight, based on the weight of the coating composition.

[0248] The additive may be any suitable additive.

[0249] Examples of the additives are thickeners, ultraviolet absorbers, light stabilizers, surfactants, polymerization inhibitors, photosensitizers, curing catalysts, defoamers, plasticizers, fillers, pigments, dyes, flow control agents, antioxidants, flame retardants, antistatic agents, thixotropic agents, leveling agents, tackifiers, chelating agents, matting agents, and compatibilizers.

[0250] Examples of thickeners are hydroxymethylcellulose and bentonite. Examples of UV absorbers are benzotriazoles such as 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol and 2-(2H-benzotriazol-2-yl)-p-cresol, triazines such as 2-(4,6-diphenyl-1,3,5-triazin-2-yl)5-((hexyl)oxy)phenol), cyanoacrylates and benzophenones. Examples of light stabilizers are hindered amine light stabilizers (HALS) such as 2,2,6,6-tetramethylpiperidine, 2,6-di-tert-butylpiperidine and bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate. Examples of fillers are talc, diatomaceous earth, clay, aluminum silicate, magnesium silicate, calcium carbonate, calcium sulfate, barium sulfate, aluminum hydroxide, aluminum oxide, and organic fillers such as polyacrylic acid and cellulose. Examples of chelating agents are ethylenediaminetetraacetic acid and β-diketone.

[0251] Initiators are compounds which form free radicals upon thermal treatment (thermal free radical initiators) or irradiation (photoinitiators).

[0252] Examples of thermal free radical initiators are peroxides such as potassium persulfate, dibenzoyl peroxide, cyclohexanone peroxide, di-tert-butyl peroxide, acetylcyclohexylsulfonyl peroxide, diisopropyl percarbonate, tert-butyl peroctoate, cumene hydroperoxide, dicumyl peroxide and tert-butyl perbenzoate, azobisisobutyronitrile and benzopinacol.

[0253] Examples of photoinitiators are acetophenone, 2,2-dimethoxy-2-phenylacetophenone (benzil dimethyl ketal), 2,2-diethoxyacetophenone, 4-dimethylaminoacetophenone, benzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, 4-hydroxybenzophenone, 4-phenylbenzophenone, 2-chlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, thioxanthone, isopropyl-9H-thioxanthene-9-one, methyl phenylglyoxylate, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, benzoin dimethyl ketal, cyclohexyl phenyl ketone, 1-hydroxycyclohexyl phenyl ketone, p-isopropyl-2-hydroxyisobutyrophenone, 2-hydroxy-2-methyl-1-phenyl-1 -acetone, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-methyl-1-(4-methylthienyl)-2-morpholinopropan-1-one, 4-(2-hydroxyethoxy)phenyl 2-hydroxy-2-propyl ketone, acylphosphine oxides (such as diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide), methyl-2-benzoyl benzoate and ethylphenyl(2,4,6-trimethylbenzoyl)phosphinate.

[0254] Mixtures of initiators may also be used. Examples of mixtures of initiators are mixtures of at least two photoinitiators, mixtures of at least one photoinitiator and at least one thermal free radical initiator, and mixtures of at least two thermal free radical initiators.

[0255] Common mixtures of photoinitiators are mixtures of bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone, mixtures of 1-hydroxycyclohexyl phenyl ketone and benzophenone, mixtures of bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide and 1-hydroxy-cyclohexyl phenyl ketone, mixtures of diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide and 2-hydroxy-2-methyl-1-phenyl-1-propanone, mixtures of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone, and mixtures of 4-methylbenzophenone and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

[0256] The at least one initiator is preferably a photoinitiator, more preferably a UV photoinitiator. UV photoinitiators are initiators that form free radicals when treated with UV radiation. Preferred initiators are selected from the group consisting of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, ethylphenyl (2,4,6-trimethylbenzoyl) phosphinate, benzophenone, phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide, 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and 2,2-dimethoxy-2-phenylacetophenone (benzil dimethyl ketal).

[0257] The polymer (5) may be any polymer different from the polyurethane (1). The polymer (5) may be a polymer carrying an ethylenically unsaturated group or a polymer not carrying an ethylenically unsaturated group. Examples of the polymer (5) are polyurethanes, acrylic polymers, mixtures of polyurethanes and acrylic polymers, polyesters, polyethers, polycarbonates, epoxy resins, alkyd resins, polyolefins and polyvinyl acetates, and acrylated or methacrylated derivatives thereof.

[0258] If polymer (5) is a polymer not carrying ethylenically unsaturated groups, the hydroxyl value of polymer (5) is preferably in the range of 1 to 300 mg KOH / g, and the acid value is preferably lower than 50 mg KOH / g.

[0259] Acrylated and methacrylated derivatives can be prepared by methods known in the art, for example by esterifying the OH groups of polyesters, acrylic polymers and polyethers with acrylic acid or methacrylic acid or by ring-opening the epoxy groups of epoxy resins with acrylic acid or methacrylic acid.

[0260] Polyurethane is a polymer containing a urethane linking group. Polyurethane is usually obtained by the reaction of a diol with a diisocyanate. The diol can be a polyester diol, an acrylic polymer diol, a polycarbonate diol or a polyether diol. The polyurethane can contain additional linking groups in the backbone that are less than the number of urethane groups, such as ester, ether, thioether or urethane linking groups. Acrylated or methacrylated alcohols or diols can also be used as synthesis components to obtain acrylated or methacrylated polyurethanes.

[0261] Acrylic polymers are usually obtained by free radical polymerization of polymerizable unsaturated monomers containing acrylate or methacrylate and optionally other polymerizable unsaturated monomers by methods known in the art (such as emulsion polymerization). Examples of other polymerizable unsaturated monomers are polymerizable unsaturated monomers carrying OH groups such as (meth) 2-hydroxyethyl acrylate, (meth) 2-hydroxypropyl acrylate, (meth) 3-hydroxypropyl acrylate, (meth) 4-hydroxybutyl acrylate and (meth) allyl alcohol, and polymerizable unsaturated monomers carrying acidic groups such as acrylic acid, methacrylic acid, maleic acid, citraconic acid, itaconic acid, maleic anhydride, citraconic anhydride and itaconic anhydride. Preferably, polymerizable unsaturated monomers also include polymerizable unsaturated monomers carrying OH groups. The hydroxyl value of acrylic polymers is preferably in the range of 1 to 200 mg KOH / g, more preferably in the range of 2 to 100 mg KOH / g, and most preferably in the range of 3 to 50 mg KOH / g. The weight average molecular weight of the acrylic polymer is preferably 1,000 to 200,000 g / mol, more preferably 2,000 to 100,000 g / mol, and most preferably 3,000 to 50,000 g / mol.

[0262] For example, by preparing an acrylic polymer as described above, but in the presence of a polyurethane, a mixture of a polyurethane and an acrylic polymer can be obtained.

[0263] Polyester is a polymer comprising monomers connected via an ester linking group. Polyester is generally obtained by esterification or transesterification of a component carrying two acidic groups and a diol. Polyester may contain a linking group other than an ester group whose number is less than or equal to the number of ester groups, such as a carbonate, ether, thioether or urethane linking group. The hydroxyl value of polyester is preferably about 1 to 300 mg KOH / g, more preferably about 50 to 250 mg KOH / g, and even more preferably about 80 to 180 mg KOH / g. The acid value of polyester resin is preferably about 1 to 200 mg KOH / g, more preferably about 15 to 100 mg KOH / g, and even more preferably less than 50 mg KOH / g. The weight average molecular weight of polyester is preferably 500 to 500000 g / mol, more preferably 1000 to 300000 g / mol, and even more preferably 1500 to 200000 g / mol.

[0264] Polyethers are polymers containing ether linking groups. Polyethers are usually prepared by acid-catalyzed polymerization of ethers (such as ethylene oxide, propylene oxide, butylene oxide or tetrahydrofuran) using alcohols. Examples of polyethers are polyoxyethylene polyethers, polyoxypropylene polyethers, polyoxybutylene polyethers and polytetrahydrofuran. Polyethers can include additional linking groups in the main chain that are less than the number of ether groups, such as esters, carbonates, thioethers or urethane linking groups.

[0265] Polycarbonate is a polymer containing carbonate linking groups. Polycarbonate is usually obtained by the reaction of carbonate and diol. Polycarbonate can contain additional linking groups in the main chain whose number is less than the number of carbonate groups, such as ester, ether, thioether or urethane linking groups.

[0266] Epoxy resins are polymers that carry epoxy groups. Epoxy polymers can be obtained by reacting polyols with epichlorohydrin followed by dehydrohalogenation. Examples of polyols are bisphenol A and bisphenol F and novolac resins (which are polymers formed by reacting phenol with formaldehyde).

[0267] Alkyd resins are polyesters carrying fatty acid derived groups. Alkyd resins are usually obtained by esterification or transesterification of components carrying two acidic groups, polyols and glycerol fatty acid triesters. Examples of components carrying two acidic groups are phthalic anhydride and maleic anhydride. Examples of polyols are trimethylolpropane, glycerol and pentaerythritol. Examples of glycerol fatty acid triesters are soybean oil, linseed oil and coconut oil.

[0268] Polyolefins are polymers obtainable by polymerizing at least one olefin monomer, optionally in the presence of at least one polymerizable unsaturated monomer that is not an olefin monomer, by methods known in the art, such as emulsion polymerization. Olefin monomers are monomers containing only H and C atoms. Examples of olefin monomers are ethylene, propylene, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-heptene, 1-hexene, 1-decene, and 1-dodecene; conjugated dienes and non-conjugated dienes such as butadiene, ethylidene norbornene, dicyclopentadiene, and 1,5-hexadiene and styrene. Examples of polymerizable unsaturated monomers that are not olefin monomers are vinyl acetate, vinyl alcohol, maleic acid, citraconic acid, itaconic acid, maleic anhydride, citraconic anhydride, and itaconic anhydride.

[0269] Preferred polymers (5) are selected from the group consisting of polyurethanes, acrylic polymers, mixtures of polyurethanes and acrylic polymers, and acrylated or methacrylated derivatives thereof.

[0270] The coating composition of the present invention generally comprises polyurethane (1) in the range of 10 to 70% by weight based on the weight of the coating composition, more preferably in the range of 15 to 50% by weight based on the weight of the coating composition, most preferably in the range of 20 to 45% by weight based on the weight of the coating composition.

[0271] The coating composition of the present invention typically comprises additives in the range of 0.05% to 40% by weight based on the weight of the coating composition, and most preferably in the range of 0.1% to 20% by weight based on the weight of the coating composition.

[0272] The coating composition of the present invention preferably comprises at least one initiator in the range of 0.05 to 7.0% by weight based on the weight of polyurethane (1), more preferably in the range of 0.1 to 5.0% by weight based on the weight of polyurethane (1).

[0273] The coating composition of the present invention generally comprises the polymer (5) in the range of 0 to 50% by weight, based on the coating composition, more preferably in the range of 0 to 25% by weight, based on the coating composition.

[0274] The coating composition of the invention typically comprises at least 20% by weight, more preferably at least 40% by weight, of water based on the weight of the coating composition.The coating composition of the invention typically comprises less than 10% by weight of an organic solvent based on the weight of the coating composition.

[0275] The coating composition may be a dispersion or a solution. Preferably, the coating composition is a dispersion.

[0276] In a preferred embodiment, the coating composition of the present invention is a primer composition, preferably a primer composition that does not contain a pigment.

[0277] In another preferred embodiment, the coating composition of the present invention is a pigmented wood stain composition.

[0278] The coating composition of the present invention can be prepared by mixing the composition of the present invention, at least one additive, at least one initiator, optionally at least one polymer (5) and optionally additional water. In the mixing step, the at least one additive, the at least one initiator and the at least one polymer (5) (if present) can be used "as is" or as a solution or dispersion in an organic solvent and / or water. In the mixing step, the polymer (5) selected from the group consisting of polyurethanes, acrylic polymers, mixtures of polyurethanes and acrylic polymers and acrylated or methacrylated derivatives thereof is usually used as an aqueous solution or dispersion.

[0279] Another aspect of the present invention is a crosslinked layer formed from the coating composition of the present invention.

[0280] The crosslinked layer can be obtained by a method comprising the steps of: (i) applying the coating composition of the present invention to a substrate to form a layer, (ii) optionally drying the layer of step (i), and (iii) treating the layer of step (i) or step (ii) with heat, radiation or electron beam to form a crosslinked layer.

[0281] The coating compositions of the present invention can be applied to the substrate by any method known in the art, such as by a doctor bar, spraying, troweling, knife coating, brushing, rolling, roller coating, flow coating and lamination, doctor blade, various printing processes such as gravure, transfer, lithography and inkjet printing, and by using a rod.

[0282] The layer obtained directly after applying the coating composition to the substrate preferably has a thickness in the range of 20 to 500 micrometers, more preferably in the range of 40 to 300 micrometers, most preferably in the range of 60 to 240 micrometers and in particular 60 to 200 micrometers.

[0283] The layer obtained directly after application of the coating composition to the substrate is generally referred to as the wet layer.

[0284] The layer from step (i) may be dried in step (ii) to remove at least a substantial portion of the water (and other volatiles such as organic solvents).

[0285] The layer obtained after removing at least most of the water (and other volatiles, such as organic solvents) is often referred to as the dried layer.

[0286] Step (ii), if present, is preferably carried out at a temperature in the range of 15° C. to 160° C., more preferably in the range of 40° C. to 160° C. In case a thermal free radical initiator is present in the coating composition, the drying conditions (temperature and time) are preferably chosen such that the thermal free radical initiator is not activated.

[0287] In step (iii), the layer of step (i) or step (ii) is treated with electron beam, heat or radiation to form a cross-linked layer. Heat may also be applied by near infrared (NIR) radiation, such as radiation with a wavelength in the range of 760 to 2500 nm. Preferably, the layer of step (i) or (ii) is treated with ultraviolet radiation, sunlight or electron beam. More preferably, the layer of step (i) or (ii) is treated with radiation with a wavelength in the range of 200 to 700 nm, even more preferably in the range of 200 to 500 nm, and most preferably in the range of 250 to 400 nm.

[0288] Examples of radiation sources are low-pressure mercury vapor lamps, medium-pressure mercury vapor lamps, high-pressure mercury vapor lamps, lasers, pulsed lamps (flash lamps), halogen lamps and excimer lamps. The radiation dose is usually selected to be sufficient for crosslinking. In the case of UV radiation, 80 to 3000 mJ / cm 2 , preferably 100 to 2000 mJ / cm 2 A combination of different radiation sources may also be used.

[0289] Step (iii) can be carried out in the presence of oxygen or preferably in the absence of oxygen (e.g., in an inert gas atmosphere). Suitable inert gases are nitrogen, argon and carbon dioxide. The layer of step (i) or (ii) can also be covered with a transparent medium such as a transparent polymer film, glass or water and irradiated through the transparent medium. Irradiation can also be carried out by passing the substrate coated with the layer of step (i) or (ii) through a radiation source at a constant speed.

[0290] In a preferred embodiment, step (ii) is performed and in step (iii) the layer of step (ii) is treated with radiation to form a cross-linked layer.

[0291] Step (i), and optionally step (ii) and step (iii) may be repeated to obtain multiple cross-linked layers.

[0292] The substrate can be any suitable substrate. The substrate can be a wood substrate, an engineering wood substrate, an engineering bamboo substrate, an engineering cellulose substrate except engineering wood or engineering bamboo substrate, a fiber reinforced composite substrate (FRC), a wood-plastic composite substrate (WPC), a plastic substrate (such as a melamine formaldehyde substrate), a paper substrate, a recycled paper substrate, a paperboard (also referred to as a cardboard) substrate, a recycled paperboard (also referred to as a recycled cardboard) substrate, a metal substrate, a stone substrate, a glass substrate, a textile substrate, a leather substrate, a ceramic substrate, a mineral building material substrate (such as molded cement block and fiber-cement board). The substrate can be pre-coated with a coating composition different from the coating composition of the present invention. Preferably, the substrate is not pre-coated with a coating composition different from the coating composition of the present invention.

[0293] Examples of wood substrates are oak, beech, maple, alder, ash, pine, fir, spruce, chestnut, acacia, birch, elm, teak, walnut and roach, and also cork.

[0294] The wood may be, for example, in the form of sawn timber (also known as lumber), in the form of planks for flooring (e.g. parquet), in the form of fixtures for house construction or household applications, or in the form of solid wood furniture. The cork may be, for example, in the form of tiles for flooring, or in the form of fixtures for household applications.

[0295] Engineered wood substrates are derived wood substrates that are manufactured by bonding or fixing strips, particles, fibers, veneers or boards of wood with adhesives or other fixing methods to form a composite material. Examples of adhesives are urea-formaldehyde resins, phenolic resins, melamine formaldehyde resins, polymeric methylene diphenyl diisocyanate, polyvinyl acetate and polyurethane. Examples of engineered wood substrates are glued laminated timber, cross-laminated timber (CLT), parallel strand sawn timber (PSL), strand laminated timber (LSL), laminated veneer sawn timber (LVL), plywood, oriented strand board (OSB), composite board, particle board (also called particle board or chip plywood), fiberboard such as hardboard (also called high-density fiberboard, HDF) and medium-density fiberboard (MDF).

[0296] The engineered wood substrate may be in the form of sheets for engineered wood flooring (eg, laminate flooring), in the form of fixtures for building construction or household applications, and in the form of furniture (eg, flat-pack furniture).

[0297] Engineered bamboo substrates are derived bamboo substrates made by bonding or fixing bamboo sections with adhesives or other fixing methods to form a composite material. An example of an engineered bamboo substrate is laminated bamboo.

[0298] Engineered cellulose substrates other than engineered wood substrates and engineered bamboo substrates are products derived from lignin-containing materials other than wood and bamboo (such as rye straw, wheat straw, rice straw, hemp stalks, kenaf stalks and bagasse), which are manufactured by bonding or fixing parts of lignin-containing materials other than wood and bamboo with adhesives or other fixing methods to form composite materials.

[0299] The fiber-reinforced composite substrate (FRC) is made of rice-derived fibers and plastic.

[0300] Wood-plastic composites (WPC) are composite materials made from wood fibers or wood powder and thermoplastic polymers such as polyethylene, polypropylene, polyvinyl chloride or polyacetic acid.

[0301] Preferably, the substrate is selected from the group consisting of a wood substrate, an engineered wood substrate, an engineered bamboo substrate, an engineered cellulose substrate other than an engineered wood or engineered bamboo substrate, a fiber reinforced composite substrate (FRC), a wood-plastic composite substrate (WPC), a plastic substrate (such as a melamine formaldehyde substrate), a paper substrate, a recycled paper substrate, a paperboard (also known as cardboard) substrate, a recycled paperboard (also known as recycled cardboard) substrate.

[0302] More preferably, the substrate is selected from the group consisting of a wood substrate, an engineered wood substrate, an engineered bamboo substrate, an engineered cellulose substrate other than an engineered wood or engineered bamboo substrate.

[0303] Even more preferably, the substrate is selected from the group consisting of a wood substrate and an engineered wood substrate. Most preferably, the substrate is selected from the group consisting of a wood substrate and an engineered wood substrate comprising a veneer (such as a veneer). In particular, the substrate is selected from the group consisting of an oak substrate and an engineered wood substrate comprising an oak veneer (such as an oak veneer).

[0304] Another part of the invention is a substrate coated with a layer according to the invention.

[0305] Another part of the present invention is the use of the coating composition of the invention as a primer composition, preferably as a primer composition which does not comprise pigments.

[0306] Another part of the invention is the use of the coating composition of the invention as a colored wood stain composition.

[0307] An advantage of the compositions of the invention, and in particular the coating compositions of the invention, is that these compositions form wet layers, for example on black glass panels, which already have good transparency.

[0308] The advantages of the compositions of the invention, and in particular the coating compositions of the invention comprising polyurethanes which also contain units derived from component C1, are particularly that these compositions, for example on black glass panes, form wet layers which are transparent and therefore exhibit high transparency.

[0309] An advantage of the compositions of the invention, and in particular the coating compositions of the invention, is that the dried layers formed from these compositions on substrates, for example on glass plates, are redispersible or redissolvable in water at ambient temperature over a certain period of time. This allows the removal of dried residues formed from the compositions on the machines and equipment used to apply the compositions to the substrates.

[0310] The compositions of the invention, and in particular the coating compositions of the invention, are also advantageous in that the layers, in particular the dried layers, formed from these compositions on the substrate are redispersible or redissolvable in the composition itself within a certain period of time at ambient temperature.

[0311] The compositions of the invention, and in particular the coating compositions of the invention, are also advantageous in that the crosslinked layers formed from these compositions on substrates, in particular on wood substrates or engineered wood substrates comprising veneers, such as oak veneers, exhibit high water resistance.

[0312] The compositions of the invention, and in particular the coating compositions of the invention, are also advantageous in that the crosslinked layers formed from these compositions on substrates, in particular on wood substrates or engineered wood substrates comprising veneer, such as oak veneer, exhibit good polishability.

[0313] The compositions of the invention, and in particular the coating compositions of the invention, are also advantageous in that the crosslinked layers formed from these compositions on substrates, for example on black glass plates, are transparent and therefore exhibit high transparency.

[0314] The compositions of the invention, and in particular the coating compositions of the invention, exhibit an advantageous combination of the following properties: redispersibility or redissolubility of the dried layer before crosslinking and at the same time high water resistance of the crosslinked layer on wood substrates and or engineered wood substrates comprising veneer, such as oak veneer.

[0315] The compositions of the invention, and in particular the coating compositions of the invention, exhibit an advantageous combination of the following properties: redispersibility or redissolubility of the dried layer before crosslinking and at the same time high water resistance and good polishability of the crosslinked layer on wood substrates and engineered wood substrates comprising veneer, such as oak veneer.

[0316] The compositions of the invention, and in particular the coating compositions of the invention, exhibit an advantageous combination of the following properties: redispersibility or redissolubility of the dry layer before crosslinking and at the same time high water resistance and good polishability of the crosslinked layer on wood substrates and engineered wood substrates including veneers, such as oak veneers, and good to high transparency of the wet layer and high transparency of the crosslinked layer.

[0317] Examples

[0318] Compound or composition NCO content [NCO weight / weight of compound or composition] is determined by first treating the compound / composition with di-n-butylamine and then back-titrifying the unreacted di-n-butylamine to determine the amount of di-n-butylamine reacted. The following method can be used: 10mL of a 1N solution of di-n-butylamine in xylene is added to 1g of the compound / composition to be analyzed dissolved in 100mL of N-methylpyrrolidone. The resulting mixture is stirred at room temperature for five minutes. Then, the resulting reaction mixture is back-titrated with 1N hydrochloric acid to measure the volume of hydrochloric acid required to neutralize the unreacted di-n-butylamine. This reveals how many mol di-n-butylamine reacts with the NCO group. The NCO content is the weight of (mol of di-n-butylamine reacted x molecular weight of NCO) / compound / composition. The weight of the compound / composition is 1g. The molecular weight of NCO is 42g / mol.

[0319] Ethylenically unsaturated group density of polyisocyanate (A1) [Milliequivalent ethylenically unsaturated groups / g polyisocyanate (A1)] 1 H-NMR was determined using 1,4-dimethyl terephthalate as an internal standard. 1H-NMR is obtained from a mixture of a specific amount of a polyisocyanate (A1) carrying at least one ethylenic bond (= weight of polyisocyanate) and a specific amount of 1,4-dimethyl terephthalate (= weight of 1,4-dimethyl terephthalate) in deuterated chloroform. The ratio of the integrated intensity of the signal of the selected protons of the ethylenically unsaturated groups provided by the polyisocyanate (A1) to the integrated intensity of the signal provided by the aromatic protons of 1,4-dimethyl terephthalate is determined. The ethylenically unsaturated group density of the polyisocyanate (A1) carrying at least one ethylenically unsaturated group [mmol ethylenically unsaturated group / g polyisocyanate (A1)] is (weight of 1,4-dimethyl terephthalate x number of aromatic protons of 1,4-dimethyl terephthalate x ratio of signal integrated intensity of selected protons of ethylenically unsaturated groups provided by polyisocyanate (A1) to signal integrated intensity of aromatic protons provided by 1,4-dimethyl terephthalate) / (molecular weight of 1,4-dimethyl terephthalate x number of selected protons of ethylenically unsaturated groups of polyisocyanate (A1) x weight of polyisocyanate). The molecular weight of 1,4-dimethyl terephthalate is 194 g / mol. The number of aromatic protons of 1,4-dimethyl terephthalate is 4. The selected protons of the ethylenically unsaturated groups provided by the polyisocyanate (A1) are the two protons at the terminal ends of the acryloyl groups.

[0320] Carrying at least one ethylenically unsaturated bond Allophanate group density of polyisocyanate (A1) [Milliequivalent allophanate groups / g polyisocyanate (A1)] is determined by NMR by a method known in the art.

[0321] Ethylenically unsaturated group density of polyurethane [Milliequivalent ethylenically unsaturated groups / g polyurethane] is determined by calculation. The ethylenically unsaturated group density of the polyurethane is the sum of [weight ratio (B1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1) multiplied by the ethylenically unsaturated group density of (B1)], and [weight ratio (B2) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1) multiplied by the ethylenically unsaturated group density of (B2)], and [weight ratio (B3) / (A1), (B1), (B2) ), (B3), (B4), (A1), (A2) and (C1) multiplied by the ethylenically unsaturated group density of (B3)], and [weight ratio (A1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1) multiplied by the ethylenically unsaturated group density of (A1)], and [weight ratio (C1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2) and (C1) multiplied by the ethylenically unsaturated group density of (C1)].

[0322] Density of COOH groups and their salt groups in polyurethane [Milliequivalent COOH and its salt groups / gPU] is determined by calculation. The COOH group and its salt group density of polyurethane is the sum of the following terms:

[0323] [weight ratio (B1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1)] multiplied by the COOH group density of (B1), and

[0324] [weight ratio (B2) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1) multiplied by the COOH group density of (B2)], and

[0325] [Weight ratio (C1) / (A1), (B1), (B2), (B3), (B4), (A1), (A2), (A3) and (C1)] multiplied by the COOH group density of (C1).

[0326] Number average molecular weight Mn and weight average molecular weight Mw Determined using gel permeation chromatography calibrated with polystyrene standards.

[0327] Example 1

[0328] Preparation of polyisocyanates A1a containing at least one ethylenically unsaturated group

[0329] Hexamethylene diisocyanate was introduced into the reaction vessel under nitrogen. 20 mol% (based on hexamethylene diisocyanate) of 2-hydroxyethyl acrylate was added. The mixture was heated to 80°C and 200 ppm by weight (based on HDI) of N,N,N-trimethyl-N-(2-hydroxypropyl)ammonium 2-ethylhexanoate was added. The temperature was slowly raised to 120°C and the reaction was carried out at this temperature, and when the NCO content reached 26.0 wt% based on the weight of the reaction mixture, the reaction was stopped by adding 250 ppm by weight (based on HDI) of di(2-ethylhexyl) phosphate. Unreacted hexamethylene diisocyanate was removed using a thin film evaporator at 135° C. and 2.5 mbar to give a polyisocyanate A1a having an NCO content of 15.0 wt. %, a weight average molecular weight (Mw) of 563.48 g / mol, an average NCO functionality of 2.0, an ethylenically unsaturated group density of 2.15 milliequivalents of ethylenically unsaturated bonds / g of A1a, and an allophanate group density of 1.74 milliequivalents of allophanate groups / g of A1a.

[0330] Example 2

[0331] Preparation of aqueous polyurethane dispersion PUD1a containing polyurethane 1a

[0332] At 22°C, 46.64 g of 2,2-bis(hydroxymethyl)propionic acid, 146.55 g of polytetrahydrofuran (MW 1000 g / mol), 89.34 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08 g of 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200 g of butanone were mixed. 516.59 g of the polyisocyanate A1a of Example 1 was added, the temperature was raised to 80°C, and the reaction mixture was allowed to react until an NCO content of 0.33 wt % based on the weight of the reaction mixture was reached. The mixture was diluted with 372 g of acetone, causing the temperature to drop below 80°C. 111.59 g of a 10 wt % solution of NaOH in water was added to the mixture, and the reaction mixture was allowed to react for 5 min. 1150 g of water was added to the reaction mixture under rapid stirring. The organic solvent was removed by distillation to obtain an aqueous composition PUD1a containing polyurethane 1a, which had a solid content of 40.3 wt % and the properties shown in Table 1.

[0333] Comparative Example 1

[0334] Preparation of comparative aqueous polyurethane dispersion cPUD1 comprising comparative polyurethane c1

[0335] At 22°C, 51.96 g of 2,2-bis(hydroxymethyl)propionic acid, 44.57 g of polytetrahydrofuran (MW 1000 g / mol), 231.84 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08 g of 2,2,6,6-tetramethylpiperidine-1-oxyl (polymerization inhibitor) and 200 g of butanone were mixed. 396.33 g of hexamethylene diisocyanate trimer (NCO content: 22 wt %), 75.18 g of hexamethylene diisocyanate were added, the temperature was raised to 80°C, and the reaction mixture was allowed to react until an NCO content of 0.4 wt % based on the weight of the reaction mixture was reached. The mixture was diluted with 372 g of acetone, causing the temperature to drop below 80°C. 124.1 g of a 10 wt % solution of NaOH in water (80% neutralization) was added to the mixture, and the reaction mixture was allowed to react for 10 min. 1150 g of water was added to the reaction mixture under rapid stirring. The organic solvent was removed by distillation to obtain an aqueous composition cPUD1 containing polyurethane c1, which had a solid content of 40.3 wt % and the properties shown in Table 1.

[0336] Comparative Example 2

[0337] Preparation of comparative aqueous polyurethane dispersion cPUD2 comprising comparative polyurethane c2

[0338] At 22°C, 49.17 g of 2,2-bis(hydroxymethyl)propionic acid (DMPA), 126.42 g of polytetrahydrofuran (MW 1000 g / mol), 167.35 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08 g 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200 g butanone were mixed. 393.27 g HA 3000 (available from BASF, an allophanate-modified polyisocyanate based on isocyanurated hexamethylene diisocyanate and not carrying ethylenically unsaturated groups, NCO content: 19 wt %) and 63.79 g of hexamethylene diisocyanate, the temperature is raised to 80° C., and the reaction mixture is allowed to react until an NCO content of 0.37 wt % based on the weight of the reaction mixture is reached. The mixture is diluted with 372 g of acetone, causing the temperature to drop below 80° C. 117.42 g of a 10 wt % solution of NaOH in water (80% neutralization) is added to the mixture, and the reaction mixture is allowed to react for 10 min. 1150 g of water are added to the reaction mixture under rapid stirring. The organic solvent is removed by distillation to obtain an aqueous composition cPUD2 containing polyurethane c2, which has a solid content of 39.6 wt % and the properties as shown in Table 1.

[0339] Example 3

[0340] Preparation of aqueous polyurethane dispersion PUD1b containing polyurethane 1b

[0341] At 22°C, 39.85 g of 2,2-bis(hydroxymethyl)propionic acid, 144.18 g of polytetrahydrofuran (MW 1000 g / mol), 87.9 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08g 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200g butanone were mixed. 508.23g of the polyisocyanate A1a of Example 1 was added, the temperature was raised to 80°C, and the reaction mixture was allowed to react until an NCO content of 0.6% by weight based on the weight of the reaction mixture was reached. The mixture was diluted with 370g of acetone, causing the temperature to drop below 80°C. 18.97g of a 50% by weight solution of N-aminoethyl-2-aminoethanesulfonic acid sodium salt in water was added to the mixture, and the reaction mixture was allowed to react for 10min. 95.36g of a 10% by weight solution of NaOH in water was added to the mixture, and the reaction mixture was allowed to react for 5min. 1150g of water was added to the reaction mixture under rapid stirring. The organic solvent was removed by distillation to obtain an aqueous composition PUD1b containing polyurethane 1b, which had a solid content of 40.6% by weight and the properties shown in Table 1.

[0342] Comparative Example 3

[0343] Preparation of comparative aqueous polyurethane dispersion cPUD3 comprising comparative polyurethane c3

[0344] At 22°C, 39.72 g of dimethylolpropionic acid (DMPA), 123.49 g of polytetrahydrofuran (MW 1000 g / mol), 163.48 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08 g 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200 g butanone were mixed. 384.00 g HA 3000 (available from BASF, an allophanate-modified polyisocyanate based on hexamethylene diisocyanate and not carrying ethylenically unsaturated groups, NCO content: 19 wt %), 62.24 g of hexamethylene diisocyanate, the temperature is raised to 80° C., and the reaction mixture is allowed to react until an NCO content of 0.98% based on the weight of the reaction mixture is reached. The mixture is diluted with 372 g of acetone, causing the temperature to drop below 80° C. 26.00 g of a 50 wt % solution of N-aminoethyl-2-aminoethanesulfonic acid sodium salt in water are added to the mixture, and the reaction mixture is allowed to react for 10 min. 95.02 g of a 10 wt % solution of NaOH in water are added to the mixture, and the reaction mixture is allowed to react for 5 min. 1150 g of water are added to the reaction mixture under rapid stirring. The organic solvent is removed by distillation to obtain an aqueous composition cPUD3 containing polyurethane c3, which has a solid content of 40.2 wt % and the properties shown in Table 1.

[0345] Example 4

[0346] Preparation of aqueous polyurethane dispersion PUD1c containing polyurethane 1c

[0347] At 22°C, 39.85 g of 2,2-bis(hydroxymethyl)propionic acid and 144.18 g of 6800 / 2 (aliphatic polyester diol with a hydroxyl number of 112 mg KOH / g from BASF SE), 87.9 g of 2-hydroxyethyl acrylate, 0.8 g of Kerobit TBK (polymerization inhibitor), 0.08 g of 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200 g of butanone were mixed. 508.23 g of polyisocyanate A1a from Example 1 were added, the temperature was raised to 80° C., and the reaction mixture was allowed to react until an NCO content of 0.6 wt % based on the weight of the reaction mixture was reached. The mixture was diluted with 370 g of acetone, causing the temperature to drop below 80° C. 18.97 g of a 50 wt % solution of N-aminoethyl-2-aminoethanesulfonic acid sodium salt in water was added to the mixture, and the reaction mixture was allowed to react for 10 min. 95.36 g of a 10 wt % solution of NaOH in water was added to the mixture, and the reaction mixture was allowed to react for 5 min. 1150 g of water were added to the reaction mixture under rapid stirring. The organic solvent was removed by distillation to obtain an aqueous composition PUD1c containing polyurethane 1c having a solid content of 41.5 wt % and the properties as shown in Table 1.

[0348] Example 5

[0349] Preparation of aqueous polyurethane dispersion PUD1d containing polyurethane 1d

[0350] At 22°C, 39.85 g of 2,2-bis(hydroxymethyl)propionic acid and 144.18 g of 7800 / 1 (polyester diol from BASF AG, hydroxyl number: 112 mg KOH / g), 87.9 g 2-hydroxyethyl acrylate, 0.8 g Kerobit TBK (polymerization inhibitor), 0.08 g 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor) and 200 g butanone were mixed. 508.23 g polyisocyanate A1a from Example 1 were added, the temperature was raised to 80° C., and the reaction mixture was allowed to react until an NCO content of 0.6 wt % based on the weight of the reaction mixture was reached. The mixture was diluted with 370 g acetone, causing the temperature to drop below 80° C. 18.97 g of a 50 wt % solution of N-aminoethyl-2-aminoethanesulfonic acid sodium salt in water were added to the mixture, and the reaction mixture was allowed to react for 10 min. 95.36 g of a 10 wt % solution of NaOH in water were added to the mixture, and the reaction mixture was allowed to react for 5 min. 1150 g water were added to the reaction mixture with rapid stirring. The organic solvent was removed by distillation to obtain an aqueous composition PUD1d containing polyurethane 1d having a solid content of 39.2% by weight and the properties shown in Table 1.

[0351] Example 6

[0352] Preparation of coating compositions comprising aqueous polyurethane dispersions PUD1a, PUD1b, PUD1c and PUD1d of Examples 2, 3, 4 and 5, respectively, and comparative coating compositions comprising comparative aqueous polyurethane dispersions cPUD1, cPUD2 and cPUD3 of Comparative Examples 1, 2 and 3, respectively.

[0353] The aqueous polyurethane dispersions PUD1a, PUD1b, PUD1c and PUD1d of Examples 2, 3, 4 and 5 and the comparative aqueous polyurethane dispersions cPUD1, cPUD2 and cPUD3 of Comparative Examples 1, 2 and 3 were diluted with water to a solid content of 35 wt %. 1173 (photoinitiator, available from BASF) was mixed with 1 part by weight of Byk-346 (silicone surfactant). TM 100 g of diluted aqueous polyurethane dispersion (35 wt %) and 2.0 g of 1 / 1 (wt / wt) mixture of 1173 and Byk-346 and 10.0 g PU 1340 (thickener, available from BASF) was mixed for 4 minutes to obtain a coating composition. The coating composition was stored at room temperature overnight and used for the application tests described in Examples 7 to 10 the next day.

[0354] Example 7

[0355] Preparation of a black glass plate coated with the coating composition of Example 6

[0356] The coating composition of Example 6 was remixed manually using a wooden spatula and applied to a black glass plate surface using a 100 micron twin box film applicator to form a layer. The clarity of the wet layer (i.e., the layer just applied) was analyzed by visual inspection and graded as follows:

[0357] 1: White

[0358] 2: Creamy / white

[0359] 3: Milky white

[0360] 4: Transparent

[0361] 60 minutes after the coating composition was applied, UV irradiation was performed using a Hg lamp with a lamp power of 50% (2 x 10 m / min, about 1200 mJ / cm 2 The dried layer was treated with a dosage of 50% to form a cross-linked layer. After cooling to room temperature, the transparency of the cross-linked layer was analyzed by visual inspection and graded as follows:

[0362] 1: Turbid, with small holes

[0363] 2: Turbid

[0364] 3: Transparent

[0365] The results are listed in Table 1.

[0366] Example 8

[0367] Preparation of glass plate coated with the coating composition of Example 6

[0368] The coating composition of Example 6 was remixed manually using a wooden spatula and applied to the surface of the long glass plate using a 200 micron small box film applicator to form a wet layer. The layer on the long glass plate was dried at room temperature for 10 minutes and then dried in a convection drying oven at 50°C for 15 minutes.

[0369] After the long glass plate has cooled to room temperature, approximately one third of the long glass plate (dry layer facing upward) is kept under a jet of demineralized water for 20 seconds, and then the upward side of the water-treated portion of the long glass plate is immediately wiped with a paper towel.

[0370] Whether the dry layer on the upward side after wiping of the water-treated portion of the long glass plate was removed was analyzed by visual inspection and graded as follows:

[0371] No: Drying layer not removed or only partially removed

[0372] Yes: Drying layer is removed

[0373] The results are listed in Table 1.

[0374] Example 9

[0375] Preparation of veneered oak board coated with the coating composition of Example 6

[0376] The coating composition of Example 6 was remixed manually using a wooden spatula and applied to the veneered oak board surface using a 100 micron wide box applicator to form a wet layer. The layer on the oak veneer board was dried at room temperature for 10 minutes and then dried in a convection drying oven at 50°C for 15 minutes.

[0377] After drying, the dried layer on the oak veneer panel was cooled to room temperature and subjected to UV irradiation using a Hg lamp with a lamp power of 50% (2 x 10 m / min, approximately 1200 mJ / cm 2 The dried layer was treated with a dosage of 200 g / cm2 to form a cross-linked layer. The cross-linked layer was sanded with P400 sandpaper, and the coating process was repeated again using the procedure described.

[0378] Water resistance was tested (1 hour water exposure) by placing a water column (diameter: about 2.5 cm, height: about 4.0 cm) on the surface of the cross-linked layer of the veneered oak board. This was done with the aid of a 50 mL penicillin bottle (diameter: about 2.5 cm, height: about 8 cm) half-filled with water. After 1 hour, the water column was removed and the appearance of the cross-linked layer portion of the veneered oak board exposed to water for 1 hour was analyzed by visual inspection immediately and also after standing at room temperature for 24 hours.

[0379] The water resistance (16 hours water exposure) was tested by placing a water column (diameter: about 2.5 cm, height: about 4.0 cm) on the surface of the crosslinked layer of the veneered oak board. This was done with the aid of a 50 ml penicillin bottle (diameter: 2.5 cm, height: 8 cm) half-filled with water. After 16 hours, the water column was removed and the appearance of the crosslinked layer portion of the veneered oak board exposed to water for 16 hours was analyzed by visual inspection immediately and also after standing at room temperature for 24 hours.

[0380] The appearance of the parts of the cross-linked layers of veneered oak boards exposed to water shall be graded as follows:

[0381] 1: Clearly visible marks; surface structure changes

[0382] 2: Clearly visible marks; surface structure is basically intact

[0383] 3: Slight change in gloss and color; no change in surface structure, but visible expansion

[0384] 4: Only noticeable changes in brightness and color at at least one viewing angle, no visible but palpable expansion

[0385] 5: No visible change at all possible viewing angles

[0386] The results are listed in Table 1.

[0387] Example 10

[0388] Preparation of veneered oak board coated with the coating composition of Example 6

[0389] A veneered oak panel coated with the coating composition of Example 6 was prepared as described in Example 9.

[0390] Polishability was determined as follows: After UV radiation treatment, the veneered oak boards were cooled to room temperature and the polishability of the coated veneered oak boards was analyzed by visual inspection and graded as follows:

[0391] 1: No polishing

[0392] 2: Very low polishability

[0393] 3: Low polishability

[0394] 4: Good polishability

[0395] 5: Very good polishability

[0396] The results are listed in Table 1.

[0397]

[0398]

[0399] Table 1. The higher the value of Examples 7 to 10 shown in the table, the better the properties.

[0400] a) DB density of PU = density of ethylenically unsaturated groups of polyurethane [milliequivalent ethylenically unsaturated groups / gPU]

[0401] b) DB(A1) / DB(PU)=equivalent ratio of ethylenically unsaturated groups of polyisocyanate (A1) / ethylenically unsaturated groups of components (B1), (B2), (B3) and (A1) and (C1)

[0402] c) Equivalent ratio of NCO groups of (A1) and (A2) / OH groups of (B1), (B2), (B3) and (B4)

[0403] d) COOH density of PU = COOH group and its salt group density of polyurethane

[0404] e) Water resistance of the cross-linked layer, 1h / 0h = Water resistance of the cross-linked layer after exposure to standing water for 1h, visual inspection immediately after removing the water exposure

[0405] f) Water resistance of the cross-linked layer, 1h / 24h = Water resistance of the cross-linked layer after exposure to standing water for 1h, visual inspection after 24h after the water exposure is removed

[0406] g) Water resistance of the cross-linked layer, 16h / 0h = Water resistance of the cross-linked layer after exposure to standing water for 16h, visual inspection immediately after removal of the water exposure

[0407] h) Water resistance of the cross-linked layer, 16h / 24h = Water resistance of the cross-linked layer after exposure to standing water for 16h, visual inspection after 24h after removal of water exposure

[0408] Table 1 shows that the wet layers formed on the black glass plate by the coating compositions of the present invention respectively comprising the waterborne ethylenically unsaturated polyurethane compositions PUD1b, PUD1c and PUD1d are transparent and thus exhibit high transparency. The wet layer of the coating composition comprising the waterborne ethylenically unsaturated polyurethane composition PUD1a is milky white immediately after being applied on the black glass plate. However, the wet layers of the comparative coating compositions respectively comprising the comparative waterborne ethylenically unsaturated polyurethane compositions cPUD1, cPUD 2 and cPUD3 are white immediately after being applied on the black glass plate.

[0409] Table 1 also shows that the crosslinked layers of the coating compositions of the present invention respectively comprising the waterborne ethylenically unsaturated polyurethane compositions PUD1a, PUD1b, PUD1c and PUD1d on the black glass plate are transparent and thus exhibit high transparency. However, the crosslinked layer of the comparative coating composition comprising the comparative waterborne ethylenically unsaturated polyurethane composition cPUD3 is turbid and exhibits poor transparency.

[0410] Table 1 also shows that the dried layers formed on the long glass plates by the coating compositions of the present invention respectively comprising the waterborne ethylenically unsaturated polyurethane compositions PUD1a, PUD1b, PUD1c and PUD1d are redispersible or soluble in water at ambient temperature within a certain period of time. However, the dried layers formed on the long glass plates by the comparative coating composition comprising the comparative waterborne ethylenically unsaturated polyurethane composition cPUD3 are not redispersible or soluble in water at ambient temperature within a certain period of time.

[0411] Table 1 also shows that the cross-linked layers formed on the veneered oak boards by the coating compositions of the present invention respectively comprising the waterborne ethylenically unsaturated polyurethane compositions PUD1a, PUD1b, PUD1c and PUD1d show high water resistance, while the cross-linked layers formed on the veneered oak boards by the comparative coating compositions respectively comprising the comparative waterborne ethylenically unsaturated polyurethane compositions cPUD1, cPUD2 and cPUD3 show much lower water resistance.

[0412] Table 1 also shows that the polishability of the veneered oak board coated with a crosslinked layer formed by the coating composition of the present invention comprising the waterborne ethylenically unsaturated polyurethane compositions PUD1a, PUD1b, PUD1c and PUD1d, respectively, is better than the polishability of the veneered oak board coated with a crosslinked layer formed by the comparative coating composition comprising the comparative waterborne ethylenically unsaturated polyurethane compositions cPUD1, cPUD2 and cPUD3, respectively.

[0413] Table 1 thus shows that the coating compositions of the invention comprising the aqueous ethylenically unsaturated polyurethane compositions PUD1a, PUD1b, PUD1c and PUD1d, respectively, exhibit an advantageous combination of the following properties: high transparency of the wet layer, good redispersibility or redissolubility of the dry layer and high water resistance and very good polishability of the crosslinked layer on wood-based substrates, as well as good to high transparency of the crosslinked layer.

[0414] Example 11

[0415] Preparation of aqueous polyurethane dispersion PUD1e containing polyurethane 1e

[0416] At 22°C, 39.81 g of 2,2-bis(hydroxymethyl)propionic acid, 144.04 g of polytetrahydrofuran (MW 1000 g / mol), 87.81 g of 2-hydroxyethyl acrylate, 0.8 g of TBK (polymerization inhibitor), 0.08 g 2,2,6,6-tetramethylpiperidin-1-oxyl (polymerization inhibitor), 0.56 g Kat315 and 200g of butanone are mixed. 507.75g of the polyisocyanate A1a of Example 1 is added, the temperature is raised to 80°C, and the reaction mixture is allowed to react until an NCO content of 0.65% by weight based on the weight of the reaction mixture is reached. The mixture is diluted with 370g of acetone, causing the temperature to drop below 80°C. 18.95g of a 50% by weight solution of N-aminoethyl-2-aminoethanesulfonic acid sodium salt in water is added to the mixture, and the reaction mixture is allowed to react for 10min. 95.36g of a 10% by weight solution of NaOH in water is added to the mixture, and the reaction mixture is allowed to react for 5min. 1150g of water is added to the reaction mixture under rapid stirring. The organic solvent is removed by distillation to obtain an aqueous composition PUD1e containing polyurethane 1e, which has a solid content of 36.3% by weight and the properties as shown in Table 2.

[0417]

[0418] Table 2.

[0419] a) DB density of PU = density of ethylenically unsaturated groups of polyurethane [milliequivalent ethylenically unsaturated groups / gPU]

[0420] b) DB(A1) / DB(PU)=equivalent ratio of ethylenically unsaturated groups of polyisocyanate (A1) / ethylenically unsaturated groups of components (B1), (B2), (B3) and (A1) and (C1)

[0421] c)Equivalent ratio of NCO groups of (A1) and (A2) / OH groups of (B1), (B2), (B3) and (B4)

[0422] d) COOH density of PU = COOH group and its salt group density of polyurethane

Claims

1. A composition comprising (i) at least one polyurethane (1) carrying ethylenically unsaturated groups and COOH groups, these COOH groups being at least partly in the form of their salt groups, which polyurethane (1) is obtainable by reaction of at least one polyol (B1) carrying at least one COOH group, at least one monool (B2) carrying at least one ethylenically unsaturated group, optionally at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups, at least one polyol (B4) which carries no ethylenically unsaturated groups and no COOH groups, at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group, optionally at least one polyisocyanate (A2) not carrying ethylenically unsaturated groups, and optionally at least one compound (C1) carrying at least one NH2 group and no OH groups, wherein the equivalent ratio of the ethylenically unsaturated groups of the polyisocyanate (A1) to the ethylenically unsaturated groups of the components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.20 / 1.00 to 0.95 / 1.00, and wherein the equivalent ratio of NCO groups of the polyisocyanates (A1) and (A2) / OH groups of the components (B1), (B2), (B3) and (B4) is in the range of 1.00 / 1.00 to 1.50 / 1.00, (ii) water, and (iii) optionally at least one compound (2) which carries at least one ethylenically unsaturated group and no COOH group.

2. The composition according to claim 1, wherein The equivalent ratio of ethylenically unsaturated groups of polyisocyanate (A1) / ethylenically unsaturated groups of components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.40 / 1.00 to 0.80 / 1.

00.

3. The composition according to claim 1, wherein The equivalent ratio of ethylenically unsaturated groups of polyisocyanate (A1) / ethylenically unsaturated groups of components (B1), (B2), (B3), (A1) and (C1) is in the range of 0.50 / 1.00 to 0.70 / 1.

00.

4. The composition according to any one of claims 1 to 3, wherein These ethylenically unsaturated groups are selected from the group consisting of acryloyl and methacryloyl groups.

5. The composition according to any one of claims 1 to 4, wherein The polyol (B4) not carrying ethylenically unsaturated groups and COOH groups is selected from the group consisting of polyester polyols not carrying ethylenically unsaturated groups and COOH groups, polycarbonate polyols not carrying ethylenically unsaturated groups and COOH groups, and polyether polyols not carrying ethylenically unsaturated groups and COOH groups.

6. The composition according to any one of claims 1 to 5, wherein The polyisocyanate (A1) has 1 The ethylenically unsaturated group density is in the range of 0.10 to 10.00 milliequivalents of ethylenically unsaturated groups / g (A1) as determined by H-NMR.

7. The composition according to any one of claims 1 to 6, wherein The polyisocyanate (A1) also contains at least one allophanate group.

8. The composition according to any one of claims 1 to 7, wherein The polyurethane (1) has a weight average molecular weight Mw in the range of 5000 g / mol to 30000 g / mol.

9. The composition according to any one of claims 1 to 8, wherein The salt of the COOH group of the polyurethane (1) is an alkali metal salt.

10. The composition according to any one of claims 1 to 9, wherein The polyurethane (1) has an ethylenically unsaturated group density of at least 1.00 milliequivalent ethylenically unsaturated groups / g of polyurethane (1).

11. The composition according to any one of claims 1 to 10, wherein The composition is a dispersion having an average particle size in the range of 5 to 150 nm.

12. The composition according to any one of claims 1 to 11, wherein The composition comprises polyurethane (1) in the range of 10 to 70% by weight based on the weight of the composition.

13. The composition according to any one of claims 1 to 12, wherein The polyurethane (1) can be obtained by the following reaction: 1 to 20% by weight of at least one polyol (B1) carrying at least one COOH group, 5 to 50% by weight of at least one monool (B2) carrying at least one ethylenically unsaturated group, 0 to 30% by weight of at least one polyol (B3) carrying at least one ethylenically unsaturated group and no COOH groups, 5 to 60% by weight of at least one polyol (B4) carrying no ethylenically unsaturated groups and no COOH groups, 20 to 85% by weight of at least one polyisocyanate (A1) carrying at least one ethylenically unsaturated group, 0 to 40% by weight of at least one polyisocyanate (A2) carrying no ethylenically unsaturated groups, and 0 to 15% by weight of at least one compound (C1) carrying at least one NH2 group and no OH groups Based on the sum of the weights of (B1), (B2), (B3), (B4), (A1), (A2) and (C1).

14. An aqueous coating composition comprising the composition according to any one of claims 1 to 13, at least one additive, optionally at least one initiator and optionally at least one polymer (5) different from the polyurethane (1), wherein the coating composition comprises the polyurethane (1) in the range of 10 to 70% by weight, based on the weight of the coating composition.

15. A layer formed from the aqueous coating composition according to claim 14.

16. A substrate coated with a layer as claimed in claim 15.

17. The substrate according to claim 16, wherein The substrate is a wood substrate or an engineered wood substrate including a veneer.

18. Use of the coating composition according to any one of claims 1 to 13 as a primer composition.