Novel polymers for battery applications
By designing polymers with specific structures, the problems of flammability and instability of traditional electrolytes are solved, the electrochemical and mechanical properties of the battery are improved, and the high safety and long life of the battery are achieved.
Patent Information
- Application Number
- CN202380027969.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-17
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional electrolytes in existing batteries are flammable and unstable. Polymer electrolytes have problems with insufficient adhesion and mechanical properties in high-capacity electrode applications, making it difficult to meet the high safety standards and long-life needs of batteries.
A polymer with a specific structure was designed, and prepared by open ring polymerization and open ring copolymerization techniques to form a polymer with excellent electrochemical and mechanical properties for the preparation of electrolytes and cathode materials, improving the performance of the battery.
The thermal stability and elastic recovery performance of the electrolyte are achieved, the ionic conductivity and oxidation stability of the battery are improved, and they are suitable for high-voltage cathodes and extend the battery life.
Smart Images

Figure BDA0005044493470000081 
Figure BDA0005044493470000091 
Figure BDA0005044493470000101
Abstract
Description
Technical Field
[0001] The present invention relates to polymers for batteries and battery components. The present invention also relates to batteries and battery components (such as electrolytes and cathodes) containing the polymers, and methods for preparing the polymers and battery components. Background Art
[0002] The sale of new petrol and diesel cars in the UK will be phased out by 2030. [1] This is important for improving the sustainability of transportation by reducing greenhouse gas emissions and dependence on fossil fuels. However, significant technological advances are needed to increase the appeal of electric vehicles; a similar experience to internal combustion engine cars is needed. This means; fast charging times; long battery life; high safety standards; and high battery capacity. These needs can be addressed by developing better batteries.
[0003] Batteries consist of electrolytes, which separate the two electrodes: the anode and the cathode. Their role is to store and release lithium. The electrolyte facilitates the transport of ions between the electrodes. Traditionally, electrolytes are flammable liquids; these are often unstable and present safety issues when developing high-capacity electrodes, such as lithium metal anodes. [2] Solid-state electrolytes are an important area of battery research. [3] They can be broadly classified as ceramics or polymers. Sulfide and oxide materials have been the focus of ceramic research, such as Li 9.6 P3S 12 and Li7La3Zr2O 12 . [4] They typically have excellent conductivity and can avoid the formation of dendrites (uneven deposition of lithium on the anode during charging, which can lead to short circuits and explosions). However, they can face issues with flexibility, processability, and stability of the electrode-electrolyte interface. [5] Polymer electrolytes have largely succeeded where inorganic electrolytes have failed. Solid polymer electrolytes (SPEs) are more resistant to changes in electrode volume, have improved processability, and are often flexible. [3a]
[0004] Polymers can play another key role in batteries: as a binder material. PVDF is a fluorinated polymer that is widely used in batteries to adhere cathode particles. However, PVDF is not adhesive and flexible enough to work with high-capacity cathodes: cathodes expand and contract significantly during charge and discharge, resulting in loss of contact with the binder and degradation of electrochemical performance. Therefore, people are looking for new polymer binders that are electrochemically stable, flexible, and sticky. [6]
[0005] The first polymer electrolyte, composed of polyethylene oxide (PEO) and alkali metal salts, was reported by Fenton et al. in 1973. [7] PEO has a flexible main chain, and ether oxygen is a good donor, so it can make Li + Solvation produces an ion-conducting polymer salt. Ion transport occurs only at T g The amorphous region above is formed because it is assisted by the segmental motion of the polymer chains. [3a] PEO-based electrolytes have been extensively studied and optimized through methods such as copolymerization, cross-linking, and blending. [8] However, many still have poor room temperature ionic conductivity (<10 -4 S cm -1 , in comparison, conventional liquid electrolytes are about 10 -2 S cm -1 ) and insufficient electrochemical stability (<4 V). [9]
[0006] Despite progress in this area, there remains a need for structurally well-defined polymer materials with electrochemical and mechanical properties that make them suitable for use in batteries and battery components.
[0007] The present invention has been designed in consideration of the above. Summary of the invention
[0008] According to a first aspect of the present invention, there is provided a polymer having a structure according to formula I:
[0009] AB-A'
[0010] (I)
[0011] in
[0012] A is a polycarbonate block;
[0013] A' is absent or is a polycarbonate block A; and
[0014] B is different from A and is a block composed of poly(ester-co-carbonate) or polycarbonate.
[0015] According to a second aspect of the present invention, there is provided a method for preparing a polymer, the method comprising the following steps:
[0016] (a) performing a ring-opening polymerization of (i) a cyclic carbonate or (ii) a mixture of a cyclic carbonate and a cyclic ester to form a polymer block B, wherein the polymer block B is a polycarbonate or a poly(ester-co-carbonate); and
[0017] (b) Growing polymer block A on one or both ends of polymer block B by ring-opening copolymerization of: (i) epoxide or oxetane and (ii) carbon dioxide.
[0018] According to a third aspect of the present invention, there is provided a polymer obtained, directly obtained or obtainable by the method of the second aspect.
[0019] According to a fourth aspect of the present invention, there is provided an electrolyte comprising a mixture of the polymer of the first or third aspect and a metal salt.
[0020] According to a fifth aspect of the present invention, there is provided a method for preparing an electrolyte, the method comprising the following steps:
[0021] (i) preparing a polymer according to the method of the second aspect; and
[0022] (ii) Mixing the polymer with the metal salt.
[0023] According to a sixth aspect of the present invention, there is provided a cathode for a battery, the cathode comprising the polymer of the first or third aspect and / or the electrolyte of the fourth aspect.
[0024] According to a seventh aspect of the present invention, there is provided a battery comprising the polymer of the first or third aspect, the electrolyte of the fourth aspect and / or the cathode of the sixth aspect.
[0025] According to an eighth aspect of the present invention, there is provided use of the polymer of the first or third aspect in manufacturing a battery or a battery component. DETAILED DESCRIPTION
[0026] definition
[0027] The term "(m-nC)" or "(m-nC) group" used alone or as a prefix refers to any group having from m to n carbon atoms.
[0028] The term "alkyl" as used herein refers to a straight or branched chain alkyl moiety typically having 1, 2, 3, 4, 5 or 6 carbon atoms. The term includes reference to groups such as methyl, ethyl, propyl (n-propyl or isopropyl), butyl (n-butyl, sec-butyl or tert-butyl), pentyl, hexyl, etc. Most suitably, the alkyl group may have 1, 2, 3 or 4 carbon atoms.
[0029] As used herein, the term "alkylene" refers to the divalent equivalent of an alkyl group as described above.
[0030] As used herein, the term "alkenyl" refers to a straight or branched alkenyl moiety typically having 1, 2, 3, 4, 5, or 6 carbon atoms. The term includes reference to alkenyl moieties containing 1, 2, or 3 carbon-carbon double bonds (C=C). The term includes reference to groups such as ethenyl, propenyl (allyl), butenyl, pentenyl, and hexenyl, and cis- and trans-isomers thereof.
[0031] As used herein, the term "alkynyl" refers to a straight or branched chain alkynyl moiety typically having 1, 2, 3, 4, 5, or 6 carbon atoms. The term includes reference to alkynyl moieties containing 1, 2, or 3 carbon-carbon triple bonds (C≡C). The term includes reference to groups such as ethynyl, propynyl, butynyl, pentynyl, and hexynyl.
[0032] As used herein, the term "alkoxy" refers to -O-alkyl, wherein the alkyl is straight or branched and contains 1, 2, 3, 4, 5 or 6 carbon atoms. In one class of embodiments, the alkoxy has 1, 2, 3 or 4 carbon atoms. The term includes reference to groups such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, tert-butoxy, pentoxy, hexoxy, and the like.
[0033] As used herein, the term "aryl" or "aromatic" refers to an aromatic ring system containing 6, 7, 8, 9 or 10 ring carbon atoms. Aryl is typically phenyl, but may also be a polycyclic ring system having two or more rings, at least one of which is aromatic. The term includes reference to groups such as phenyl, naphthyl, and the like.
[0034] The term "aryl-(m-nC)alkyl" refers to an aryl group covalently linked to an (m-nC)alkylene group, both of which are described herein. Examples of aryl-(m-nC)alkyl groups include benzyl, phenethyl, and the like.
[0035] The term "heteroaryl" or "heteroaromatic" refers to an aromatic monocyclic, bicyclic or polycyclic ring containing one or more (e.g., 1-4, particularly 1, 2 or 3) heteroatoms selected from nitrogen, oxygen or sulfur. Examples of heteroaryl are monocyclic and bicyclic groups containing 5-12 ring members, more typically 5-10 ring members. Heteroaryl can be, for example, a 5- or 6-membered monocyclic ring or a 9- or 10-membered bicyclic ring, such as a bicyclic structure formed by a fused five- and six-membered ring or two fused six-membered rings. Each ring can contain up to about 4 heteroatoms, typically selected from nitrogen, sulfur and oxygen. Typically, the heteroaryl ring will contain up to 3 heteroatoms, more typically up to 2, such as a single heteroatom.
[0036] The term "heteroaryl-(m-nC)alkyl" refers to a heteroaryl group covalently linked to a (m-nC)alkylene group, both of which are described herein.
[0037] The term "carbocyclyl", "carbocyclic" or "carbocycle" refers to a non-aromatic saturated or partially saturated monocyclic, or fused, bridged or spirocyclic bicyclic carbocyclic ring system. Monocyclic carbocyclic rings contain about 3 to 12 (suitably 3 to 7) ring atoms. Bicyclic carbocyclic rings contain 7 to 17 carbon atoms in the ring, suitably 7 to 12 carbon atoms in the ring. Bicyclic carbocyclic rings can be fused, spiro or bridged ring systems.
[0038] The term "heterocyclyl", "heterocyclic" or "heterocycle" refers to a non-aromatic saturated or partially saturated monocyclic, or fused, bridged or spiro bicyclic heterocyclic ring system. The monocyclic heterocyclic ring contains about 3 to 12 (suitably 3 to 7) ring atoms, having 1 to 5 (suitably 1, 2 or 3) heteroatoms selected from nitrogen, oxygen or sulfur in the ring. The bicyclic heterocyclic ring contains 7 to 17 atoms in the ring, suitably 7 to 12 atoms. The bicyclic heterocyclic ring can be a fused, spiro or bridged ring system.
[0039] The term "halogen" or "halo" as used herein refers to F, Cl, Br or I. Specifically, the halogen may be F or Cl, with Cl being more commonly used.
[0040] The term "haloalkyl" as used herein refers to an alkyl group in which one or more hydrogen atoms have been replaced by a halogen (e.g., fluorine) atom. Typically, a haloalkyl group is a fluoroalkyl group. Examples of haloalkyl groups include -CH2F, -CHF2, and -CF3.
[0041] The term "substituted" as used herein with reference to a moiety means one or more, in particular up to 5. Preferably, the term "substituted" as used herein with reference to a moiety means that 1, 2 or 3 hydrogen atoms in the moiety are replaced independently of each other by the corresponding number of said substituents. Even more preferably, the term "substituted" as used herein with reference to a moiety means that 1 or 2 hydrogen atoms in the moiety are replaced independently of each other by the corresponding number of said substituents. The term "optionally substituted" as used herein means substituted or unsubstituted.
[0042] Of course, it is to be understood that substituents are only placed where they are chemically possible, and one skilled in the art will have no difficulty determining (either experimentally or theoretically) whether a particular substitution is possible.
[0043] Throughout the description and claims of this specification, when subject matter is described using the term "comprise," the same subject matter described using the term "consisting of" or "consisting essentially of" is also considered.
[0044] Throughout the description and claims of this specification, the singular encompasses the plural unless the context otherwise requires. In particular, where the indefinite article is used, the specification is to be understood as contemplating plurality as well as singularity unless the context otherwise requires.
[0045] Features, integers, characteristics, compounds, chemical moieties or groups described in conjunction with a particular aspect, embodiment or example of the invention should be understood to be applicable to any other aspect, embodiment or example described herein, unless incompatible therewith. All features disclosed in this specification (including any attached claims, abstract and drawings) and / or all steps of any method or process so disclosed may be combined in any combination, except for combinations in which at least some of such features and / or steps are mutually exclusive. The invention is not limited to the details of any foregoing embodiments. The invention extends to any novel one or any novel combination of the features disclosed in this specification (including any attached claims, abstract and drawings), or any novel one or any novel combination of the steps of any method or process so disclosed.
[0046] Unless otherwise indicated, when the amount or concentration of a particular component of a given product is specified as a weight percentage (wt% or %w / w), the weight percentage refers to the weight percentage of the component relative to the total weight of the entire product. It will be understood by those skilled in the art that the sum of the weight percentages of all components of the product will total 100 weight %. However, in the case where all components are not listed (e.g., where a product is referred to as "comprising" one or more particular components), the weight percentage balance may optionally be composed of unspecified ingredients to reach 100 weight %.
[0047] polymer
[0048] In a first aspect, there is provided a polymer having a structure according to Formula I:
[0049] AB-A'
[0050] (I)
[0051] in
[0052] A is a polycarbonate block;
[0053] A' is absent or is a polycarbonate block A; and
[0054] B is different from A and is a block composed of poly(ester cocarbonate) or polycarbonate.
[0055] Through detailed studies, the inventors have designed new polymer materials with electrochemical and mechanical properties that make them suitable for batteries and battery components (such as electrolytes and cathodes). The polymers can be directly and flexibly prepared using environmentally friendly raw materials through ring-opening polymerization (ROP) and ring-opening copolymerization (ROCOP) techniques, which provide a high degree of control over the structure of the polymer, allowing the properties of the polymer to be adjusted according to specific applications.
[0056] It is to be understood that Formula I includes diblock copolymers (ie, when A' is absent) and triblock copolymers (ie, when A' is a polycarbonate block A).
[0057] In an embodiment, A' is absent and the polymer is a diblock copolymer.
[0058] In an embodiment, A' is a polycarbonate block A and the polymer is a triblock copolymer.
[0059] The molecular weight of the polymer (M n ) can be 10-200 kg mol -1 Suitably, the molecular weight (M) of the polymer n ) can be 15-100 kg mol -1 More preferably, the molecular weight (M n ) can be 20-70 kg mol -1 More preferably, the molecular weight (M n ) is 30-55 kg mol -1 The molecular weight of the polymer (M n ) can be obtained by 1 Determined by H NMR integration.
[0060] The polymer may contain 10-70 wt% of block A. The wt% of block A described herein refers to the total amount of such blocks present in the polymer. Thus, when A' is a polycarbonate block A, the wt% described herein refers to the total amount of both blocks A (rather than the amount of each block A). Suitably, the polymer contains 16-65 wt% of block A. More suitably, the polymer contains 20-45 wt% of block A. Most suitably, the polymer contains 30-40 wt% of block A. The wt% of the blocks in the polymer can be determined by 1 Determined by H NMR integration.
[0061] In an embodiment, the polymer is a diblock copolymer having a molecular weight of 20-70 kg mol -1 The molecular weight (M n ), comprising 20-60 wt% of block A. Suitably, the polymer is a diblock copolymer having 20-60 kg mol -1The molecular weight (M n ), comprising 20-45 wt% of block A. More suitably, the polymer is a diblock copolymer having 35-55 kg mol -1 The molecular weight (M n ), containing 20-35 wt.% of block A.
[0062] In an embodiment, the polymer is a triblock copolymer having a molecular weight of 45-70 kg mol -1 The molecular weight (M n ), comprising 25-65 wt% of block A. Suitably, the polymer is a triblock copolymer having 47-68 kg mol -1 The molecular weight (M n ), comprising 30-55 wt% of block A. Suitably, the polymer is a triblock copolymer having 45-55 kg mol -1 The molecular weight (M n ), containing 30-40 wt.% of block A.
[0063] The copolymers of the present invention are suitably block phase separated (rather than block phase miscible). Phase separation of the blocks in the copolymer can be achieved by the presence of two different glass transition temperatures (T g ) are used to represent; one for block A and one for block B.
[0064] Block A may have a glass transition temperature (T g Suitably, block A has a glass transition temperature (T g More suitably, block A has a glass transition temperature (T g Most suitably, block A has a glass transition temperature (T g ).
[0065] Block B may have a glass transition temperature (T g Suitably, block B has a glass transition temperature (T g More preferably, block B has a glass transition temperature (T g Most suitably, block B has a glass transition temperature (T g ).
[0066] In an embodiment, block A has a glass transition temperature (T g ), block B has a glass transition temperature (T) of -55 to -25°C g). Suitably, the polymer has a mass fraction of 20-70 kg mol -1 The molecular weight (M n ), comprising 16-65 wt% of block A. More suitably, the (1) polymer is a diblock copolymer having 20-70 kg mol -1 The molecular weight (M n ), containing 20-60 wt. % of block A, or (2) the polymer is a triblock copolymer having 45-70 kg mol -1 The molecular weight (M n ), containing 25-65 wt.% of block A.
[0067] A portion of the A and / or B block repeating units may independently contain side chain neutral functional groups FG N and / or side chain anionic functional groups FG A Such functional groups can be used to tune the properties of the polymer (e.g., adhesion) depending on the desired battery application. For example, functional groups capable of participating in hydrogen bonding can improve the ability of the polymer to withstand the volume changes that occur during (de)lithiation. Exemplary side chain neutral functional groups FG N Including -P(O)(OH)2, -COOH, -OH, -SO3H, -NH2, -C(O)NH2, -F, -CF3 and -CN. Exemplary side chain anionic functional groups FG A Included - PO3 2- 、-PO2(OH) - 、-COO - 、-SO3 - 、-SO2N - SO2CF3, -N - SO2CF3, -(CF2)2O(CF2)2SO3 - , -BO4 - 、-(C6H4)4B - 、-(C6F4)4B - and -CHFCF2SO3 - The skilled person will appreciate the chemical techniques by which such functional groups can be introduced into some or all of the repeating units forming blocks A and / or B.
[0068] In embodiments, a portion of the A and / or B block repeat units comprise a neutral functional group -P(O)(OH)2. Inclusion of phosphonate groups in the polymer that can participate in hydrogen bonding can improve the ability of the polymer to withstand the volume changes that occur during (de)lithiation.
[0069] Block A may have a structure according to formula Ai:
[0070]
[0071] in
[0072] represents the point of attachment of an oxygen atom which is part of B;
[0073] L is a linking group that separates the two oxygen atoms it connects from 2 to 3 carbon atoms apart; and
[0074] X 1 It is a terminal group.
[0075] One skilled in the art will appreciate that the use of square brackets denotes a repeating unit.
[0076] Repeating units of the type shown in Formula Ai can be prepared by ROCOP of CO2 with an epoxide (e.g., where L separates the two oxygen atoms by a distance of 2 oxygen atoms) or an oxetane (e.g., where L separates the two oxygen atoms by a distance of 3 oxygen atoms). It should be understood that various epoxides and oxetanes can be used to form the repeating units in Formula AI, some of which are described herein in conjunction with the second aspect of the invention.
[0077] L is a linking group that suitably separates the two oxygen atoms to which it is connected by a distance of 2 carbon atoms. The two carbon atoms may form part of a ring. The ring may be a 5 to 7 membered carbocyclic or heterocyclic ring. Most suitably, the ring is a 6 membered carbocyclic ring.
[0078] It should be understood that the terminal group X 1 Can take various forms. Typically, X 1 It's H.
[0079] Block A may have a structure according to Formula A-ii:
[0080]
[0081] in
[0082] represents the point of attachment of an oxygen atom which is part of B;
[0083] X 1 is a terminal group; and
[0084] Each R 1 independently absent or a group -X-(R 2 ) v ,in
[0085] Each R 2 Independently the side chain neutral functional group FG as described above N or side chain anionic functional groups
[0086] FG A ;
[0087] Each v is independently 0 or 1; and
[0088] Each X is (when v is 1) R 2 A linking group to the cyclohexyl ring, or (when v is 0) a terminal (monovalent) group.
[0089] Repeating units of the type shown in formula A-ii can be prepared by ROCOP of CO2 with cyclohexene oxide. Since various substituted epoxides of this type are readily available or can be directly prepared by known chemical methods, it is understood that R 1 When present it can take many forms.
[0090] When v is 0, X is a terminal group. For example, X can be a vinyl group present on the cyclohexyl ring during polymerization. Alternatively, X can be a linking group that connects the cyclohexyl ring to one of the above functional groups (when v is 1). Continuing with the example of the vinyl groups present on the cyclohexyl ring during polymerization, after polymerization, some of these vinyl groups can be attached to the cyclohexyl ring containing R. 2 The group-XR 2 , where X is a linking group -CH2CH2SCH2CH2-, R 2 It's FG N -P(O)(OH)2. In this sense, it is understood that block A may include a mixture of (divalent) linking groups and (monovalent) terminal groups X. Furthermore, it should be understood that the specific groups mentioned in this paragraph are for illustrative purposes only, and one of ordinary skill in the art will recognize that X can take a variety of forms. Typically, X will consist of less than 80 atoms, more suitably less than 40 atoms, and even more suitably less than 20 atoms.
[0091] In an embodiment, R 1 Does not exist or is
[0092]
[0093] The repeating units of block B are different from the repeating units of block A and can take a variety of forms. For example, block B can be composed of repeating units, each of which independently has a structure according to formula Bi:
[0094]
[0095] in
[0096] W is O or CH2; and
[0097] V is a group that separates O and W by 3-5 carbon atoms,
[0098] Provided that in at least some of the repeating units in block B, W is O.
[0099] Suitably, V is a group which separates O from W by 3-4 carbon atoms.
[0100] Block B may be polycarbonate. It will be appreciated that the repeating units forming block B are structurally different from those repeating units forming block A of polycarbonate.
[0101] Alternatively, block B is poly(ester-co-carbonate). Suitably, block B comprises 60-95 mol % of ester repeating units and 5-40 mol % of carbonate repeating units. More suitably, block B comprises 65-90 mol % of ester repeating units and 10-35 mol % of carbonate repeating units. Even more suitably, block B comprises 70-90 mol % of ester repeating units and 10-30 mol % of carbonate repeating units. Most suitably, block B comprises 75-85 mol % of ester repeating units and 15-25 mol % of carbonate repeating units.
[0102] Suitably, block B is poly(caprolactone-co-carbonate) or poly(ester-co-trimethylene carbonate). More suitably, block B is poly(caprolactone-co-trimethylene carbonate). It will be appreciated that the ester and carbonate repeat units may be present in the copolymer in any order (e.g., random or alternating).
[0103] In an embodiment, B is poly(caprolactone-r-trimethylene carbonate). Suitably, block B comprises 70-90 mol% of caprolactone repeating units and 10-30 mol% of trimethylene carbonate repeating units.
[0104] When the polymer is a diblock copolymer, block B may terminate at any suitable end group. For the diblock polymers of the present invention, the growth of block B may start from the hydroxyl group of a monohydroxy chain transfer agent (e.g., methylbenzyl alcohol). In this case, the remaining portion of the chain transfer agent (e.g., all of the portion except the hydrogen atom that initiates the hydroxyl group) may form the end group of block B. The end group may have the formula -OR 3 , where R 3 It is an organic group containing less than 50 atoms, more suitably less than 25 atoms.
[0105] When the polymer is a triblock copolymer, the growth of block B can be initiated by the hydroxyl groups of a dihydroxy chain transfer agent (e.g., benzyl alcohol). In this case, block B can include the residual portion of the chain transfer agent (e.g., all but the hydrogen atom of the starting hydroxyl group), which can be located about 40-60% along its length. The residual portion can have the formula -OR4 -O-, where R 4 It is an organic group containing less than 50 atoms, more suitably less than 25 atoms.
[0106] Block A may be amorphous. Alternatively, or in addition, the polymer itself may be amorphous. Amorphous polymers have no observable melting point when analyzed by differential scanning calorimetry.
[0107] In a second aspect, the present invention provides a method for preparing a polymer, the method comprising the steps of:
[0108] (a) performing a ring-opening polymerization of (i) a cyclic carbonate or (ii) a mixture of a cyclic carbonate and a cyclic ester to form a polymer block B, wherein the polymer block B is a polycarbonate or a poly(ester-co-carbonate); and
[0109] (b) Growth of polymer block A at one or both ends of polymer block B by ring-opening copolymerization of: (i) an epoxide or an oxetane and (ii) carbon dioxide.
[0110] The polymer of the first aspect can be directly prepared by sequential ROP and ROCOP reactions. From an environmental point of view, the use of CO2 as a reagent in ROCOP is particularly beneficial.
[0111] The ROP in step (a) can be initiated using a monofunctional initiator, such as a monohydroxy chain transfer agent (e.g., methylbenzyl alcohol). When a monofunctional initiator is used in step (a), step (b) includes growing polymer block A at one end of polymer block B. Thus, the resulting polymer is a diblock copolymer AB.
[0112] The ROP in step (a) can be initiated using a bifunctional initiator, such as a dihydroxy chain transfer agent (e.g., benzyl alcohol). When a bifunctional initiator is used in step (a), step (b) includes growing polymer block A at both ends of polymer block B. Therefore, the resulting polymer is a triblock copolymer ABA.
[0113] The polymer block B prepared in step (a) may be any of those polymers listed above for the block B of the polymer of the first aspect, and / or have those properties (e.g., glass transition temperature (T g Additionally or alternatively, the polycarbonate grown in step (b) may be any of those polycarbonates listed above for block A of the polymer of the first aspect, and / or have those properties (e.g., glass transition temperature (T gAdditionally or alternatively, the di- / tri-block copolymer prepared by the method may be any of those polymers listed above for the polymer of the first aspect, and / or have those properties (e.g., the weight % and / or molecular weight (M) of block A). n )).
[0114] The method can be carried out in the presence of a suitable catalyst. Catalysts capable of catalyzing the ROP of cyclic carbonates and / or cyclic esters and the ROCOP of epoxides / oxetanes with CO2 are known in the art. Suitably, the catalyst is an organozinc catalyst. Non-limiting examples of catalysts capable of carrying out steps (a) and (b) are:
[0115]
[0116] If necessary, the method can be carried out in a one-pot process. In other words, steps (a) and (b) can be carried out sequentially without any intermediate isolation steps. For example, all reagents required to carry out steps (a) and (b), except CO2, can be introduced into the reaction vessel to initiate step (a). When desired, step (a) can be terminated and step (b) started by introducing CO2 into the reaction vessel.
[0117] The method may further comprise the following additional steps:
[0118] (c) by introducing the side chain neutral functional group FG described above in relation to the first aspect N and / or side chain anionic functional groups FG A to modify a portion of the repeating units of block A and / or block B. Suitably, step (c) comprises modifying a portion of the repeating units of block A.
[0119] As described above with respect to the first aspect, the epoxide / oxetane used in step (b) may take a variety of forms. Suitable oxetanes include 1,3-propylene oxide, 2,2-dimethyloxetane and 3,3-dimethyloxetane. Suitable epoxides include 2,3-dimethyloxirane, capped epoxides, glycidyl ethers and cyclic epoxides.
[0120] The capped epoxide may have the following structure:
[0121]
[0122] Where R x is selected from hydrogen, (1-4C)alkyl, (2-4C)alkenyl, (1-4C)haloalkyl, aryl, aryl-(1-2C)alkyl, -(OCH2CH2) r OMe and -(CH2) sC(O)OR x1 , where r is 1-10, s is 0-6, R x1 is (1-5C)alkyl or aryl-(1-2C)alkyl. x Specific non-limiting examples include hydrogen, methyl, ethyl, phenyl, -CH2Cl, -CH=CH2, -CH2C(O)OtBu, -C(O)OBn, -(CH2) 1-4 C(O)OMe and -(OCH2CH2) 1-6 OMe.
[0123] Glycidyl ethers can have the following structures:
[0124]
[0125] Where R y is selected from hydrogen, (1-4C)alkyl, (2-4C)alkenyl, (2-4C)alkynyl and –(CH2) t R y1 , where t is 0-4, R y1 is an aryl, heteroaryl, carbocyclic or heterocyclic group, wherein R y Any ring in is optionally replaced by one or more groups R y2 Replacement, R y Any (1-4C)alkyl in R y3 Replace; each R y2 are independently selected from (1-3C)alkyl and nitro, R y3 is (1-4C) alkoxy or aryloxy. y Specific non-limiting examples of include hydrogen, (1-4C)alkyl, -CH2OCH2CH3, -CH2O-CH(CH3)2, -CH2-O-C6H5 and:
[0126]
[0127] Cyclic epoxides can have the following structures:
[0128]
[0129] wherein D is a 5- to 7-membered carbocyclic or heterocyclic ring, which is optionally fused or spiro-linked to 1 or 2 rings E, wherein each E is independently selected from carbocyclyl, heterocyclyl, aryl and heteroaryl, and wherein any one of the rings D and E is optionally substituted by one or more substituents R Z Replace, each R Z are independently selected from (1-4C)alkyl, (2-4C)alkenyl, -(CH2) 1-2 Si(OR z1 )3, -(CH2) 1-2OSi(R z1 )3 and group -L z1 -L z2 -R z2 , where R z1 is (1-2C)alkyl, L z1 does not exist or is (1-3C) alkylene, L z2 does not exist, is -O- or -C(O)O- and R z2 is hydrogen, (1-6C)alkyl, (1-5C)haloalkyl, heterocyclyl, aryl or aryl-(1-2C)alkyl, wherein R z2 Any ring in is optionally substituted with (1-3C)alkyl or oxo. Specific non-limiting examples of cyclic epoxides include:
[0130]
[0131] Suitably, the epoxide or oxetane is an epoxide. More suitably, the epoxide is a cyclic epoxide. More suitably, the epoxide is a 6-membered cyclic epoxide. Most suitably, the epoxide is selected from:
[0132]
[0133] Cyclic carbonates and cyclic esters that can be used for the process step (a) can take various forms. For example, the cyclic carbonate can be a 6 to 10-membered cyclic carbonate, and the cyclic ester can be a 6 to 10-membered cyclic ester. Suitably, the cyclic carbonate can be a 6 to 8-membered cyclic carbonate, and the cyclic ester can be a 6 to 8-membered cyclic ester. Most suitably, the cyclic carbonate is trimethylene carbonate, and the cyclic ester is ε-caprolactone.
[0134] In an embodiment, step (a) comprises performing a ring-opening polymerization of a cyclic carbonate to form a polymer block B which is a polycarbonate.
[0135] In embodiments, step (a) comprises carrying out the ring-opening polymerization of the mixture of cyclic carbonate and cyclic ester to form the polymer block B of poly (ester-to-carbonate). Suitably, the mixture comprises 60-95mol% of cyclic ester and 5-40mol% of cyclic carbonate. More suitably, the mixture comprises 65-90mol% of cyclic ester and 10-35mol% of cyclic carbonate. Even more suitably, the mixture comprises 70-90mol% of cyclic ester and 1-30mol% of cyclic carbonate. Most suitably, the mixture comprises 75-85mol% of cyclic ester and 15-25mol% of cyclic carbonate.
[0136] Those skilled in the art will be able to select appropriate conditions (e.g., solvents, temperature, etc.) for carrying out the method. A non-limiting example of a suitable solvent for carrying out steps (a) and (b) is toluene. The method can be carried out at a temperature of 50-150° C. (e.g., 90-110° C.).
[0137] Suitably, step (b) is carried out at a CO2 pressure of <2 MPa. More suitably, step (b) is carried out at a CO2 pressure of <1 MPa. Even more suitably, step (b) is carried out at a CO2 pressure of <0.5 MPa. Most suitably, step (b) is carried out at a CO2 pressure of 0.05–2 MPa.
[0138] In a third aspect, there is provided a polymer obtained, directly obtained or obtainable by the method of the second aspect.
[0139] Battery Application
[0140] In a fourth aspect, the present invention provides an electrolyte comprising a mixture of the polymer of the first or third aspect and a metal salt.
[0141] The inventors surprisingly found that the polymers described herein are particularly suitable for use in electrolytes, such as electrolytes for batteries. When mixed with metal salts, the polymers exhibit good thermal stability and elastic recovery properties. The electrolytes also exhibit good ionic conductivity at ambient and elevated temperatures, as well as oxidation stability above 5V, indicating compatibility with high voltage cathodes.
[0142] The metal salt may be a Na, Li or K salt. Suitably, the metal salt is a Li salt.
[0143] The metal salt may have the formula M + X - , where M + Selected from Na + , Li + and K + , X - Selected from BF4 - 、ClO4 - , bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, bis(oxalate)borate, perfluoroalkylsulfonate (e.g. CF3SO3 - ), polyfluoroalkyl sulfonates, PF6, AsF6 - , cyano(trifluoromethanesulfonyl)imide, bis(pentafluoroethanesulfonyl)imide, B(CN)4 - , 4,5-dinitrile-1,2,3-triazole, perylene diimide, 4,5-dicyano-2-(trifluoromethyl)imidazolium, and combinations of two or more thereof. Suitably, M + It's Li+ and / or X - is bis(trifluoromethanesulfonyl)imide. Most suitably, M + It's Li + And X - It is bis(trifluoromethanesulfonyl)imide.
[0144] The electrolyte may comprise 0.1-80 wt % of the metal salt. Suitably, the electrolyte comprises 15-50 wt % of the metal salt. More suitably, the electrolyte comprises 15-25 wt % of the metal salt. Suitably, the metal salt is lithium bis(trifluoromethanesulfonyl)imide.
[0145] In a fifth aspect, the present invention provides a method for preparing an electrolyte, the method comprising the steps of:
[0146] (i) providing a polymer according to the first or third aspect, or preparing a polymer according to the method of the second aspect; and
[0147] (ii) Mixing the polymer with the metal salt.
[0148] Step (ii) may comprise mixing the polymer and the metal salt in a solvent. Any suitable solvent may be used. A non-limiting example of a suitable solvent is anhydrous THF.
[0149] The method may further comprise the step (iii) of drying the mixture obtained in step (ii). Suitably, the mixture is dried at a temperature of 50-80°C, optionally under vacuum.
[0150] In a sixth aspect, the present invention provides a cathode for a battery, the cathode comprising the polymer of the first or third aspect and / or the electrolyte of the fourth aspect. The cathode is suitable for use in a Li-ion battery.
[0151] The cathode may be a composite cathode. The composite cathode may include a cathode material (e.g., LiNi 0.8 Mn 0.1 Co 0.1 O2, referred to as NMC811), a conductive additive (e.g., carbon), and either or both of the polymer of the first aspect and the electrolyte of the fourth aspect. The cathode material, the conductive additive, and the polymer and / or the electrolyte may be provided in the cathode as a mixture (e.g., an intimate and substantially uniform mixture). In the composite cathode, particles of the cathode material may be coated with the polymer of the first aspect and / or the electrolyte of the fourth aspect. The composite cathode may also include a ceramic electrolyte (e.g., argyrodite Li6PS5Cl)
[0152] The composite cathode can be prepared by mixing (eg, ball milling) powders of the composite cathode components under dry (ie, solvent-free) conditions and then forming the resulting powder into the composite cathode (eg, by cold pressing under high pressure).
[0153] Composite cathodes can also be prepared by mixing powders of the composite cathode components in a liquid (eg, xylene) to form a slurry and then casting the slurry onto a current collector (eg, an Al current collector) using, for example, a doctor blade.
[0154] The composite cathode can also be prepared by coating the polymer of the first aspect and / or the electrolyte of the fourth aspect onto particles of the cathode material. The coating technique is suitably carried out in solution and then the coated particles are dried. The coated particles of the cathode material can then be mixed with other cathode components (e.g., conductive additives), for example by dry or wet techniques as described above.
[0155] The cathode can be used in an alkali metal ion battery or an alkali metal battery (eg, Li, Na, or K). The cathode is suitable for a lithium ion or lithium metal battery.
[0156] In a seventh aspect, the present invention provides a battery comprising the polymer of the first or third aspect, the electrolyte of the fourth aspect and / or the cathode of the sixth aspect.
[0157] In one arrangement, a battery comprises the electrolyte of the fourth aspect disposed between an anode and a cathode.
[0158] In another arrangement, the battery includes a ceramic electrolyte (e.g., argyrodite Li6PS5Cl) disposed between an anode and a cathode, wherein the battery further includes an electrolyte of the fourth aspect disposed between the ceramic electrolyte and the cathode and / or anode.
[0159] In another arrangement, the battery comprises the cathode of the sixth aspect, wherein the ceramic electrolyte (e.g., argyrodite Li6PS5Cl) is disposed between the cathode and the anode, and wherein the cathode comprises a conductive additive (e.g., carbon) and a cathode material (e.g., LiNi 0.8 Mn 0.1 Co 0.1 O2, referred to as NMC811), wherein particles of the cathode material are coated with the polymer of the first aspect and / or the electrolyte of the fourth aspect.
[0160] The battery may be an alkali metal ion battery or an alkali metal battery (eg, Li, Na or K). Suitably the battery is a Li ion battery or a Li metal battery.
[0161] In an eighth aspect, the invention provides the use of a polymer of the first or third aspect in the manufacture of a battery or a battery component (eg an electrolyte or cathode).
[0162] The following numbered statements 1 to 76 are not claims, but describe specific aspects and embodiments of the invention:
[0163] 1. A polymer having a structure according to formula I:
[0164] AB-A'
[0165] (I)
[0166] in
[0167] A is a polycarbonate block;
[0168] A' is absent or is a polycarbonate block A; and
[0169] B is different from A and is a block composed of poly(ester-co-carbonate) or polycarbonate.
[0170] 2. A polymer according to statement 1, wherein the polymer has a molecular weight of 10-200 kg mol -1 The number average molecular weight (M n ).
[0171] 3. A polymer according to statement 1, wherein the polymer has 15-100 kg mol -1 The number average molecular weight (M n ).
[0172] 4. A polymer according to statement 1, wherein the polymer has a molecular weight of 20-70 kg mol -1 The number average molecular weight (M n ).
[0173] 5. A polymer according to statement 1, wherein the polymer has 30-55 kg mol -1 The number average molecular weight (M n ).
[0174] 6. The polymer according to any of the preceding statements, wherein the polymer comprises 10 to 70% by weight of block A.
[0175] 7. The polymer according to any of the preceding statements, wherein the polymer comprises 16 to 65% by weight of block A.
[0176] 8. The polymer according to any of the preceding statements, wherein the polymer comprises 30 to 40% by weight of block A.
[0177] 9. A polymer according to any of the preceding statements, wherein A has a glass transition temperature of ≥ 20°C, T g .
[0178] 10. A polymer according to any of the preceding statements, wherein A has a glass transition temperature of ≥ 60°C, Tg .
[0179] 11. A polymer according to any of the preceding statements, wherein A has a glass transition temperature of ≥ 80°C (eg, 90-110°C), T g .
[0180] 12. A polymer according to any of the preceding statements, wherein B has a glass transition temperature of ≤ 20°C, T g .
[0181] 13. A polymer according to any of the preceding statements, wherein B has a glass transition temperature of ≤ 0°C, T g .
[0182] 14. A polymer according to any of the preceding statements, wherein B has a glass transition temperature of ≤ -25°C (e.g., -50 to -30°C), T g .
[0183] 15. A polymer according to any of the preceding statements, wherein block A has a glass transition temperature (T g ), block B has a glass transition temperature (T) of -55 to -25°C g ).
[0184] 16. A polymer according to any of the preceding statements, wherein A' is a polycarbonate block A, such that the polymer is a triblock copolymer.
[0185] 17. A polymer according to any of the preceding statements, wherein A' is absent, such that the polymer is a diblock copolymer.
[0186] 18. A polymer according to any one of statements 1 to 15, wherein the polymer is a diblock copolymer and has a molecular weight of 20-70 kg mol -1 The molecular weight (M n ), containing 20-60 wt. % of block A.
[0187] 19. A polymer according to any one of statements 1 to 15, wherein the polymer is a diblock copolymer and has a molecular weight of 20-60 kg mol -1 The molecular weight (M n ), containing 20-45 wt.% of block A.
[0188] 20. A polymer according to any one of statements 1 to 15, wherein the polymer is a diblock copolymer and has a molecular weight of 35-55 kg mol -1 The molecular weight (M n ), containing 20-35 wt.% of block A.
[0189] 21. A polymer according to any one of statements 1 to 15, wherein the polymer is a triblock copolymer and has a molecular weight of 45-70 kg mol -1 The molecular weight (M n ), containing 25-65 wt.% of block A.
[0190] 22. A polymer according to any one of statements 1 to 15, wherein the polymer is a triblock copolymer and has a molecular weight of 47-68 kg mol -1 The molecular weight (M n ), containing 30-55 wt.% of block A.
[0191] 23. A polymer according to any one of statements 1 to 15, wherein the polymer is a triblock copolymer and has a molecular weight of 45-55 kg mol -1 The molecular weight (M n ), containing 30-40 wt.% of block A.
[0192] 24. A polymer according to any of the preceding statements, wherein A has a structure according to formula Ai:
[0193]
[0194] in
[0195] represents the point of attachment of an oxygen atom which is part of B;
[0196] L is a linking group that separates the two oxygen atoms it connects from 2 to 3 carbon atoms apart; and
[0197] X 1 It is a terminal group.
[0198] 25. A polymer according to statement 24, wherein L is a linking group that separates the two oxygen atoms to which it is attached by a distance of 2 carbon atoms.
[0199] 26. A polymer according to statement 24, wherein L is a linking group that separates the two oxygen atoms to which it is attached by a distance of 2 carbon atoms, the two carbon atoms forming part of a ring.
[0200] 27. A polymer according to statement 26, wherein the ring is a 5- to 7-membered carbocyclic or heterocyclic ring.
[0201] 28. The polymer of claim 26 wherein the ring is a 6-membered carbocyclic ring.
[0202] 29. A polymer according to any of the preceding statements, wherein B consists of repeating units, each repeating unit independently having a structure according to formula Bi:
[0203]
[0204] in
[0205] W is O or CH2; and
[0206] V is a group which separates O from W by 3 to 5 carbon atoms.
[0207] Provided that in at least some of the repeating units in block B, W is O.
[0208] 30. A polymer according to statement 29, wherein V is a group separating O from W by a distance of 3-4 carbon atoms.
[0209] 31. A polymer according to any of the preceding statements, wherein a portion of the A and / or B block repeating units independently comprise side chain neutral functional groups FG selected from -P(O)(OH)2, -COOH, -OH, -SO3H, -NH2, -C(O)NH2, -F, -CF3 and -CN N .
[0210] 32. A polymer according to any of the preceding statements, wherein a portion of the A and / or B block repeating units independently comprises a group consisting of -PO3 2- 、-PO2(OH) - 、-COO - 、-SO3 - 、-SO2N - SO2CF3, -N - SO2CF3, -(CF2)2O(CF2)2SO3 - , -BO4 - 、-(C6H4)4B - 、-(C6F4)4B - and -CHFCF2SO3 - The side chain anionic functional group FG A .
[0211] 33. A polymer according to any of the preceding statements, wherein a portion of the A and / or B block repeating units comprises a neutral functional group -P(O)(OH)2.
[0212] 34. A polymer according to any of the preceding statements, wherein a portion of the A block repeating units comprises a neutral functional group -P(O)(OH)2.
[0213] 35. A polymer according to any of the preceding statements, wherein A has a structure according to formula A-ii:
[0214]
[0215] in
[0216] represents the point of attachment of an oxygen atom which is part of B;
[0217] X 1 is a terminal group; and
[0218] Each R 1 independently absent or a group -X-(R 2 ) v ,in
[0219] Each R 2 Independently a side chain neutral functional group FG as defined in statement 31, 32 or 33 N Or side chain anionic functional group FG A ;
[0220] Each v is independently 0 or 1; and
[0221] Each X is (when v is 1) R 2 A linking group to the cyclohexyl ring, or (when v is 0) a terminal group.
[0222] 36. A polymer according to statement 35, wherein each X consists of less than 80 atoms.
[0223] 37. A polymer according to statement 35 or 36, wherein each R 1 Does not exist or is:
[0224]
[0225] 38. A polymer according to any of the preceding statements, wherein B is poly(ester-co-carbonate).
[0226] 39. A polymer according to any of the preceding statements, wherein B is poly(caprolactone-co-trimethylene carbonate).
[0227] 40. A polymer according to statement 38 or 39, wherein block B comprises 60-95 mol % of ester repeating units and 5-40 mol % of carbonate repeating units.
[0228] 41. A polymer according to statement 38 or 39, wherein block B comprises 65-90 mol % of ester repeating units and 10-35 mol % of carbonate repeating units.
[0229] 42. A polymer according to statement 38 or 39, wherein block B comprises 70-90 mol % of ester repeating units and 10-30 mol % of carbonate repeating units.
[0230] 43. A polymer according to statement 38 or 39, wherein block B comprises 75-85 mol % of ester repeating units and 15-25 mol % of carbonate repeating units.
[0231] 44. A method for preparing a polymer, the method comprising the steps of:
[0232] (a) performing a ring-opening polymerization of (i) a cyclic carbonate or (ii) a mixture of a cyclic carbonate and a cyclic ester to form a polymer block B, wherein the polymer block B is a polycarbonate or a poly(ester-co-carbonate); and
[0233] (b) Growth of polymer block A at one or both ends of polymer block B by ring-opening copolymerization of: (i) an epoxide or an oxetane and (ii) carbon dioxide.
[0234] 45. A method according to statement 44, wherein the ring-opening polymerization in step (a) is initiated using a monofunctional initiator, and step (b) comprises growing polymer block A at one end of polymer block B.
[0235] 46. A method according to statement 44, wherein the ring-opening polymerization in step (a) is initiated using a bifunctional initiator, and step (b) comprises growing polymer block A at both ends of polymer block B.
[0236] 47. A process according to statement 44, 45 or 46, wherein steps (a) and (b) are performed in a one-pot process.
[0237] 48. A method according to statement 47, wherein step (a) is terminated and step (b) is initiated by adding carbon dioxide.
[0238] 49. A process according to any one of statements 44 to 48, wherein step (a) comprises carrying out a ring-opening polymerization of a mixture of cyclic carbonates and cyclic esters to form polymer blocks B which are poly(ester-co-carbonates).
[0239] 50. The method according to statement 49, wherein the cyclic carbonate is a 6- to 10-membered cyclic carbonate and the cyclic ester is a 6- to 10-membered cyclic ester.
[0240] 51. A method according to statement 49, wherein the cyclic carbonate is trimethylene carbonate and the cyclic ester is ε-caprolactone.
[0241] 52. A method according to any one of statements 44 to 51, wherein step (b) comprises growing polymer block A at one or both ends of polymer block B by ring-opening copolymerization of: (i) an epoxide, and (ii) carbon dioxide.
[0242] 53. The method according to statement 52, wherein the epoxide is 2,3-dimethyloxirane, a blocked epoxide, a glycidyl ether, or a cyclic epoxide.
[0243] 54. A method according to statement 52, wherein the epoxide is a cyclic epoxide.
[0244] 55. The method according to statement 52, wherein the epoxide is selected from:
[0245]
[0246] 56. A method according to any one of statements 44 to 55, further comprising the steps of:
[0247] (c) modifying a portion of the block A and / or block B repeating units by introducing:
[0248] A side chain neutral functional group selected from -P(O)(OH)2, -COOH, -OH, -SO3H, -NH2, -C(O)NH2,
[0249] -F, -CF3 and -CN; and / or
[0250] Side chain anionic functional groups selected from -PO3 2- 、-PO2(OH) - 、-COO - 、-SO3 - 、-SO2N - SO2CF3,
[0251] -N - SO2CF3, -(CF2)2O(CF2)2SO3 - , -BO4 - 、-(C6H4)4B - 、-(C6F4)4B - and -CHFCF2SO3 - .
[0252] 57. A method according to statement 56, wherein step (c) comprises modifying a portion of the block A and / or block B repeating units by introducing a side chain neutral functional group -P(O)(OH)2.
[0253] 58. A method according to statement 56 or 57, wherein step (c) comprises modifying a portion of the block A repeating units.
[0254] 59. An electrolyte comprising a mixture of a polymer according to any one of Statements 1 to 43 and a metal salt.
[0255] 60. An electrolyte according to statement 59, wherein the metal salt is a Na salt, a Li salt or a K salt.
[0256] 61. An electrolyte according to statement 59, wherein the metal salt has the formula M + X - , where M + Selected from Na + , Li + and K + , X - Selected from BF4 - 、ClO4 - , bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, bis(oxalate)borate, perfluoroalkylsulfonate (e.g. CF3SO3 - ), polyfluoroalkyl sulfonates, PF6, AsF6 - , cyano(trifluoromethanesulfonyl)imide, bis(pentafluoroethanesulfonyl)imide, B(CN)4 - , 4,5-dinitrile-1,2,3-triazole, perylene diimide, 4,5-dicyano-2-(trifluoromethyl)imidazolium, and combinations of two or more thereof.
[0257] 62. An electrolyte according to statement 61, wherein M + For Li + .
[0258] 63. An electrolyte according to statement 61 or 62, wherein X - It is bis(trifluoromethanesulfonyl)imide.
[0259] 64. An electrolyte according to any one of statements 61 to 63, wherein the electrolyte comprises 0.1-80 wt % of the metal salt.
[0260] 65. An electrolyte according to statement 64, wherein the electrolyte comprises 10-50 wt % of the metal salt.
[0261] 66. An electrolyte according to statement 64, wherein the electrolyte comprises 15-25 wt % of the metal salt.
[0262] 67. A method for preparing an electrolyte, the method comprising the steps of:
[0263] (i) preparing a polymer according to the method of any one of Statements 44 to 58; and
[0264] (ii) Mixing the polymer with the metal salt.
[0265] 68. A cathode for a battery, the cathode comprising a polymer as described in any one of Statements 1 to 43 or an electrolyte as described in any one of Statements 59 to 66.
[0266] 69. A cathode according to statement 68, wherein the cathode is a composite cathode comprising a cathode material (e.g., LiNi 0.8 Mn 0.1 Co 0.1 O2, referred to as NMC811), a conductive additive (such as carbon) and either or both of a polymer as defined in any one of Statements 1 to 43 or an electrolyte as defined in any one of Statements 59 to 66.
[0267] 70. A cathode according to statement 69, wherein particles of the cathode material are coated with a polymer and / or an electrolyte.
[0268] 71. A cathode according to statement 69 or 70, wherein the cathode further comprises a ceramic electrolyte (eg, argyrodite Li6PS5Cl).
[0269] 72. A battery comprising a polymer as defined in any one of Statements 1 to 43, an electrolyte as defined in any one of Statements 59 to 66, and / or a cathode as defined in any one of Statements 68 to 71.
[0270] 73. A battery according to statement 72, wherein the battery comprises an electrolyte as defined in any one of statements 59 to 66 disposed between the anode and the cathode.
[0271] 74. A battery according to statement 72, wherein the battery comprises an electrolyte as defined in any one of statements 59 to 66, the electrolyte being arranged as an intermediate layer between a ceramic electrolyte (e.g., argyrodite Li6PS5Cl) and the anode and / or cathode.
[0272] 75. A battery according to statement 72, wherein the battery comprises a cathode as defined in statement 70, wherein a ceramic electrolyte (e.g., argyrodite Li6PS5Cl) is disposed between the cathode and the anode.
[0273] 76. Use of a polymer as defined in any one of statements 1 to 43 in the manufacture of a battery or a battery component (eg an electrolyte or cathode).
[0274] Example
[0275] One or more embodiments of the present invention will now be described, for purposes of illustration only, with reference to the accompanying drawings, in which:
[0276] Figure 1.ROP of ε-CL and TMC, followed by ROCOP of VCHO with CO2, to prepare copolymers PVCHC-PCL / PTMC by switching catalysis. When preparing triblock copolymers, R1 = poly(CL-r-TMC), R2 = (CL-r-TMC-b-VCHC). When preparing diblock copolymers, R1 = R2 = H. (i) ROP was performed at 100°C in 26 mL of a reaction mixture of 40 vol% VCHO and 60 vol% toluene for 10 min. Typical molar ratios: [LZn2Ph2] / [CTA] / [TMC] / [CL] / [VCHO] = 1 / 4 / 375 / 1500 / 3000, where [CTA], [ε-CL] and [TMC] are adjusted to achieve the desired composition and M n To prepare the triblock copolymer, the chain transfer agent (CTA) benzyl alcohol (BDM) was used; methyl benzyl alcohol (Me-BnOH) was used to prepare the diblock. The catalyst concentration was 0.92 mM. (ii) The reaction vessel temperature was maintained at 100 °C and the vessel atmosphere was changed to 1 bar CO2 to initiate the mechanical switch to VCHO / CO2 ROCOP.
[0277] Figure 2 . Exemplary polymer characterization data. (a) Designation of purified block polymer PVCHC-PCL / PTMC-PVCHC 1 H NMR spectrum (CDCl3). (b) The polymer hydroxyl end groups reacted with 2-chloro-4,4,5,5-tetramethyldioxophosphone 31 P{H} spectra (CDCl3). Top: triblock copolymer PVCHC-PCL / PTMC-PVCHC showing PVCHC-OH end groups. Bottom: homopolymer PCL / PTMC showing PCL-OH and PTMC-OH end groups. (c) GPC trace of polymer sample ABA (44, 0.53) performed with THF eluent and calibrated to polystyrene standards.
[0278] Figure 3 Thermal and mechanical behaviors of ABA (50, 0.35) polymer electrolyte membranes containing 17 wt % LiTFSI. (a) DSC trace: ABA (50, 0.35) (top) exhibits a lower T at -49 °C g1 , a weak higher T at 89°C g2 ABA (50, 0.35) with 17 wt% LiTFSI exhibits a lower T at -40 °C g1 , a weak higher T at 100°C g2(b) TGA trace of ABA(44,0.53) containing 17 wt% LiTFSI. (c) Cyclic tensile test (20% strain, 10 mm min -1 (d) Elastic recovery at zero stress after 20% strain as a function of the number of cycles, defined as 100×(ε 20% -ε(0,ε 20% )) / ε 20% , where ε 最大 and ε(0,ε 最大 ) is the maximum strain and the maximum strain ε 最大 Strain in the cycle after zero stress.
[10]
[0279] Figure 4 . Li ion conductivity data of ABA (50.0.35) with 17 wt% LiTFSI. (a)
[0280] Lithium ion conductivity as a function of temperature obtained by electrochemical impedance spectroscopy. (b) VFT fitting.
[0281] Figure 5 The relationship between the ionic conductivity of polymer electrolytes and the M n , hard weight % and LiTFSI weight %; and other electrochemical data. (a): For triblock and diblock copolymers, the ionic conductivity of the material at 30 ° C is a function of the polymer's M n , where all polymers have a fixed hard weight fraction of 0.5. For triblock and diblock copolymers, the ionic conductivity of the material at 30 °C is plotted as a function of the hard weight fraction of the polymer, where all polymers have a hard weight fraction of approximately 50 kg mol -1 Fixed M n (c) Lithium ion conductivity data showing the effect of salt concentration. ABA(50,0.35) samples with 50, 40, 30, 20, and 17 wt % LiTFSI were studied. (d) Cyclic voltammetry curve of ABA(50,0.35) polymer electrolyte with 17 wt % LiTFSI in a cell configuration of lithium on stainless steel at 60 °C at 0.5 mV s -1 Scan rate measurement.
[0282] Materials and methods
[0283] Material
[0284] Unless otherwise stated, all solvents and reagents were purchased and used from commercial sources (Sigma-Aldrich). 4-tert-Butyl-2,6-diformylphenol [H4L](ClO4)2 and H2L were synthesized in air.
[11] Synthesis of Catalyst [LZn2(Ph)2]
[10] , monomer purification and subsequent polymerization were performed under inert conditions using standard Schlenk line techniques and a nitrogen-filled glove box. Vinylcyclohexene oxide (VCHO) and ε-caprolactone (ε-CL) were dried by stirring over CaH2, distilled under reduced pressure and stored under nitrogen. 1,4-Benzenedimethanol (BDM) was recrystallized three times from toluene and kept under nitrogen. Trimethylene carbonate (TMC) was purchased from TCI. It was recrystallized from anhydrous Et2O under nitrogen atmosphere and dried in vacuo before use.
[0285] NMR
[0286] The results were obtained using a Bruker AVIII HD 400 NMR spectrometer. 1 H and 31 P{H}NMR spectrum. Obtained using a Bruker AVII500 NMR spectrometer 13 C{H} NMR spectrum.
[0287] GPC
[0288] GPC data were obtained using a Shimadzu LC-20AD instrument equipped with a refractive index (RI) detector and two PSSSDV 5 μm linear M columns. HPLC grade THF was used as the eluent, flowing at 1.0 mL / min at 30°C. Monodisperse polystyrene standards were used for calibration. Prior to analysis, samples were passed through a 0.2 μm syringe filter.
[0289] DSC
[0290] DSC of the polymers was performed using a DSC3+ (Mettler-Toledo Ltd) instrument. A sealed empty crucible was used as a control and the DSC was calibrated using zinc and indium. The concentration of the polymers was 0.1% by volume under a N2 flow (80 mL min -1 ) at 20℃min -1 The sample was cooled from 25°C to -80°C at a rate of 1.5 and then kept isothermally at -80°C for 5 min. -1 The sample was heated to 200°C at a rate of 100°C / min; kept at 2000°C for another 5 min; and then heated at 10°C / min -1 The rate of cooling is from 200°C to -80°C. The glass transition temperature (T g) is reported as the midpoint of the transition from the third second cycle.
[0291] TGA
[0292] TGA was performed on a TGA / DSC 1 (Mettler Toledo, Inc.) system. -1 ) at 5℃min -1 The polymer sample was heated from 30°C to 500°C at a rate of .
[0293] Tensile measurement
[0294] For the tensile test, dumbbell-shaped specimens (length = 35 mm, gauge length = 10 mm, width = 2 mm) were cut using a Zwick ZCP020 cutter according to ISO 527-2, type 5B specimens. The specimens were tested on a Shimadzu EZ-LZ universal testing machine at a speed of 10 mm min. -1 Uniaxial tensile measurements were performed at a stretching rate of 1000 nm to obtain the stress-strain relationship.
[0295] Electrochemical impedance spectroscopy
[0296] Ionic conductivity was measured by impedance spectroscopy using an MTZ-35 impedance analyzer (Biologic) in the frequency range of 10 MHz–0.01 Hz with an amplitude set to 10 mV. The electrolyte was sandwiched between gold electrodes in a controlled environment sample holder, which was then enclosed in a mesothermal system. Measurements were made at 10 °C intervals between 20 and 70 °C. The samples were equilibrated at each temperature for 20 min before a new recording was made. Resistance was calculated using a modified Debye equivalent circuit using EBioLabs.
[0297] Voltammetry
[0298] Linear scan and cyclic voltammetry were performed on a VMP2 (Bio-Logic). A 4 mm ABA disk (50, 0.35) and a 3 mm lithium disk were sandwiched between two stainless steel disks. The cells were annealed at 60 °C under OCV for 3 h and then charged at 0.5 mV s -1 All procedures were performed in an argon-filled glove box.
[0299] experiment
[0300] Synthesis of H2L
[0301] Ligands were synthesized according to published procedures.
[10] [H4Ln](ClO4) (5.0 g, 6.7 mmol) and MeOH (500 mL) were added to a round bottom flask to give a red / orange solution. The solution was cooled to 0°C and then NaBH4 (7.58 g, 200 mmol) was slowly added to give a colorless solution. The solution was stirred at room temperature for 1 h and then water was added until precipitation was observed (400 mL). The resulting suspension was allowed to stand for 10 h and then filtered, washed with water and dried under vacuum at 40°C to give a white solid. The precipitate was crystallized from methanol to give white crystals (2.56 g, 4.63 mmol, 72%). 1 H NMR (400MHz, CDCl3, 298K): δ (ppm) = 6.93 (s, 4H, Ar-H), 3.73 (s, 8H, CH2), 2.52 (s, 8H, CH2), 1.25 (s, 18H, CH3), 1.01 (s, 12H, CH3).
[0302] Synthesis of [LZn2(Ph)2]
[0303] The catalysts were synthesized according to published procedures.
[10] Under anaerobic conditions, a THF solution (5 mL) of [H2L] (0.40 g, 0.7 mmol) and a THF solution (2 mL) of ZnPh2 (0.25 g, 1.2 mmol) were precooled to -40 ° C and then added to a glass vial to obtain a turbid solution. The mixture was stirred at 25 ° C for 25 h and filtered to obtain a white solid (260 mg, 0.311 mmol, 55%).
[0304] Switching catalysis of VCHO, CO2, TMC and ε-CL
[0305] In a glove box, TMC was added to 1,4-BDM, followed by ε-CL, VCHO, toluene, and LZn2Ph2. The reaction vessel was sealed, removed from the glove box, and heated to 100°C with rapid stirring. When the ε-CL conversion was 90% (about 20 min), the reaction vessel atmosphere was changed to 1 bar CO2. When the VCHO conversion was 15% (about 30 h), the reaction vessel was cooled, opened to the atmosphere, and 0.2 mL of 0.1 M benzoic acid in chloroform was added and stirred. The crude reaction mixture was purified by 1 The conversion of ε-CL and VCHO was determined by H NMR spectroscopy. The reaction mixture was precipitated three times from methanol (3×200 mL) to give a white polymer. The material was dried in vacuo and the block copolymer was isolated as a colorless solid (about 2 g). Figure 1 Specified in a 1 Examples of H NMR spectra; the amounts of reagents used to produce various triblock and diblock copolymers are shown in Table 3.
[0306] Table 1: Reagent quantities for the synthesis of triblock and diblock poly(carbonate-b-ester-r-carbonate).
[0307]
[0308] a The entry for a triblock copolymer is ABA(X,Y), and for a diblock copolymer is AB(X,Y), where X is M n,NMR and Y is the hard weight fraction; b The amount of catalyst LZn2Ph2 in the reaction mixture; c The amount of chain transfer agent (CTA). Benzenedimethanol (BDM) is used to make triblock copolymers, and methylbenzyl alcohol (MeBnOH) is used to make diblock copolymers; c The amount of ε-CL, TMC and VCHO in the reaction mixture. The total volume was made up to 26 mL with toluene.
[0309] Results and discussion
[0310] Polymer synthesis
[0311] pass Switch Catalysis, using according to the literature
[11] The synthesized LZn2Ph2 catalyst produced PVCHC-PCL / PTMC-PVCHC and the corresponding diblock polymer PVCHC-PCL / PTMC. LZn2Ph2 is known to be active for both lactone ROP and epoxide / CO2ROCOP and is able to selectively polymerize from a monomer mixture.
[12] It has phenyl co-ligands: these ligands cannot initiate polymerization, but can react in situ with alcohol initiators to produce initiating species. This produces only hydroxyl telechelic polymers; an important property when targeting ABA and AB block polymers. A typical polymerization was performed using LZn2Ph2 / chain transfer agent / TMC / ε-CL / VCHO in relative ratios of 1 / 4 / 375 / 1500 / 3000. The reaction mixture was 26 mL: approximately 40 vol% VCHO and 60 vol% toluene. The optimal catalyst concentration was 0.92 mM. For triblock copolymers, 1,4-benzenedimethanol (BDM) was used as a chain transfer agent; 4-methylbenzyl alcohol (Me-BnOH) was used to prepare diblock copolymers. The experiment was stirred at 1600 rpm and heated to 100°C.
[0312] To facilitate a systematic study of the properties, two series of triblock polymers were targeted: n ) polymer (ABA(X,0.50)), and a polymer with a fixed M nand polymers (ABA (~50, Y)) with different hard weight % (Table 1). n Both the hard block content and the nanostructure that enables phase separation affect the physical properties of the polymer. The ratios of chain transfer agent, ε-CL, TMC, and VCHO were adjusted to produce the desired polymer weight and composition. A series of AB diblock polymers were also prepared using monofunctional initiators, characterized by M n and the same systematic variation of hardblock content.
[0313] Initially, ROP of ε-CL and TMC produced poly(CL-r-TMC) ( Figure 1 ). The crude reaction mixture 1 H NMR spectrum showed that the ε-CL conversion reached 90% after 20 minutes. At this time, the atmosphere of the reaction vessel was changed to 1 bar CO2 to start the mechanical reaction to VCHO / CO2 ROCOP. Switch This starts from the polyester chain ends, producing the ABA triblock copolymer PVCHC-PCL / PTMC-PVCHC (Scheme 1). ROCOP was allowed to proceed for 30 hours. Afterwards, the reaction mixture was quenched by the addition of 0.2 mL of a 0.1 M benzoic acid solution in chloroform: this solution reacts with the catalyst to stop the polymerization. 1 The crude polymer samples were analyzed by H NMR spectroscopy, and the monomer conversion of ε-CL and VCHO was determined by integrating the peaks corresponding to the monomer (δ = 2.70, 4.87 ppm) and polymer (δ = 4.14, 3.20 ppm). This was not possible for TMC because its signal overlapped with that of ε-CL. The polymer was purified by precipitation from methanol, dried under vacuum, and used 1 H NMR spectrum, 31 The products were characterized by P{H} end group analysis, diffusion ordered NMR spectroscopy (DOSY) and gel permeation chromatography (GPC).
[0314] In the purified polymer 1 In the H NMR spectrum, the expected signals corresponding to PVCHC and PCL-r-PTMC were observed. Integration of the peaks revealed the molar composition of the polymers ( Figure 2 a). Since the signals attributed to TMC (4.08–4.25, 1.99 ppm) all show some overlap with the ε-CL and VCHO signals, respectively, their ratios are difficult to observe; however, the polymer is estimated to be 20 mol% TMC, as targeted. The polymerization was highly selective for the formation of polyesters and polycarbonates, as no ether bonds were observed (3.30–3.60 ppm). Block-linking signals could not be detected due to the high molar mass of the polymer. Repeated precipitation of the polymer did not change the polymer composition, supporting the formation of block copolymers rather than blends. The polymerization was performed according to literature procedures.
[13] After the hydroxyl groups of the polymer react with the phosphorus reagent, 31 P{H}NMR spectrum was used for chain end group analysis. The vinyl cyclohexenol end group signal (146.6 ppm) was observed, indicating the selective block copolymer formation ( Figure 2 b). DOSY further confirmed the block structure. A single diffusion coefficient was observed, indicating the connecting blocks of PVCHC and PCL / PTMC; if a homopolymer blend was present, two different diffusion coefficients would be observed.
[0315] The molecular weight of the polymer is determined by 1 H NMR spectroscopy and GPC estimation, in addition, theoretical values can be calculated based on the monomer / initiator ratio and monomer conversion. 计算 and DP NMR There was good agreement between the two, indicating that there was little impurity (such as H2O) acting as an additional chain transfer agent (Table 1). GPC was performed using THF as the eluent. A monomodal mass distribution was observed, with the polymer showing a high M n ( Figure 2 c). This supports the formation of one type of polymer chain rather than a mixture of homopolymer and block copolymer. For most samples, M n,NMR and M n,GPC There is good agreement between the two (Table 1). It is not expected that this polymer would have a narrow polydispersity index (D).
[14] ε-CL provides a major growth site for ROP, thus having a wider dispersion. n,NMR and M n,GPC There were differences between the two groups, especially for ABA (66, 0.52), ABA (50, 0.35) and ABAB (69, 0.58). This may be due to the GPC effect: it has been reported previously
[15] The M of other polymers n,NMR and M n,GPC There is a difference. This can be attributed to the fact that polycarbonate exhibits a different chain folding behavior than polystyrene, with which the column was calibrated. This results in a lower hydrodynamic volume and therefore lower measured molar mass values.
[0316] Table 2: Characterization data of triblock copolymers and diblock copolymers
[0317]
[0318] a The entry for triblock copolymers is ABA(X,Y) and the entry for diblock copolymers is AB(X,Y), where X is M n,NMR , Y is the hard weight score; bCalculated from the initial [ε-CL+TMC+VCHO]0 / [BDM]0 ratio and monomer conversion; c From the purified polymer 1 The H NMR spectrum is characterized by the aromatic initiator resonances (7.34 ppm for 1,4-BDM and 7.62 ppm for
[0319] Me-BnOH is 7.17 ppm) and the integral of PVCHC (5.76 ppm) and PCL / PTMC (2.00, 1.38 ppm) resonances is determined; d The M of the total block copolymer was determined by GPC with THF eluent and calibrated with PS standards. n ; e By DSC (10℃min -1 Heating rate) estimation, third heating curve; f Thermal degradation temperature of polymer with 17 wt% LiTFSI as determined by TGA. Reported as the temperature at 5% mass loss.
[0320] Thermal properties
[0321] Thermal data were obtained using DSC. The polymer was completely amorphous with a low T at about -40 °C. g , corresponding to the inner polymer (CL-r-TMC) block, has a weaker higher T at about 100 °C. g , corresponding to the hard poly(VCHO-alternative-CO2) block ( Figure 3 a) T g The values are consistent with those in the literature, among which the T g =106℃, T of PCL / PTMC g =-56℃.
[14] For higher T values close to homopolymer values g value and lower T g The observation of values of indicates the presence of phase separation in the polymer. This is desirable for good mechanical properties: flexibility, ductility, elastic recovery, high temperature stability, and tensile strength.
[0322] Since these polymers are being investigated for battery applications, it is of interest to investigate their performance after the addition of lithium salts. Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was chosen because this salt is widely used in lithium-ion battery research.
[17] 17 wt% LiTFSI (relative to the total polymer M) was added to the polymer. n ), and the electrolyte membrane was prepared by solvent casting.
[18]
[0323] The DSC traces of the polymer with salt retain their amorphous nature and show a T of 2.34 Å relative to that of the pure polymer. g change( Figure 3 a). ABA (50, 0.35) showed a higher T under the addition of salt g and lower T g The lower T g Corresponding to polyester block poly (CL-r-TMC): as in the literature [17,19] It was observed that the salt was able to form transient crosslinks within the block. g , Kimura et al. have shown that the T g It increases from 0 to 10 wt% salt, which may be due to the interaction between carbonyl oxygen and Li ions.
[20] This supports the higher T relative to polycarbonate PVCHC. g increase.
[0324] The thermal stability of the polymers was measured with the addition of 17 wt % LiTFSI. For all polymers, T d,5% Above 200 °C (Table 1): This is high enough for the desired application. The TGA curve shows three distinct regions: 200-270 °C corresponds to the decomposition of the poly(CL-r-TMC) block; 270-385 °C corresponds to the decomposition of the PVCHC block; 385–500 °C corresponds to the decomposition of LiTFSI ( Figure 3 b).
[0325] Mechanical properties
[0326] The elastic recovery rate: the ability of a material to return to its original shape after being strained, of ABA (50, 0.35) polymer electrolyte membranes containing 17 wt.% LiTFSI was determined. In batteries, polymers experience stress and strain during charge and discharge cycles, so this is a critical parameter. Dumbbell-shaped specimens were cut from the polymer membrane using a cutter. Three samples of ABA (50, 0.35) were tested: the mean value is reported, and the error is expressed as the standard deviation. Each sample was tested at 10 mm min -1 The stretching rate was subjected to 10 hysteresis cycles to a 20% strain. This strain was used because it is slightly higher than the volume change experienced by high capacity cathode particles.
[21] The first elastic cycle differs from those that follow due to the initial disentanglement of the polymer chains. An elastic recovery of 70% was recorded: this is lower than that observed for an ideal elastomer, but still suggests that the material shows recovery after undergoing strain ( Figure 4 c, 2d).
[0327] Ion transport
[0328] Using electrochemical impedance spectroscopy (EIS), lithium ion conductivity measurements of a series of polymers were obtained in a 2-electrode cell (Table 3). Electrolyte membranes with a thickness of ~250 μm were prepared in a Teflon mold by solvent casting the polymer plus a 17 wt% LiTFSI solution in THF (20 wt%). They were dried for 48 h by evaporation of the solvent under ambient pressure and N2 atmosphere, and then vacuum dried at 40 °C for 72 h. The measurements were performed at temperature intervals of 10 °C between 20 °C and 70 °C.
[0329] The triblock copolymer and diblock copolymer with the highest ionic conductivity at 30 °C are ABA (50, 0.35) and AB (37, 0.21), respectively: 5.9 × 10 -6 S cm -1 and 9.8×10 -6 S cm -1 The ionic conductivity versus temperature of each sample has been plotted and shows that ABA(50,0.35)( Figure 4 a). The ionic conductivity increases with the increase of temperature: from 5.9×10 -6 S cm -1 When it increases to 70℃, it is 7.2×10 -5 S cm -1 , which is due to the increase in the mobility of polymer chains with increasing temperature, thereby increasing the ion mobility.
[0330] The temperature dependence of ionic conductivity can be fitted by Vogel-Fulcher-Tammann (VFT) by plotting Eq. 1 ( Figure 4 b) (A modified Arrhenius equation) is used for modeling:
[0331] σ=AT -1 / 2 exp[-B / (T-T0)] (1)
[0332] Where A is a constant proportional to the number of carrier ions, B is proportional to Li + The activation energy of the movement is related to T0, which is the temperature at which the configuration entropy is zero (T0≈T g –50k).
[0333] For the studied polymers, the plot shows a linear relationship. This suggests an ionic conduction mechanism in which ions hop between empty coordination sites with the help of segmental motion of the polymer. This is true for all studied polymers. The gradient of the plot allows calculation of the activation energy of the electrolyte: ABA(51,0.35) has an activation energy of 17.4 kJ mol -1This value is higher than that of poly(CL-r-TMC) reported by Mindemark et al. (9.4 kJ mol -1 ).
[14] This indicates that the presence of the PVCHC hard block creates an additional energy barrier for ion movement. a There is a positive correlation between and lnA, similar to the observation of Balsara et al. for poly(styrene-b-ethylene oxide) electrolytes.
[22] Therefore, the lower E a does not necessarily correspond to higher ionic conductivity, since there are also fewer carrier ions.
[0334] Table 3: Lithium ion conductivity data of ABA and AB polymers
[0335]
[0336] a The entry for triblock copolymers is ABA(X,Y) and the entry for diblock copolymers is AB(X,Y), where X is M n,NMR , Y is the hard weight score; b From the purified polymer 1 The H NMR spectra were determined by integration of the aromatic initiator resonances (7.34 ppm for 1,4-BDM and 7.17 ppm for Me-BnOH) with those of PVCHC (5.76 ppm) and PCL / PTMC (2.00, 1.38 ppm); c By DSC (10℃min -1 Heating rate), the lower (T g1 ) and higher (T g2 ) glass transition temperature; d Ionic conductivity measured using impedance spectroscopy. The ionic conductivity was calculated by fitting the obtained data to the resistance obtained in a modified Debye circuit;
[23] di Lithium ion conductivity at 70℃, except for * The values are made at 60°C and are marked with ** The value is carried out at 50℃, and the error of the value is 9%; dii The Li ion conductivity at 30°C has an error of 11%; e Activation energy of Li ion transport obtained by VFT fitting; f Relative free charge carrier concentrations of polymer electrolytes obtained from VFT fitting.
[0337] For this group of polymers, the ionic conductivity is not significantly affected by the glass transition temperature of either the soft or hard blocks. g1Between -53 and -33°C, T g1 There is no significant trend with ionic conductivity. T of polymer samples AB (45, 0.47) and AB (69, 0.58) g1 The ionic conductivity is also the lowest (2.0×10 -7 S cm -1 , 2.1×10 -7 S cm -1 ). This shows that for this system, reducing T g1 Up to -20–-33°C is an effective strategy for improving ionic conductivity; below this, other factors become more important.
[19]
[0338] The relationship between the ionic conductivity of the material and its M n The ionic conductivity of the triblock polymer with a fixed hardness weight fraction of 0.5 at 30 °C increases with M n The opposite trend was observed for the diblocks: with an increase in M n As their ionic conductivity increases, they decrease ( Figure 5 a) For triblock copolymers, this may be due to the high M n The polymer has a larger crystallite size.
[19] This is an encouraging finding because high M n The polymer may show improved mechanical properties, such as higher storage modulus. For diblocks, higher M n Leading to significantly higher T g ——For AB(69,0.58), T g1 An increase of 36°C relative to the pure polymer - this leads to a decrease in ionic conductivity.
[0339] For a fixed M n About 50 kg mol -1 For the triblock copolymer, the ionic conductivity peaks at a hard weight fraction of 0.35: more or less hard block content leads to a decrease in ionic conductivity. A similar trend is seen for the diblock copolymer: the ionic conductivity is highest at a hard weight fraction of 0.33 ( Figure 5 b) At this composition, the polymer is likely to form a phase that is favorable for ion transport.
[0340] The effect of salt concentration on the ionic conductivity of polymer ABA (50, 0.28) was studied. Electrolyte membranes containing 17, 20, 30, 40, and 50 wt% LiTFSI were prepared. For ionic conductivity, the optimal amount of LiTFSI was 20 wt% ( Figure 5 c). This is because too little salt can lead to a reduction in free charge carriers, whereas too much salt can lead to transient cross-linking of the polymer chains. [17,24] This can be observed in the DSC traces: In general, as the salt concentration decreases, the lower the T g Also lowered.
[0341] Electrochemical performance
[0342] The polymer with the highest ionic conductivity at 30°C is AB (37.0.21) (9.8×10 -5 S cm -1 ) and AB (54.0.33) (2.2×10 -5 S cm -1 ABA(50,0.35) showed the best performance overall and was further investigated as the lead polymer.
[0343] The electrochemical stability of carbonyl coordination polymers is generally greater than that of PEO electrolytes. To evaluate the electrochemical stability window of this material, linear sweep voltammetry (LSV) was performed on ABA (50, 0.35) electrolyte. The stability between the open circuit voltage (OCV) and 6 V at 60 °C was evaluated using a lithium | polymer | stainless steel cell configuration with a scan rate of 0.05 mV s -1 The cell was shown to be stable by holding the OCV for 3 hours before scanning. The polymer + The above are oxidatively stable; this indicates compatibility with high voltage cathodes. Its stability is comparable to other polyester- and polycarbonate-based electrolytes in the literature, such as poly(CL-r-TMC) (>5 V) and poly(styrene-b-CL-r-TMC) (5 V).
[14]
[25] Cyclic voltammetry was performed on ABA(50,0.35) between 3 and 4.5 V using the same cell configuration as in the linear sweep. It showed good oxidative stability over 35 cycles. Figure 5 d).
[0344] in conclusion
[0345] pass Switch Catalysis has enabled the synthesis of block copolymers of two different structures: AB and ABA type polymers have been produced, where A is a polycarbonate block (PVCHC) and B is a poly(ester-co-carbonate) (PCL-r-TMC). Experimental data are consistent with block formation and allow the measurement of hard block weight % and molar mass values. Polymer electrolytes were prepared using LiTFSI salts. All tested polymer electrolytes have adequate thermal stability, T d,5%>200℃, and by observing the upper and lower T g Phase separation was demonstrated. The material showed a moderate elastic recovery of 70% investigated by cyclic tensile tests.
[0346] The Li ion conductivity was measured using electrochemical impedance spectroscopy. The conductivity was good at high temperature (for ABA (50, 0.35), σ 70℃ =2.2×10 -4 S cm -1 ), showing medium performance at ambient temperature (for ABA (50, 0.35), σ 30℃ =5.9×10 -6 S cm -1 ). Relevant trends in polymer composition and structure were elucidated. Electrochemical performance has been investigated: linear sweep voltammetry showed that the electrolyte is stable at >5V, and cyclic voltammetry has successfully cycled the material between 3V and 4.5V for 35 times.
[0347] While specific embodiments of the present invention have been described herein for purposes of reference and illustration, various modifications will become apparent to those skilled in the art without departing from the scope of the invention as defined in the appended claims.
[0348] References
[0349] [1]H.Government,(Ed.:DfTransport),2021.
[0350] [2]X.Wang,R.Kerr,F.Chen,N.Goujon,JMPringle,D.Mecerreyes,M.Forsyth,PCHowlett,Adv.Mater.,n / a,1905219.
[0351] [3]aL.Long,S.Wang,M.Xiao,Y.Meng,J.Mater.Chem.A2016,10038-10069;bT.Famprikis,P.Canepa,JADawson,MSIslam,C.Masquelier,Nature Materials2019,18,1278-1291;cP.Albertus,V.Anandan,C.Ban,N.Balsara,I.Belharouak,J.Buettner-Garrett,Z.Chen,C.Daniel,M.Doeff,N.J.Dudney,B.Dunn,S.J.Harris,S.Herle,E.Herbert,S.Kalnaus,J.A.Libera,D.Lu,S.Martin,B.D.McCloskey,M.T.McDowell,Y.S.Meng,J.Nanda,J.Sakamoto,ECSelf,S.Tepavcevic,E.Wachsman,C.Wang,ASWestover,J.Xiao,T.Yersak,ACS Energy Letters 2021,6,1399-1404.
[0352] [4]aY.Kato,S.Hori,T.Saito,K.Suzuki,M.Hirayama,A.Mitsui,M.Yonemura,H.Iba,R.Kanno,Nat.Energy 2016,1,16030;bH.Buschmann,J. S.Berendts,A.Kuhn,P.Bottke,M.Wilkening,P.Heitjans,A.Senyshyn,H.Ehrenberg,A.Lotnyk,V.Duppel,L.Kienle,J.Janek,Phys.Chem.Chem.Phys.2011,13,19378-19392.
[0353] [5]K.Jeong,S.Park,S.-Y.Lee,J.Mater.Chem.A2019,7,1917-1935.
[0354] [6]H.Chen,M.Ling,L.Hencz,HYLing,G.Li,Z.Lin,G.Liu,S.Zhang,Chem.Rev.2018,118,8936-8982.
[0355] [7]DEFenton,JMParker,PVWright,Polymer 1973,14,589.
[0356] [8]aZ.Geng,NSSchauser,J.Lee,RPSchmeller,SMBarbon,RASegalman,NALynd,CJHawker,Macromolecules 2020;bE.Tsuchida,H.Ohno,K.Tsunemi,N.Kobayashi,Solid State Ion.1983,11,227-233;cY.Zhao,Y.Bai,W.Li,M.An,Y.Bai,G.Chen,Chem.Mater.2020.
[0357] [9]DTHJr.,NPBalsara,2013,43,503-525.
[0358]
[10] MRKember,PDKnight,PTRReung,CKWilliams,J.Am.Chem.Soc.2009,48,931-933.
[0359]
[11] TTDChen,University of Oxford 2020.
[0360]
[12] aC.Romain,JAGarden,G.Trott,A.Buchard,AJPWhite,CKWilliams,Chem.Eur.J.2017,23, 7367-7376;bM.R.Kember,J.Copley,A.Buchard,CKWilliams,Polym.Chem.2012,3,1196-1201.
[0361]
[13] A.Spyros,DSArgyropoulos,RHMarchessault,Macromolecules 1997,30,327-329.
[0362]
[14] J.Mindemark,B.Sun,E. D.Brandell,J.Power Sources 2015,298,166-170.
[0363]
[15] J. Kimpel, University of Oxford 2019.
[0364]
[16] H.Zhang,B.Liu,H.Ding,J.Chen,Z.Duan,Polymer 2017,129,5-11.
[0365]
[17] J.Mindemark,MJLacey,T.Bowden,D.Brandell,Prog.Polym.Sci.2018,81,114-143.
[0366]
[18] A.Bergfelt,G.Hernández,R.Mogensen,MJLacey,J.Mindemark,D.Brandell,T.M.Bowden,ACS Appl.Polym.Mater.2020,2,939-948.
[0367]
[19] DMPesko,Y.Jung,ALHasan,MAWebb,GWCoates,TFMiller,NPBalsara,Solid State Ion.2016,289,118-124.
[0368]
[20] K.Kimura,J.Motomatsu,Y.Tominaga,J.Phys.Chem.C 2016,120,12385-12391.
[0369]
[21] Y.Shi,X.Zhou,G.Yu,Acc.Chem.Res.2017,50,2642-2652.
[0370]
[22] M.Chintapalli,TNPLe,NRVenkatesan,NGMackay,AARojas,JLThelen,XCChen,D.Devaux,NPBalsara,Macromolecules 2016,49,1770-1780.
[23] RAHuggins,Ionics 2002,8,300-313.
[0371]
[24] MARatner,DFShriver,Chemical Reviews 1988,88,109-124.
[0372]
[25] A.Bergfelt,M.J.Lacey,J.Hedman,C. D.Brandell,T.Bowden,RSCAdvances 2018,8,16716-16725.
Claims
1. A polymer having a structure according to formula I: AB-A' (I) in A is a polycarbonate block; A' is absent or is a polycarbonate block A; and B is different from A and is a block composed of poly(ester-co-carbonate) or polycarbonate.
2. The polymer according to claim 1, wherein the polymer has a mass fraction of 15 to 100 kg mol -1 The number average molecular weight (M n ).
3. The polymer according to claim 1, wherein the polymer has a molecular weight of 30-55 kg mol -1 The number average molecular weight (M n ).
4. The polymer of claim 1, 2 or 3, wherein the polymer comprises 16-65 wt% of block A.
5. The polymer of claim 1, 2 or 3, wherein the polymer comprises 30-40 wt% of block A.
6. The polymer according to any one of the preceding claims, wherein A has a glass transition temperature, T g .
7. The polymer according to any one of the preceding claims, wherein B has a glass transition temperature of ≤ 0°C, T g .
8. A polymer according to any one of the preceding claims, wherein A' is a polycarbonate block A, such that the polymer is a triblock copolymer.
9. The polymer of any one of claims 1 to 7, wherein A' is absent, such that the polymer is a diblock copolymer.
10. A polymer according to any one of the preceding claims, in: (1) The polymer is a diblock copolymer with a molecular mass of 20-70 kg mol -1 The molecular weight (M n ) and contains 20-60 wt% of block A, or (2) the polymer is a triblock copolymer having 45-70 kg mol -1 The molecular weight (M n ) and contains 25-65 wt.% of block A.
11. A polymer according to any one of the preceding claims, wherein A has a structure according to formula Ai: in 1 represents the point of attachment of an oxygen atom which is part of B; L is a linking group that separates the two oxygen atoms it connects from 2 to 3 carbon atoms apart; and X 1 It is a terminal group.
12. The polymer according to claim 11, wherein L is a linking group that separates the two oxygen atoms to which it is attached by a distance of 2 carbon atoms, the two carbon atoms forming part of a ring.
13. A polymer according to any one of the preceding claims, wherein a portion of the A and / or B block repeating units independently comprise side chain neutral functional groups FG N and / or side chain anionic functional group FG A , where FG N Selected from -P(O)(OH) 2 , -COOH, -OH, -SO 3 H, -NH 2 、-C(O)NH 2 , -F, -CF 3 and -CN, FG A Selected from-PO 3 2- ,-PO 2 (OH) - 、-COO - 、-SO 3 - 、-SO 2 N - SO 2 CF 3 、-N - SO 2 CF 3 ,-(CF 2 ) 2 O(CF 2 ) 2 SO 3 - , -BO 4 - 、-(C 6 H 4 ) 4 B - 、-(C 6 F 4 ) 4 B - and -CHFCF 2 SO 3 - .
14. A polymer according to any one of the preceding claims, wherein A has a structure according to formula A-ii: in 1 represents the point of attachment of an oxygen atom which is part of B; X 1 is a terminal group; and Each R 1 independently absent or a group -X-(R 2 ) v ,in Each R 2 Independently a side chain neutral functional group FG as defined in claim 13 N Or side chain anionic functional group FG A ; Each v is independently 0 or 1; and Each X is (when v is 1) R 2 A linking group to the cyclohexyl ring, or (when v is 0) a terminal group.
15. A polymer according to any preceding claim, wherein B is poly(ester-co-carbonate).
16. The polymer according to any one of the preceding claims, wherein B is poly(caprolactone-co-trimethylene carbonate), wherein block B comprises 70-90 mol% of ester repeating units and 10-30 mol% of carbonate repeating units.
17. A method for preparing a polymer, the method comprising: The following steps are involved: (a) performing a ring-opening polymerization of (i) a cyclic carbonate or (ii) a mixture of a cyclic carbonate and a cyclic ester to form a polymer block B, wherein the polymer block B is a polycarbonate or a poly(ester-co-carbonate); and (b) Growth of polymer block A at one or both ends of polymer block B by ring-opening copolymerization of: (i) an epoxide or an oxetane and (ii) carbon dioxide.
18. The method according to claim 17, wherein the ring-opening polymerization in step (a) is initiated using a monofunctional initiator, and step (b) comprises growing polymer block A at one end of polymer block B.
19. The method according to claim 17, wherein the ring-opening polymerization in step (a) is initiated using a bifunctional initiator, and step (b) comprises growing polymer block A at both ends of polymer block B.
20. The process of claim 17, 18 or 19, wherein steps (a) and (b) are performed in a one-pot process and wherein step (a) is terminated and step (b) is initiated by adding carbon dioxide.
21. The method according to any one of claims 17 to 20, further comprising the steps of: (c) modifying a portion of the block A and / or block B repeating units by introducing: Side chain neutral functional group selected from -P(O)(OH) 2 , -COOH, -OH, -SO 3 H, -NH 2 、-C(O)NH 2 , -F, -CF 3 and-CN; and / or Side chain anionic functional groups selected from -PO3 2- ,-PO 2 (OH) - 、-COO - 、-SO 3 - 、-SO 2 N - SO 2 CF 3 、-N - SO 2 CF 3 ,-(CF 2 ) 2 O(CF 2 ) 2 SO 3 - , -BO 4 - 、-(C 6 H 4 ) 4 B - 、-(C 6 F 4 ) 4 B - and -CHFCF 2 SO 3 - .
22. An electrolyte comprising a mixture of a polymer according to any one of claims 1 to 16 and a metal salt.
23. The electrolyte of claim 22, wherein the metal salt has the formula M + X - , where M + Selected from Na + , Li + and K + , X - Selected from BF 4 - , ClO 4 - , bis(fluorosulfonyl)imide, bis(trifluoromethanesulfonyl)imide, bis(oxalate)borate, perfluoroalkylsulfonate (e.g. CF 3 SO 3 - ), polyfluoroalkyl sulfonates, PF 6 , AsF 6 - , cyano(trifluoromethanesulfonyl)imide, bis[(pentafluoroethane)sulfonyl]imide, B(CN) 4 - , 4,5-dinitrile-1,2,3-triazole, perylene diimide, 4,5-dicyano-2-(trifluoromethyl)imidazolium, and combinations of two or more thereof.
24. A cathode for a battery, the cathode comprising a polymer as claimed in any one of claims 1 to 16 or an electrolyte as claimed in claim 22 or 23.
25. A battery comprising a polymer as claimed in any one of claims 1 to 16, an electrolyte as claimed in claim 22 or 23, and / or a cathode as claimed in claim 24.
Citation Information
Cited By
Polarization process activation characteristic determination method and device, equipment and medium
CN121186450A