Thermally conductive compositions for high temperature applications
By using auxiliary antioxidants with specific melting point temperatures and thermally conductive particulate fillers in phase-change thermally conductive materials, the problem of degradation of existing materials at high temperatures is solved, and the improvement of high temperature stability and thermal conductivity is achieved.
Patent Information
- Application Number
- CN202380025141.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-03
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-01
AI Technical Summary
Existing phase change thermally conductive materials are prone to degradation at high temperatures, resulting in reduced performance and cannot remain stable in a long-term high-temperature environment.
The thermally conductive composition is formed using auxiliary antioxidants with a melting point temperature of 40 to 85°C as a bifunctional phase change component, instead of some or all of the alkane wax, combined with non-silicone resin and thermally conductive particulate filler to improve high temperature stability .
After 1000 hours at 175°C, the thermal performance of the thermal conductivity composition decreased by less than 20%, achieving stable thermal conductivity at high temperatures and extending the service life of the material.
Smart Images

Figure BDA0005024158360000061 
Figure BDA0005024158360000062
Abstract
Description
Technical Field
[0001] The present invention relates generally to thermally conductive compositions and, more particularly, to phase change thermally conductive compositions that are stable at elevated temperatures to limit degradation of performance over time. Background Art
[0002] Thermally conductive materials are widely used as interfaces between, for example, heat generating electronic components and heat sinks to allow excess thermal energy to be transferred from the electronic components to the thermally coupled heat sink. A large number of designs and materials for such thermal interfaces have been implemented, with the highest performance being achieved when gaps between the thermal interface and the corresponding heat transfer surface are substantially avoided to promote conductive heat transfer from the electronic component to the heat sink. The thermal interface material is therefore preferably mechanically conformable to the somewhat uneven heat transfer surfaces of the respective components. In addition, the thermal interface material is preferably usable over a long service life at elevated operating temperatures.
[0003] Electronic components such as semiconductors, microprocessors, resistors, and circuit boards generate a lot of heat that must be removed for the device to work properly. High-performance computing and telecommunications applications generate a lot of heat, so thermal interface materials with extremely low thermal impedance are needed to maximize the conduction of heat away from sensitive electronic components. One conventional method to provide a low impedance interface is temperature-activated phase change materials. The operating heat of the electronic components causes the temperature in the system to rise above the softening point or melting point of the phase change component of the thermal interface material. When this happens, the interface viscosity (interfaceviscosity) drops significantly to improve conformity with the heat transfer surface, thereby improving the efficiency of heat conduction from the electronic components. The phase change component of the thermal interface material is usually composed of alkane waxes (including natural waxes, synthetic waxes, and petroleum-based waxes). Paraffin is a commonly used phase change component because its melting point temperature is in the range of about 40°C to 120°C. However, paraffin and other conventional phase change components degrade at the high temperatures experienced in high-performance electronic devices. Degradation often includes drying and cracking during long-term use at high temperatures, which can have an adverse effect on thermal performance.
[0004] Therefore, one object is to improve high temperature stability in phase change thermally conductive compositions. Summary of the invention
[0005] By the present invention, conventional alkane wax can be completely or partially replaced by a bifunctional phase change component exhibiting high temperature stability, thereby imparting high temperature stability to the thermally conductive interface material in which the bifunctional phase change component is used. The bifunctional phase change component contains an auxiliary antioxidant having a melting point temperature of 40 to 85°C.
[0006] In one embodiment, the thermally conductive composition comprises a non-silicone resin, a primary antioxidant and a secondary antioxidant, wherein the secondary antioxidant is compatible with the primary antioxidant and is present in the composition at a concentration of 20 to 50% by weight of the non-silicone resin. The secondary antioxidant is present in the composition at a ratio of 95 to 99 parts by weight of the secondary antioxidant to 1 to 5 parts by weight of the primary antioxidant. The secondary antioxidant has a melting point temperature of 40 to 85°C. The thermally conductive composition also comprises a thermally conductive particulate filler, wherein the composition exhibits a thermal conductivity of at least 1 W / m*K and a loss of less than 20% by weight after 1000 hours at 175°C.
[0007] The thermally conductive composition may include 0.5 to 20 weight percent of a non-silicone resin. In some embodiments, the thermally conductive composition may include 0.5 to 5 weight percent of a non-silicone resin. The non-silicone resin may include a pressure sensitive adhesive. The non-silicone resin may include a polyamide.
[0008] In some embodiments, the secondary antioxidant may be thiol-based. In some embodiments, the secondary antioxidant may include didodecyl 3,3'-thiodipropionate. In some embodiments, the secondary antioxidant may have a melting point temperature of 50 to 60°C.
[0009] In some embodiments, the composition may include a hydrocarbon wax having a melting point temperature of 40 to 120° C. In other embodiments, the composition may be substantially free of a wax component.
[0010] In some embodiments, the thermally conductive particulate filler is selected from the group consisting of aluminum, aluminum nitride, aluminum silica alloy, zinc oxide, and combinations thereof. 50 ) may be less than 25 μm. In some embodiments, the thermally conductive particulate filler comprises 70 to 95 weight percent of the composition.
[0011] The thermally conductive composition may include a plasticizer. In some embodiments, the plasticizer includes a trimellitate. In some embodiments, the trimellitate plasticizer is present in the composition at a concentration of 0.5 to 20% by weight in the composition. In some embodiments, the trimellitate plasticizer is present in the composition at a concentration of 0.5 to 5% by weight in the composition.
[0012] The thermally conductive composition may include a wetting agent. In some embodiments, the thermally conductive composition may include 0.1 to 1.5 weight percent of a wetting agent.
[0013] The thermally conductive composition may include additional antioxidants different from the primary and secondary antioxidants. In some embodiments, the thermally conductive composition may include a sterically hindered phenolic antioxidant different from the primary and secondary antioxidants. In some embodiments, the thermally conductive composition may include 0.1 to 1.5 weight percent of a sterically hindered phenolic antioxidant different from the primary and secondary antioxidants.
[0014] The thermally conductive composition may include a metal deactivator antioxidant different from the primary and secondary antioxidants. In some embodiments, the thermally conductive composition includes 0.1 to 1.5 weight percent of a metal deactivator antioxidant different from the primary and secondary antioxidants.
[0015] The thermally conductive printable composition comprises a non-silicone resin, a primary antioxidant, a thiol-based secondary antioxidant, a thermally conductive particulate filler, and a solvent compatible with the remaining components of the composition. The thiol-based secondary antioxidant is compatible with the primary antioxidant and is present in the composition at a concentration of 20 to 50% by weight of the non-silicone resin. The secondary antioxidant may be present in the composition at a ratio of 95 to 99 parts by weight of the secondary antioxidant to 1 to 5 parts by weight of the primary antioxidant. The secondary antioxidant may have a melting point temperature of 40 to 85°C. The thermally conductive particulate filler may be present at 50 to 98% by weight in the composition, wherein the composition exhibits a thermal conductivity of at least 1W / m*K and a loss of less than 20% by weight after 1000 hours at 175°C. The composition dissolved in the solvent may be printed onto a substrate and dried to form a thermal interface material in thermal contact with the substrate. The composition may be printed onto a substrate by known printing techniques (e.g., inkjet printing, extrusion through a die, three-dimensional printing, etc.). In some embodiments, the solvent may be selected from ethyl acetate and ethylhexyl acetate. DETAILED DESCRIPTION
[0016] Disclosed are thermally conductive compositions and articles made from the compositions, which can be used as thermal interfaces between heat-generating components and heat-dissipating devices.
[0017] In an exemplary embodiment, the electronic package includes a substrate and one or more electronic components fixed on the substrate. The electronic package also includes a heat sink (e.g., a heat sink) and a thermal interface in the thermal path between the electronic component and the heat sink. The electronic package is arranged to dissipate the heat energy generated by the electronic component by providing a high thermal conductivity path from the electronic component to a heat absorbing fluid medium in contact with the heat sink. In typical applications, the fluid medium can be a gas (e.g., air), which is driven by an air mover to absorb heat energy from the heat sink. The electronic package can be used in various electronic applications, such as data processors, data storage devices, communication boards, antennas, etc. This type of equipment can be used for computing devices, communication devices, and their peripheral devices. In a particular example, the electronic package can be used to support various functions in a cellular communication device.
[0018] The substrate may serve one or more of a variety of functions in addition to serving as a support for the electronic components. The substrate may be, for example, a circuit board, such as a printed circuit board having conductive traces on a mounting surface for electrically connecting the desired electronic components in the assembly. The electronic components may be electrically connected to the wiring traces by soldering or other known techniques. During operation, electronic components typically generate a large amount of excess heat energy that must be dissipated to maintain optimal performance.
[0019] The thermal interface provides a thermally conductive bridge between the electronic component and the heat sink, which can be thermally coupled to the thermal interface in a manner that most efficiently transfers thermal energy to the heat sink.
[0020] Resin
[0021] The thermally conductive compositions of the present invention may include non-silicone resins that provide a matrix for incorporating thermally conductive fillers and other additives. Exemplary non-silicone resins that can be used in the compositions of the present invention may include various thermoplastic materials, including thermoplastic elastomers, which may or may not be naturally tacky. Suitable thermoplastic elastomers may include, for example, copolymers, including styrenic copolymers such as styrene-butadiene-styrene styrene (SBS), styrene-ethylene / butylene-styrene (SEBS), styrene-isoprene-styrene (SIS), styrene-ethylene / propylene-styrene (SEPS), and combinations thereof. Thermoplastic elastomers also include thermoplastic / elastomer blends and alloys, such as non-crosslinked polyolefins, which are thermoplastic.
[0022] In some embodiments, the resin may include one or more hydrocarbon resins, liquids, and waxes of rubber. Example hydrocarbon resins include saturated and unsaturated rubber compounds. Example saturated rubber compounds include ethylene-propylene rubber, polyethylene / butylene, polyethylene-butylene-styrene, polyethylene-propylene-styrene, hydrogenated polyalkyl diene monools, hydrogenated polyalkyl diene diols, hydrogenated polyisoprene, and polyolefin elastomers.
[0023] In some embodiments, silyl-modified resins can be used in the matrix of the present invention. The resin is preferably non-silicone, wherein the composition does not contain more than trace amounts of silicone. In some embodiments, the composition does not contain silicone. The silyl-modified polymer can have a flexible backbone for lower modulus and glass transition temperature, such as a backbone of a polyether, polyester, polyurethane, polyacrylate, polyisoprene, polybutadiene, polystyrene-butadiene or polybutylene isoprene.
[0024] In some embodiments, resin can include one or more pressure-sensitive adhesives. As used herein, the term "pressure-sensitive adhesive" or "PSA" refers to a viscoelastic material that adheres to most substrates instantaneously and remains permanently tacky when applying slight pressure. If a polymer has the characteristics of PSA itself or acts as PSA by mixing with a diluent and other additives, the polymer is a PSA within the meaning of the term used in this article. Example pressure-sensitive adhesives include block copolymers (such as styrene copolymers described above), tackifying resins and plasticizers. Pressure-sensitive adhesives can have certain rheological characteristics useful for the present composition, including a combination of low softening point and low melt viscosity and high cohesive strength. Due to the low viscosity at low application temperatures, the adhesive resin component can be suitable for the application method in which the coating equipment contacts the coated substrate, such as in the case of screen printing and groove roller coating.
[0025] The resin may be present in an amount ranging from about 0.1 to about 50 weight percent of the total composition; in some embodiments, the resin may be present in an amount ranging from about 0.5 to about 20 weight percent of the total composition; in some embodiments, the resin may be present in an amount ranging from about 0.5 to about 10 weight percent of the total composition; in some embodiments, the resin may be present in an amount ranging from about 0.5 to about 5 weight percent of the total composition; in some embodiments, the resin may be present in an amount ranging from 1 to 3 weight percent of the total composition.
[0026] Antioxidant Phase Change Materials
[0027] The compositions of the present invention are preferably phase-changing because they include a phase-changing material having a melting point temperature or temperature range at or below the operating temperature or temperature range of the electronic component to which the thermally conductive material can be thermally coupled. The temperature-activated phase-changing material preferably changes from a solid to a liquid and from a liquid to a solid at a temperature range of about 30°C to about 160°C, and more preferably at a temperature range of 40°C to 85°C. The phase-changing materials used in conventional compositions typically include materials such as natural waxes (such as beeswax or carnuba wax), petroleum-based waxes (such as paraffin), or synthetic waxes (such as polyethylene glycol, polyethylene, polyols, or chlorinated naphthalenes).
[0028] An exemplary conventional phase change material is a wax, such as paraffin. Paraffin is a wax having the general formula C n H 2n+2 A mixture of solid hydrocarbons having a melting point in the range of about 40°C to about 140°C (and more preferably in the range of 40°C to 80°C). Polymer waxes include polyethylene waxes and polypropylene waxes and generally have a melting point range of about 40°C to about 160°C.
[0029] As described herein, conventional phase change materials such as waxes tend to degrade at high temperatures often experienced in modern electronic packaging. Applicants have discovered that by replacing some or all of the conventional phase change materials with low melting point secondary antioxidants, high performance phase change thermally conductive compositions can be obtained. Although secondary antioxidants are used in thermal materials, this is believed to be a new approach to using secondary antioxidants to drive phase change behavior in thermally conductive compositions. Such low melting point secondary antioxidants have been found to both provide a phase change effect in thermally conductive compositions and improve the high temperature reliability of such compositions.
[0030] In some embodiments, the phase change antioxidant component is a secondary antioxidant used in combination with the primary antioxidant and compatible therewith. The secondary antioxidant decomposes hydroperoxides to produce non-reactive products, thereby avoiding the proliferation of alkoxy and hydroxyl radicals, thereby delaying oxidation. The primary antioxidant works by providing its active hydrogen to the peroxy radical so that the growth of subsequent free radicals does not occur. The antioxidant free radical becomes stable by electron delocalization. In some embodiments, the secondary antioxidant is based on thiol, such as thioester. An exemplary thiol-based secondary antioxidant is 3,3'-thiodipropionic acid didodecyl ester, which has a melting point temperature of 40 to 85°C. In some embodiments, the compatible primary antioxidant is a phenolic antioxidant. Phenolic antioxidants include simple phenols, bisphenols, polyphenols and thiobisphenols.
[0031] It has been found that the concentration of the secondary antioxidant within the concentration range of the thermally conductive composition is important to maintaining the functionality of the composition, and in particular the relative concentration of the secondary antioxidant to the resin. Preferably, the secondary antioxidant is present in the composition at a concentration of 20 to 50% by weight of the non-silicone resin. Although the secondary antioxidant may preferably have a melting point temperature of 40 to 85°C to suitably act as a phase change component, the secondary antioxidant may more preferably have a melting point temperature of 50 to 60°C.
[0032] The secondary antioxidant may be present in the composition at a ratio of 95 to 99 parts by weight of the secondary antioxidant to 1 to 5 parts by weight of the primary antioxidant. In some embodiments, the secondary antioxidant may be present in the composition at a ratio of 97 to 99 parts by weight of the secondary antioxidant to 1 to 3 parts by weight of the primary antioxidant.
[0033] In some embodiments, the thermally conductive composition of the present invention is substantially free of a wax component. However, in other embodiments, the thermally conductive composition comprises a wax component. In some embodiments, the wax component is a hydrocarbon wax. In some embodiments, the melting point temperature of the hydrocarbon wax is 40 to 120°C. In some embodiments, the melting point temperature of the hydrocarbon wax is 40 to 80°C. In some embodiments, the hydrocarbon wax is paraffin wax.
[0034] Thermally conductive particles
[0035] In order to achieve the desired low thermal impedance of the thermally conductive interface, the composition of the present invention comprises thermally conductive particles dispersed therein. The particles can be both thermally conductive and electrically conductive. Alternatively, the particles can be thermally conductive but electrically insulating. Various thermally conductive particles can be used in the composition of the present invention. However, it has been found that thermally conductive particles selected from aluminum, aluminum nitride, aluminum silicon dioxide alloys, zinc oxide, and combinations thereof may be most useful in the composition of the present invention.
[0036] The granular filler material may have the form of a granular powder, whiskers, fibers, or any other suitable form. The particles may be generally spherical, plate-like, rod-like, or a combination thereof. In some embodiments, the thermally conductive particles may have a particle size of less than 25 μm, wherein the term "particle size" refers to a particle diameter or an effective particle diameter. In some embodiments, the thermally conductive particles may have a particle size of 0.01 to 25 μm. In some embodiments, the thermally conductive particles may be monodisperse.
[0037] In some embodiments, the thermally conductive particles may include one or more materials and may have a particle size distribution having particles with a particle size of 0.01 to 25 μm.
[0038] In some embodiments, the particle size distribution may be multimodal, having more than one concentration peak with a particle size of 0.01 to 25 μm. In some embodiments, the first concentration peak of the multimodal distribution is a particle size of 0.1 to 3 μm, and the second concentration peak of the multimodal distribution is a particle size of 8 to 12 μm. The first concentration peak of the multimodal distribution may account for 10 to 90% by weight of the total thermally conductive filler; in some embodiments, the first concentration peak of the multimodal distribution may account for 15 to 80% by weight of the total thermally conductive filler; in some embodiments, the first concentration peak of the multimodal distribution may account for 15 to 50% by weight of the total thermally conductive filler; in some embodiments, the first concentration peak of the multimodal distribution may account for 15 to 30% by weight of the total thermally conductive filler. The second concentration peak of the multimodal distribution may account for 10 to 90% by weight of the total thermally conductive filler; in some embodiments, the second concentration peak of the multimodal distribution may account for 15 to 80% by weight of the total thermally conductive filler; in some embodiments, the second concentration peak of the multimodal distribution may account for 25 to 60% by weight of the total thermally conductive filler. A multimodal distribution may include more than two particle size concentration peaks.
[0039] In some embodiments, the thermally conductive particulate filler may include a trimodal particle size distribution with a particle size of 0.01 to 25 μm. The first concentration peak of the trimodal distribution is an aluminum nitride particle size of 0.1 to 3 μm, the second concentration peak of the trimodal distribution is an aluminum or aluminum-silicon dioxide alloy (silicon dioxide stabilized aluminum) particle size of 8 to 12 μm, and the third concentration peak of the trimodal distribution is a zinc oxide particle size of 0.01 to 0.5 μm. The first concentration peak of the trimodal distribution accounts for 15 to 35% by weight of the total thermally conductive filler. The second concentration peak accounts for 25 to 60% by weight of the total thermally conductive filler. The third concentration peak accounts for 15 to 35% by weight of the total thermally conductive filler.
[0040] The thermally conductive particulate filler may comprise at least 25 wt % aluminum and / or aluminum-silica alloy particles, preferably at least 35 wt % aluminum and / or aluminum-silica alloy particles, and more preferably at least 40 wt % aluminum and / or aluminum-silica alloy particles.
[0041] In some embodiments, the particle size described above may represent an average particle diameter (d 50 ).
[0042] Thermally conductive particulate fillers can be dispersed in the resin and present in the composition at a loading concentration of 20 to 98% by weight of the total composition. In some embodiments, the thermally conductive filler-like filler accounts for 40 to 97% by weight of the total composition. In some embodiments, the thermally conductive filler-like filler accounts for 50 to 95% by weight of the total composition. It is desirable to provide enough thermally conductive particles so that the thermally conductive interface formed by the composition exhibits a thermal conductivity of at least 0.5 W / m*K, preferably at least 1 W / m*K, and more preferably at least 2 W / m*K.
[0043] Plasticizers
[0044] The thermally conductive composition of the present invention may include a plasticizer component to adjust the viscosity of the dispensable material, particularly under shear, and to maintain a solid state and maintain the melt viscosity within a desired range. Plasticizers that can be used in the composition of the present invention are those that are effective in promoting the fluency of the cohesive material constituting the composition. The plasticizer used in the composition of the present invention may preferably be a low volatility liquid that reduces the viscosity of the composition. In some embodiments, the plasticizer may exhibit a viscosity of less than 1000 cP at 25°C. In another embodiment, the plasticizer may exhibit a viscosity of less than 500 cP at 25°C. In yet another embodiment, the plasticizer may exhibit a viscosity of less than 100 cP at 25°C.
[0045] In some embodiments, the plasticizer may comprise from about 0.1 to about 25 weight % of the composition. In some embodiments, the plasticizer may comprise from about 0.5 to about 10 weight % of the composition. In some embodiments, the plasticizer may comprise from about 0.5 to about 5 weight % of the composition. The plasticizer may preferably be present in an amount less than 20 weight % of the composition.
[0046] Exemplary plasticizers include sebacates, adipates, terephthalates, dibenzoates, gluterates, phthalates, azelates, benzoates, sulfonamides, organic phosphates, glycols, polyethers, trimellitates, polybutadiene, epoxies, amines, acrylates, thiols, polyols, and isocyanates. Preferred plasticizers are trimellitates.
[0047] Antioxidant supplementation
[0048] In addition to the primary and secondary antioxidants described above, the compositions of the present invention may also include additional antioxidant components that are functionally complementary to the primary and secondary antioxidants, but different from the primary and secondary antioxidants described above. In some embodiments, the compositions of the present invention may include one or more supplementary primary and secondary antioxidants that are different from the primary and secondary antioxidants described above. Typical supplementary antioxidants include hindered phenols and aromatic secondary amines. Exemplary sterically hindered phenols that can be used as supplementary antioxidants in the compositions of the present invention are BASF Corporation's 1010. Metal-passivating antioxidants may also be used in the compositions of the present invention, examples of which are available from BASF Corporation. MD 1024.
[0049] In some embodiments, the thermally conductive compositions of the present invention may include one or more supplemental antioxidants at a concentration of 0.01 to 10% by weight of the composition. In some embodiments, the thermally conductive compositions of the present invention may include one or more supplemental antioxidants at a concentration of 0.05 to 5% by weight of the composition. In some embodiments, the thermally conductive compositions of the present invention may include one or more supplemental antioxidants at a concentration of 0.1 to 3% by weight of the composition.
[0050] Optional additives
[0051] According to some embodiments of the present invention, the compositions described herein may further comprise one or more additives, such as stabilizers, dispersants, colorants, binders, wetting agents, flame retardants, extenders, and corrosion inhibitors.
[0052] Thermally Conductive Composition Properties
[0053] In a preferred embodiment, the thermally conductive composition exhibits a thermal conductivity of at least 0.5 W / m*K, preferably at least 1 W / m*K, and more preferably at least 2 W / m*K. In addition, the thermally conductive composition exhibits high temperature stability, experiencing less than a 20% weight loss after 1000 hours at 175°C, and preferably less than a 10% weight loss after 1000 hours at 175°C. The thermally conductive composition preferably experiences less than a 10% drop in thermal properties (e.g., thermal conductivity or thermal impedance) after 1000 hours at 175°C, and more preferably less than a 5% drop in thermal properties after 1000 hours at 175°C.
[0054] Products
[0055] The thermally conductive composition of the present invention can be used to prepare articles of various shapes. The article can be used as an interface between a heating device and a heat dissipation device. The heating device effectively transfers heat to the interface article, so that the interface article melts at an operating temperature below 120°C, and more often below 85°C. When the phase change material melts, it forms a liquid film at the contact surface of the interface article, the electronic component, and the heat sink. The film containing the phase change material reduces the thermal impedance of the contact surface. The resin matrix of the thermally conductive interface provides a network for accommodating the liquid phase change material and prevents it from flowing out of the interface.
[0056] The composition can be melt extruded into a film with low thickness. In contrast, conventional films made from silicone-based filler compositions are usually much thicker. It has been found that for some applications, non-silicone resin films can be more advantageous relative to silicone forms. For example, silicone films tend to have poor handling characteristics and may require a supporting structure to maintain integrity. In addition, silicone resins and particulate filler materials may be incompatible because their densities are different and the viscosity of silicone resins is relatively low. Therefore, the composition of the present invention is preferably non-silicone.
[0057] Printable composition
[0058] In some embodiments, the thermally conductive composition of the present invention can be printed by conventional printing equipment (e.g., inkjet printers, filament printers, and other three-dimensional printers). In some embodiments, the composition of the present invention can be melt-extruded by a print head or die. In other embodiments, the composition of the present invention can be dissolved or suspended in a solvent or suspending fluid and then dispensed through a suitable nozzle or slot. Solvent-based printing can be implemented by printing the solution or suspension / dispersion onto a substrate, followed by drying the solvent at or above room temperature and / or under reduced pressure. Although a variety of solvents are contemplated for this purpose, acetate-based solvents such as ethyl acetate and ethylhexyl acetate are suitable solvents.
[0059] Example
[0060] The following compositions were prepared and exhibited the thermally conductive composition properties described herein.
[0061] Embodiment 1:
[0062]
[0063] Embodiment 2:
[0064]
Claims
1. A thermally conductive composition comprising: 0.5 to 20 wt. % of a non-silicone resin; Primary antioxidant; a thiol-based secondary antioxidant that is compatible with the primary antioxidant and is present in the composition at a concentration of 20 to 50% by weight of the non-silicone resin, the secondary antioxidant also being present in the composition at a ratio of 95 to 99 parts by weight of the secondary antioxidant to 1 to 5 parts by weight of the primary antioxidant, the secondary antioxidant having a melting point temperature of 40 to 85°C; and 50 to 98% by weight of a thermally conductive particulate filler, The thermally conductive composition exhibits a thermal conductivity of at least 1 W / m*K and a loss of less than 20 wt % after 1000 hours at 175°C. 2 . The thermally conductive composition of claim 1 , wherein the non-silicone resin comprises a pressure sensitive adhesive. 3 . The thermally conductive composition according to claim 1 , comprising 0.5 to 5 wt % of the non-silicone resin.
4. The thermally conductive composition of claim 3, wherein the non-silicone resin comprises a polyamide. 5 . The thermally conductive composition according to claim 1 , comprising a hydrocarbon wax having a melting point temperature of 40 to 120° C.
6. The thermally conductive composition of claim 1, wherein the composition is substantially free of wax. 7 . The thermally conductive composition of claim 1 , wherein the secondary antioxidant has a melting point temperature of 50 to 60° C.
8. The thermally conductive composition of claim 1, wherein the secondary antioxidant comprises dodecylthiopropionate.
9. The thermally conductive composition of claim 1, wherein the thermally conductive particulate filler is selected from the group consisting of aluminum, aluminum nitride, aluminum silica alloy, zinc oxide, and combinations thereof.
10. The thermally conductive composition according to claim 9, wherein the average particle size (d 50 ) is less than 25μm.
11. The thermally conductive composition according to claim 10, comprising 70 to 95 wt% of the thermally conductive particulate filler.
12. The thermally conductive composition of claim 1, comprising 0.5 to 20 wt% of a trimellitate plasticizer.
13. The thermally conductive composition of claim 12, comprising 0.5 to 5 wt% of a trimellitate plasticizer.
14. The thermally conductive composition of claim 13, comprising 0.1 to 1.5 wt% of a wetting agent. 15 . The thermally conductive composition according to claim 14 , comprising 0.1 to 1.5 wt % of a sterically hindered phenolic antioxidant different from the primary antioxidant and the auxiliary antioxidant.
16. The thermally conductive composition of claim 15, comprising 0.1 to 1.5 wt% of a metal deactivator antioxidant different from the primary antioxidant and the secondary antioxidant.
17. A thermally conductive printable composition comprising: The thermally conductive composition according to claim 1 dissolved in a compatible solvent.
18. The thermally conductive printable composition according to claim 17, wherein the solvent is selected from ethyl acetate and ethylhexyl acetate.