Polyester-based adhesive composition, polyester-based adhesive, adhesive sheet, decorative film, film for electronic component, and decorative molded article

By introducing polycarboxylic acids and polyols with specific structures into the polyester resin and crosslinking them with polyepoxy compounds, the adhesion and heat resistance of polyester-based adhesives in high temperature and humid and heat environments are solved. The problem of difficulty in taking into account both the properties and optical properties has been realized, and a high-performance polyester-based adhesive composition is realized.

CN118891337APending Publication Date: 2024-11-01MITSUBISHI CHEM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380025501.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing polyester-based adhesives are difficult to take into account the adhesion, heat resistance and optical properties in high temperature and humid environments, especially in decorative molded bodies with complex surface shapes, which have problems such as thermal decomposition and reduced transparency of the adhesive. .

Method used

By using a polyester-based resin having a specific acid value and a glass transition temperature, cross-linking is carried out in combination with a polyepoxy compound to form a polyester-based system containing polycarboxylic acids and aliphatic polyols derived from a ring-containing structure. Adhesive composition, optimize the structure of the adhesive to improve adhesion, heat resistance and optical properties.

Benefits of technology

It achieves excellent performance in adhesive strength, heat resistance and optical properties in high temperature and humid environments, and is suitable for adhesive applications of decorative molded bodies and electronic components with complex surface shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027178150000401
    Figure BDA0005027178150000401
  • Figure BDA0005027178150000411
    Figure BDA0005027178150000411
  • Figure BDA0005027178150000471
    Figure BDA0005027178150000471
Patent Text Reader

Abstract

Provided is a polyester-based adhesive composition which is capable of forming an adhesive having excellent adhesive strength, heat resistance, wet heat resistance, and optical characteristics, and which contains a polyester-based resin (A) and a polyepoxy-based compound (B), the polyester-based resin (A) containing a structural unit derived from a polycarboxylic acid and a structural unit derived from a polyhydric alcohol, and the polyepoxy-based compound (B) containing a structural unit derived from a polyhydric alcohol and a structural unit derived from a polyhydric alcohol and a structural unit derived from a polyhydric alcohol and a structural unit derived from a polyhydric alcohol and a structural unit derived from a polyhydric alcohol. The structural unit derived from the polycarboxylic acid contains a specific amount of a structural unit derived from a cyclic structure, the structural unit derived from the polyol contains a structural unit derived from an aliphatic polyol, and the polyester resin (A) further has a specific acid value and glass transition temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyester adhesive composition, a polyester adhesive, an adhesive sheet, a decorative film, a film for electronic components and a decorative molded body, and more specifically, to a polyester adhesive composition having excellent adhesive strength, heat resistance, moisture-heat resistance and optical properties, an adhesive formed by crosslinking the adhesive composition, and an adhesive sheet having an adhesive layer containing the adhesive.

[0002] The present invention also relates to a decorative film formed of the pressure-sensitive adhesive sheet and a decorative molded body formed by laminating the decorative films. Background Art

[0003] Conventionally, polyester resins have been widely used in films, plastic bottles, fibers, toner cartridges, motor parts, adhesives, and binders due to their excellent heat resistance, chemical resistance, durability, and mechanical strength. In addition, polyester resins have high polarity due to their polymer structure, and are known to exhibit excellent adhesion to polar polymers such as polyester, polyvinyl chloride, polyimide, and epoxy resins, as well as metal materials such as copper and aluminum.

[0004] In addition, in molded products such as automobile interior and exterior parts, home appliance parts, and building material parts, a decorative film is applied or a transferred decorative film is applied as a substitute for the previous coating method in order to improve the appearance and suppress the discharge of VOC (Volatile Organic Compounds). As a molding method based on the decorative film, in-mold molding based on injection molding, vacuum molding, vacuum pressure molding, etc. can be used. In addition, as a decorative film attached to the molded product, a decorative film with an adhesive layer is known.

[0005] Patent Document 1 proposes a thermoplastic polyester elastomer as a thermoplastic polyester elastomer having excellent moldability, water resistance and weather resistance, wherein the thermoplastic polyester elastomer is a copolyester in which the acid component is mainly an aromatic dicarboxylic acid and the diol component contains 1 to 60 mol % of dimer alcohol relative to the total diol components, and the reduced viscosity of the thermoplastic polyester elastomer is 0.5 to 3.0.

[0006] In addition, Patent Document 2 proposes a polyester-based adhesive composition that has little change over time such as an increase in adhesive strength even when used in a high-temperature environment, characterized in that it contains a polyester resin having a carboxyl group derived from at least one of a trivalent or higher carboxylic acid and an anhydride thereof in at least one of the side chain and the end of the molecule.

[0007] In addition, Patent Document 3 proposes an adhesive composition as a polyester having excellent solvent solubility, heat resistance, low viscosity, low relative dielectric constant and dielectric loss tangent, and excellent dielectric properties, wherein the adhesive composition contains 50 mol% or more of a naphthalene dicarboxylic acid component when the polycarboxylic acid component is set to 100 mol%, and contains at least one of a dimer alcohol component and tricyclodecane dimethanol as a polyol component.

[0008] Patent document 4 proposes an adhesive composition having excellent long-term durability in a hot and humid environment and further high adhesion, which contains a polyester resin that meets the requirements of an ester bond concentration of less than 7 mmol / g, an acid value of more than 3 mgKOH / g, and a glass transition temperature of more than -5°C.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 6-128363

[0012] Patent Document 2: Japanese Patent Application Publication No. 2019-119872

[0013] Patent Document 3: International Publication No. 2021 / 200713

[0014] Patent Document 4: Japanese Patent Application Publication No. 2020-134344 Summary of the invention

[0015] Problem that the invention aims to solve

[0016] However, in recent years, the decorative molding of molded bodies with complex surface shapes such as three-dimensional curved surfaces has been required, and sometimes the molding is performed at a higher temperature than before. In this case, there are issues such as heat resistance such as thermal decomposition of the adhesive used in the decorative film, and issues such as reduced transparency of the adhesive layer. Usually, when improving heat resistance, the glass transition temperature of the resin is considered to be increased, but on the other hand, there are problems such as the resin hardening and reduced adhesion and optical properties, making it difficult to achieve these properties at a high level.

[0017] For example, Patent Document 1 discloses a technology related to a polyester elastomer. The polyester resin has high crystallinity, so its viscosity at room temperature (23° C.) is low and it is difficult to use it for adhesive applications. In addition, since the polyester resin is not given an acid value that becomes a reaction point with a polyepoxy compound, heat resistance is not considered.

[0018] In addition, Patent Document 2 discloses a polyester adhesive for masking, which has excellent heat resistance but has a high acid value of the polyester resin that serves as a crosslinking point with the polyepoxy compound, and thus has a problem of high crosslinking density and extremely low adhesive force. In addition, moisture and heat resistance is not considered, and long-term durability in a moisture and heat environment still needs to be improved.

[0019] Patent Document 3 relates to a disclosed technology of polyester with excellent dielectric properties. In order to reduce the dielectric constant, dielectric loss tangent and water absorption, a large amount of polycyclic polycarboxylic acid with high crystal orientation is included in the polycarboxylic acid, so that the glass transition temperature becomes high, and the viscosity and molding stability when the adhesive sheet is made remain problems. In addition, since a large amount of polyols with long-chain alkyl groups with low polarity are included in the polyols, there are problems such as poor solubility in polar solvents, long-term stability of the resin solution, low compatibility with polyepoxides, etc., and low optical properties.

[0020] Patent Document 4 discloses a technology related to a polyester-based adhesive. However, since the polyester-based resin has a high glass transition temperature and low viscosity at room temperature (23° C.), it is difficult to use it for adhesive applications.

[0021] Therefore, under such background, the present invention provides a polyester-based adhesive composition having excellent adhesive strength, heat resistance, moisture-heat resistance, and optical properties, and an adhesive, an adhesive sheet, a decorative film, a film for electronic components, and a decorative molded body obtained by crosslinking the adhesive composition.

[0022] Solutions for solving problems

[0023] However, in view of these circumstances, the inventors of the present invention have conducted intensive studies and have found that by cross-linking a polyester resin having a specific acid value and glass transition temperature and containing structural units derived from polycarboxylic acids containing a cyclic structure and structural units derived from aliphatic polyols with a polyepoxy compound, a polyester adhesive composition having a low glass transition temperature and excellent adhesion as well as excellent heat resistance, moisture-heat resistance, and optical properties, which have conventionally been a compromise, can be obtained.

[0024] That is, the present invention takes the following [1] to

[21] as its gist.

[0025] [1] A polyester adhesive composition comprising a polyester resin (A) and a polyepoxy compound (B),

[0026] The polyester resin (A) satisfies all of the following conditions (1) to (6):

[0027] (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b).

[0028] (2) The content of the structural unit derived from the cyclic structure-containing polycarboxylic acid (a1) is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a).

[0029] (3) The structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1).

[0030] (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g.

[0031] (5) The glass transition temperature of the polyester resin (A) is -75 to -20°C.

[0032] (6) The structural unit derived from the cyclic ester in the polyester resin (A) accounts for less than 140 mol % based on 100 mol % of the structural unit derived from the polycarboxylic acid (a).

[0033] [2] The polyester adhesive composition according to [1], wherein the structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is a structural unit derived from a monocyclic polycarboxylic acid (a1-1).

[0034] [3] The polyester adhesive composition according to [1] or [2], wherein the structural unit derived from the aliphatic polyol (b1) contains a structural unit derived from a polyol having a hydrocarbon group in at least one side chain.

[0035] [4] The polyester adhesive composition according to any one of [1] to [3], wherein the polyester resin (A) has a structural unit derived from a dimer acid (a2) and / or a structural unit derived from a dimer alcohol (b2).

[0036] [5] The polyester adhesive composition according to any one of [1] to [4], wherein the content of the structural unit derived from the aliphatic polyol (b1) is 5 to 80 mol% relative to 100 mol% of the structural unit derived from the polyol (b).

[0037] [6] The polyester adhesive composition according to any one of [1] to [5], wherein the structural unit derived from the polyol (b) contains a structural unit derived from a dimer alcohol (b2).

[0038] [7] The polyester adhesive composition according to any one of [1] to [6], wherein the total content of the structural units derived from the dimer acid (a2) and the structural units derived from the dimer alcohol (b2) is 20 to 90% by mass relative to the total amount of the polyester resin (A).

[0039] [8] The polyester adhesive composition according to any one of [1] to [7], wherein the polyester resin (A) has an ester bond concentration of 1.5 to 8.0 mmol / g.

[0040] [9] The polyester adhesive composition according to any one of [1] to [8], wherein the crystal fusion heat of the polyester resin (A) is 3 J / g or less.

[0041]

[10] The polyester adhesive composition according to any one of [1] to [9], wherein the polyepoxy compound (B) contains a nitrogen atom-containing polyepoxy compound.

[0042]

[11] The polyester adhesive composition according to any one of [1] to

[10] , wherein the equivalent weight of the epoxy group of the polyepoxy compound (B) relative to the carboxyl group of the polyester resin (A) is 0.3 to 5 equivalents.

[0043]

[12] The polyester adhesive composition according to any one of [1] to

[11] , wherein the content of the polyepoxy compound (B) is 0.1 to 15 parts by mass relative to 100 parts by mass of the polyester resin (A).

[0044]

[13] A polyester-based adhesive obtained by crosslinking the adhesive composition according to any one of [1] to

[12] .

[0045]

[14] The polyester-based adhesive according to

[13] , which has a gel fraction of 20 to 100%.

[0046]

[15] A PSA sheet comprising a PSA layer comprising the PSA according to

[13] or

[14] .

[0047]

[16] The pressure-sensitive adhesive sheet according to

[15] , which has a haze of 3% or less.

[0048]

[17] A pressure-sensitive adhesive sheet comprising a substrate and a pressure-sensitive adhesive layer comprising the polyester pressure-sensitive adhesive according to

[13] or

[14] , wherein the pressure-sensitive adhesive layer is provided on at least one surface of the substrate.

[0049]

[18] A decorative film comprising the pressure-sensitive adhesive sheet according to

[17] .

[0050]

[19] A film for electronic components, comprising the pressure-sensitive adhesive sheet according to

[17] .

[0051]

[20] A decorative molded body, comprising laminating the decorative film according to

[18] on a molded body.

[0052]

[21] A decorative film comprising an adhesive layer formed from a polyester adhesive composition containing a polyester resin (A) and a polyepoxy compound (B),

[0053] The polyester resin (A) satisfies all of the following conditions (1) to (4):

[0054] (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b).

[0055] (2) The content of the structural unit derived from the cyclic structure-containing polycarboxylic acid (a1) is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a).

[0056] (3) The structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1).

[0057] (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g.

[0058] Effects of the Invention

[0059] The polyester-based adhesive composition of the present invention can form an adhesive having excellent adhesive strength, heat resistance, moisture and heat resistance, and optical properties. In particular, such an adhesive composition is effective as an adhesive used in decorative films and films for electronic components.

[0060] Generally, it is known that the glass transition temperature of polyester resin is increased or functional groups are added to increase the crosslinking points in order to improve the heat resistance and moisture-heat resistance of polyester adhesive compositions. However, in the present invention, a polyester resin having a specific acid value and glass transition temperature and containing structural units derived from aliphatic polyols that can reduce durability in addition to structural units derived from polycarboxylic acids containing a cyclic structure is crosslinked with a polyepoxy compound, so that the polyester adhesive composition has a low glass transition temperature, is viscous at room temperature (23° C.), has excellent adhesive strength, and has excellent heat resistance, moisture-heat resistance, and optical properties, which have been a compromise relationship in the past. DETAILED DESCRIPTION

[0061] Hereinafter, the configuration of the present invention will be described in detail, but these are merely examples of preferred embodiments.

[0062] It should be noted that in the present invention, the "class" attached after the compound name is a concept that includes not only the compound but also the derivatives of the compound. For example, the term "carboxylic acid class" includes not only carboxylic acids but also carboxylic acid derivatives such as carboxylates, carboxylic anhydrides, carboxylic acid halides, and carboxylic acid esters.

[0063] Furthermore, “X and / or Y (X and Y are arbitrary structures)” means at least one of X and Y, and has three meanings of only X, only Y, and X and Y.

[0064] The polyester adhesive composition according to one embodiment of the present invention (hereinafter sometimes referred to as "the present adhesive composition") contains a polyester resin (A) and a polyepoxy compound (B), wherein the polyester resin (A) satisfies all of the following conditions (1) to (6).

[0065] (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b).

[0066] (2) The content of the structural unit derived from the cyclic structure-containing polycarboxylic acid (a1) is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a).

[0067] (3) The structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1).

[0068] (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g.

[0069] (5) The glass transition temperature of the polyester resin (A) is -75 to -20°C.

[0070] (6) The structural unit derived from the cyclic ester in the polyester resin (A) accounts for less than 140 mol % based on 100 mol % of the structural unit derived from the polycarboxylic acid (a).

[0071] Hereinafter, each component contained in this adhesive composition is demonstrated.

[0072] <Polyester resin (A)>

[0073] The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b) in the molecule, and is preferably a polyester resin obtained by ester-bonding the polycarboxylic acid (a) and the polyol (b).

[0074] [Polycarboxylic acids (a)]

[0075] Examples of the polycarboxylic acid (a) include: polycarboxylic acids (a1) containing a cyclic structure such as monocyclic polycarboxylic acids and polycyclic polycarboxylic acids; dimer acids (a2); trivalent or higher polycarboxylic acids having 0 or 1 anhydride groups; and aliphatic polycarboxylic acids.

[0076] In the present invention, the polyester resin (A) contains a structural unit derived from a polycarboxylic acid (a1) containing a cyclic structure from the viewpoint of moist heat resistance. The polycarboxylic acid (a1) can be used alone or in combination of two or more.

[0077] Relative to 100 mol% of the structural unit derived from polycarboxylic acid (a), the content of the structural unit derived from polycarboxylic acid (a1) containing cyclic structure is 30 mol% or more, preferably 40-99 mol%, more preferably 50-95 mol%, particularly preferably 55-90 mol%, and particularly preferably 60-85 mol% or more. The upper limit is usually 100 mol%. If the content of the structural unit derived from polycarboxylic acid (a1) containing cyclic structure is too little, heat resistance and resistance to moisture and heat become insufficient. In addition, if the content is too much, the compatibility with polyepoxy compound (B) is reduced and optical properties become insufficient or the glass transition temperature becomes high and viscosity, adhesive force, and molding stability become insufficient.

[0078] The content (molar ratio) of the structural unit derived from the polycarboxylic acid (a1) having a cyclic structure relative to 100 mol % of the structural unit derived from the polycarboxylic acid (a) can be determined by the following formula.

[0079] Content of structural units derived from polycarboxylic acids containing a cyclic structure (a1) (mol%) = (content of structural units derived from polycarboxylic acids containing a cyclic structure (a1) (mol) / content of structural units derived from polycarboxylic acids (a) (mol)) × 100

[0080] In addition, the content of the structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is preferably 3 to 50% by mass, more preferably 5 to 40% by mass, further preferably 7 to 35% by mass, particularly preferably 10 to 30% by mass, and particularly preferably 15 to 25% by mass relative to the entire polyester resin (A). If the content of the structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is too small, there is a tendency that heat resistance and moist heat resistance become insufficient, and if it is too large, there is a tendency that compatibility with the polyepoxy compound (B) decreases and optical properties become insufficient, or the glass transition temperature becomes high and viscosity, adhesive force, and molding stability become insufficient.

[0081] Examples of the polycarboxylic acid (a1) containing a cyclic structure include monocyclic polycarboxylic acids (a1-1), polycyclic polycarboxylic acids (a1-2), etc. Among them, from the viewpoint of excellent adhesive force, molding stability, and optical properties, it is preferred that the polycarboxylic acid (a1) containing a cyclic structure contains a monocyclic polycarboxylic acid (a1-1), and it is particularly preferred that the polycarboxylic acid (a1) containing a cyclic structure is a monocyclic polycarboxylic acid (a1-1).

[0082] Examples of the monocyclic polycarboxylic acid (a1-1) include aromatic monocyclic dicarboxylic acids such as terephthalic acid, isophthalic acid, and phthalic acid; and alicyclic monocyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,2-cyclohexanedicarboxylic acid.

[0083] Furthermore, the monocyclic polycarboxylic acid (a-1) also includes trifunctional or higher monocyclic polycarboxylic acids introduced for the purpose of imparting a branched skeleton and an acid value to the polyester resin (A). Examples of the trifunctional or higher monocyclic polycarboxylic acids include trimellitic acid, pyromellitic acid, and pyromellitic acid.

[0084] Among the monocyclic polycarboxylic acids (a1-1), monocyclic aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid and phthalic acid are preferred from the viewpoint of excellent heat resistance and moisture-heat resistance. Terephthalic acid and isophthalic acid are particularly preferred. Isophthalic acid is further preferred from the viewpoint of reducing the crystallinity of the polyester resin (A), excellent stability after solvent dissolution, and excellent viscosity and adhesive strength.

[0085] In addition, the monocyclic polycarboxylic acid (a1-1) can also be classified into asymmetric monocyclic polycarboxylic acid and symmetric monocyclic polycarboxylic acid. From the viewpoint of reducing the crystallinity of the polyester resin (A), it is preferred that the polycarboxylic acid (a) contains asymmetric monocyclic polycarboxylic acid, and from the viewpoint of excellent solvent dissolution stability, it is preferred that the polycarboxylic acid (a) contains asymmetric monocyclic polycarboxylic acid and symmetric monocyclic polycarboxylic acid.

[0086] Examples of the asymmetric monocyclic polycarboxylic acids include isophthalic acids, phthalic acids, 1,3-cyclohexanedicarboxylic acids, and 1,2-cyclohexanedicarboxylic acids. Among them, isophthalic acids are particularly preferred from the viewpoint of excellent reactivity and adhesive strength.

[0087] Examples of the symmetrical monocyclic polycarboxylic acids include terephthalic acids and 1,4-cyclohexanedicarboxylic acids.

[0088] When the polyester resin (A) contains a structural unit derived from a monocyclic polycarboxylic acid (a1-1), the content of the structural unit derived from the monocyclic polycarboxylic acid (a1-1) is preferably 30 mol% or more, more preferably 40 to 98 mol%, further preferably 50 to 95 mol%, particularly preferably 55 to 90 mol%, and particularly preferably 60 to 85 mol%, relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a). If the content of the structural unit derived from the monocyclic polycarboxylic acid (a1-1) is too small, heat resistance and moist heat resistance tend to be insufficient, and if it is too large, compatibility with the polyepoxy compound (B) tends to be reduced, optical properties tend to be insufficient, or the glass transition temperature tends to be high, and viscosity, adhesive strength, and molding stability tend to be insufficient.

[0089] Furthermore, when an asymmetric monocyclic polycarboxylic acid and a symmetric monocyclic polycarboxylic acid are used as the monocyclic polycarboxylic acid (a1-1), the content ratio (molar ratio) in the polyester resin (A) is preferably structural units derived from asymmetric monocyclic polycarboxylic acids / structural units derived from symmetric monocyclic polycarboxylic acids = 30 / 70 to 100 / 0, more preferably 40 / 60 to 95 / 5, particularly preferably 45 / 55 to 90 / 10, further preferably 50 / 50 to 85 / 15, and particularly preferably 55 / 45 to 80 / 20.

[0090] In addition, from the viewpoint of heat resistance and moisture-heat resistance, the polycarboxylic acid (a1) containing a cyclic structure may also contain a polycyclic polycarboxylic acid (a1-2). Examples of the polycyclic polycarboxylic acid (a1-2) include polycyclic aromatic dicarboxylic acids such as biphenyl dicarboxylic acids, naphthalene dicarboxylic acids, and dimethyl naphthalene dicarboxylate.

[0091] When the polyester resin (A) contains a structural unit derived from a polycyclic polycarboxylic acid (a1-2), the content of the structural unit derived from the polycyclic polycarboxylic acid (a1-2) is preferably 50 mol% or less, more preferably 40 mol% or less, further preferably 30 mol% or less, particularly preferably 20 mol% or less, particularly preferably 10 mol% or less, and most preferably 5 mol% or less, relative to 100 mol% of the structural unit derived from the polycyclic polycarboxylic acid (a1), If the content of the structural unit derived from the polycyclic polycarboxylic acid (a1-2) is too much, there is a tendency that the transparency of the resin is reduced and the optical properties become insufficient, or the glass transition temperature becomes high and the viscosity, adhesive force, and molding stability become insufficient.

[0092] In addition, from the viewpoint of moisture-heat resistance and adhesive strength, the structural unit derived from the polycarboxylic acid (a) preferably contains a structural unit derived from a dimer acid (a2). Examples of the dimer acid (a2) include dimer acids derived from dimerization of unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, and erucic acid (mainly dimer acids having 36 to 44 carbon atoms), and hydrogenates thereof. Among them, hydrogenates are preferred from the viewpoint of suppressing gelation during the manufacture of polyester resins.

[0093] When the polyester resin (A) contains a structural unit derived from a dimer acid (a2), the content of the structural unit derived from a dimer acid (a2) is preferably 70 mol% or less, more preferably 3 to 60 mol%, further preferably 5 to 50 mol%, particularly preferably 10 to 45 mol%, and particularly preferably 15 to 40 mol%, relative to 100 mol% of the structural unit derived from a polycarboxylic acid (a). If the content of the structural unit derived from a dimer acid (a2) is too small, there is a tendency that the adhesive force and the moist heat resistance become insufficient, and if it is too large, there is a tendency that the compatibility with the polyepoxy compound (B) decreases, the optical properties become insufficient, or the solvent dissolution stability becomes insufficient.

[0094] In addition, when the polyester resin (A) contains a structural unit derived from a dimer acid (a2), the content of the structural unit derived from a dimer acid (a2) is preferably 3 to 80% by mass, more preferably 5 to 70% by mass, further preferably 10 to 60% by mass, particularly preferably 15 to 50% by mass, particularly preferably 20 to 40% by mass, and most preferably 30 to 45% by mass relative to the entire polyester resin (A). If the content of the structural unit derived from a dimer acid (a2) is too small, there is a tendency that the adhesive force and the moisture and heat resistance become insufficient, and if it is too large, there is a tendency that the compatibility with the polyepoxy compound (B) is reduced, the optical properties become insufficient, or the solvent dissolution stability becomes insufficient.

[0095] Furthermore, from the viewpoint of adhesive strength and molding stability, the structural unit derived from the polyvalent carboxylic acid (a) may contain a structural unit derived from an aliphatic polyvalent carboxylic acid.

[0096] Examples of the aliphatic polycarboxylic acids include malonic acid, dimethylmalonic acid, succinic acid, glutaric acid, adipic acid, trimethyl adipic acid, pimelic acid, 2,2-dimethylglutaric acid, azelaic acid, sebacic acid, fumaric acid, maleic acid, itaconic acid, thiodipropionic acid, diglycolic acid, 1,9-nonane dicarboxylic acid, etc. These may be used alone or in combination of two or more. Among them, adipic acid, sebacic acid, and azelaic acid are particularly preferred from the viewpoint of lowering the glass transition temperature, excellent adhesion and molding stability, and excellent optical properties of the resin.

[0097] When the polyester resin (A) contains a structural unit derived from an aliphatic polycarboxylic acid, the content of the structural unit derived from the aliphatic polycarboxylic acid is preferably 70 mol% or less, more preferably 3 to 60 mol%, further preferably 5 to 50 mol%, particularly preferably 10 to 45 mol%, and particularly preferably 15 to 40 mol%, relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a). If the content of the structural unit derived from the aliphatic polycarboxylic acid is too small, there is a tendency that the adhesive force and molding stability become insufficient, and if it is too large, there is a tendency that the heat resistance and moist heat resistance become insufficient.

[0098] When the polyester resin (A) has an acid value, it is preferred that the structural unit derived from the polycarboxylic acid (a) contains a structural unit derived from a trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride group from the viewpoint of adhesive strength.

[0099] The valence of the carboxyl group in the trivalent or higher polycarboxylic acid having 0 or 1 acid anhydride group is preferably 3 to 6, more preferably 3 to 4.

[0100] Examples of the trivalent or higher polycarboxylic acids having an anhydride group of 0 or 1 include: trivalent or higher aromatic polycarboxylic acids having an anhydride group of 0 or 1, such as trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tri(anhydrotrimellitate), trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)phthalic dianhydride, and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride; and trivalent or higher aliphatic polycarboxylic acids having an anhydride group of 0 or 1, such as hydrogenated trimellitic anhydride. These may be used alone or in combination of two or more.

[0101] Among them, trivalent or higher aromatic polycarboxylic acids having an acid anhydride group number of 0 or 1 are preferred, trivalent or higher aromatic polycarboxylic acids having an acid anhydride group number of 1 are more preferred, and trimellitic anhydride is particularly preferred.

[0102] The polyester resin (A) may also contain structural units derived from aromatic dicarboxylic acids having a sulfonic acid group such as sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfophthalic acid, 4-sulfonaphthalene-2,7-dicarboxylic acid, and 5-(4-sulfophenoxy)isophthalic acid, and structural units derived from aromatic dicarboxylates having a sulfonate group such as metal salts and ammonium salts thereof. From the viewpoint of the moist heat resistance of the polyester resin (A), the content of the structural units derived from the polycarboxylic acid (a) is preferably 10 mol% or less, more preferably 5 mol% or less, particularly preferably 3 mol% or less, further preferably 1 mol% or less, and most preferably 0 mol% with respect to 100 mol% of the structural units derived from the polycarboxylic acid (a).

[0103] [Polyols (b)]

[0104] Examples of the polyols (b) include aliphatic polyols (b1), dimer alcohols (b2), alicyclic polyols, aromatic polyols, bisphenol skeleton-containing polyols, etc. The polyols (b) may be used alone or in combination of two or more.

[0105] The polyester resin (A) contains a structural unit derived from an aliphatic polyol (b1) as a structural unit derived from a polyol (b).

[0106] Examples of the aliphatic polyols (b1) include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 2-methyl-1,3-propylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 1,10-decanediol, 2-ethyl-2-butylpropanediol, 2,4-diethyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, glycerol, trimethylolethane, trimethylolpropane, and pentaerythritol. Among these, from the viewpoint of excellent hydrolysis resistance, solvent dissolution stability and optical properties, aliphatic polyols having a hydrocarbon group in at least one side chain, such as 1,2-propylene glycol, 2-methyl-1,3-propylene glycol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol and 2,2,4-trimethyl-1,3-pentanediol, are preferred. 2-methyl-1,3-propylene glycol and 3-methyl-1,5-pentanediol are particularly preferred. From the viewpoint of excellent moisture and heat resistance and adhesive strength, 3-methyl-1,5-pentanediol is more preferred.

[0107] In addition, the aliphatic polyols having a hydrocarbon group in at least one side chain do not include dimer alcohols (b2) described later.

[0108] The content of the structural unit derived from the aliphatic polyol (b1) is preferably 5 to 95 mol%, more preferably 15 to 90 mol%, particularly preferably 25 to 85 mol%, further preferably 35 to 80 mol%, and particularly preferably 45 to 75 mol%, relative to 100 mol% of the structural unit derived from the polyol (b). If the content of the structural unit derived from the aliphatic polyol (b1) is too small, the compatibility with the polyepoxy compound (B) tends to be reduced, and the optical properties tend to be insufficient, or the solvent dissolution stability tends to be insufficient. If it is too large, the heat resistance, moisture heat resistance, and adhesive strength tend to be insufficient.

[0109] The polyester resin (A) preferably contains a structural unit derived from a dimer alcohol (b2) as a structural unit derived from a polyol (b).

[0110] Examples of the dimer alcohols (b2) include reduced products of dimer acids (mainly dimer acids having 36 to 44 carbon atoms) derived by dimerizing unsaturated aliphatic acids such as oleic acid, linoleic acid, linolenic acid, and erucic acid, and hydrogenated products thereof, etc. Among them, hydrogenated products are preferred from the viewpoint of suppressing gelation during the production of the polyester resin (A).

[0111] When the polyester resin (A) contains a structural unit derived from a dimer alcohol (b2), the content of the structural unit derived from the dimer alcohol (b2) is preferably 3 to 95 mol%, more preferably 5 to 90 mol%, particularly preferably 4 to 80 mol%, further preferably 5 to 70 mol%, particularly preferably 10 to 50 mol%, and most preferably 25 to 40 mol%, relative to 100 mol% of the structural unit derived from the polyol (b). If the content of the structural unit derived from the dimer alcohol (b2) is too small, there is a tendency that the adhesive force and the moisture heat resistance become insufficient, and if it is too large, there is a tendency that the compatibility with the polyepoxy compound (B) decreases, the optical properties become insufficient, or the solvent dissolution stability becomes insufficient.

[0112] In addition, when the polyester resin (A) contains a structural unit derived from a dimer alcohol (b2), the content of the structural unit derived from the dimer alcohol (b2) is preferably 3 to 80% by mass, more preferably 5 to 70% by mass, further preferably 10 to 60% by mass, particularly preferably 15 to 50% by mass, particularly preferably 18 to 40% by mass, and most preferably 30 to 45% by mass relative to the entire polyester resin (A). If the content of the structural unit derived from the dimer alcohol (b2) is too small, there is a tendency that heat resistance, moisture heat resistance, and adhesive strength become insufficient, and if it is too large, there is a tendency that compatibility with the polyepoxy compound (B) is reduced, optical properties become insufficient, or solvent dissolution stability becomes insufficient.

[0113] Examples of the alicyclic polyols include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediol, tricyclodecane dimethanol, and spirodiol.

[0114] Examples of the aromatic polyols include p-phenylenediol, m-phenylenediol, o-phenylenediol, 1,4-benzenediol, and ethylene oxide adducts of 1,4-benzenediol.

[0115] Examples of the polyols having a bisphenol skeleton include bisphenol A, bisphenol B, bisphenol E, bisphenol F, bisphenol AP, bisphenol BP, bisphenol P, bisphenol PH, bisphenol S, bisphenol Z, 4,4'-dihydroxybenzophenone, bisphenol fluorene, hydrogenated products thereof, and diols such as ethylene oxide adducts obtained by adding 1 to several mol of ethylene oxide or propylene oxide to the hydroxyl groups of bisphenols, and propylene oxide adducts.

[0116] Furthermore, in order to easily obtain a polymer of a target molecular weight, the polyester resin (A) can use polyester diol, polyether diol, polycaprolactone diol, polycarbonate diol, polybutadiene diol, polyisoprene diol, etc. as polyols (b). In addition, these can be used alone or in combination of two or more.

[0117] [Dimer acids (a2), dimer alcohols (b2)]

[0118] From the viewpoint of moisture and heat resistance and adhesive strength, the polyester resin (A) preferably contains a structural unit derived from dimer acids (a2) and / or a structural unit derived from dimer alcohols (b2).

[0119] When the polyester resin (A) contains a structural unit derived from a dimer acid (a2) and / or a structural unit derived from a dimer alcohol (b2), the total content of the structural unit derived from the dimer acid (a2) and the structural unit derived from the dimer alcohol (b2) is preferably 20 to 90% by mass, more preferably 30 to 85% by mass, particularly preferably 35 to 80% by mass, further preferably 40 to 75% by mass, particularly preferably 45 to 70% by mass, and most preferably 50 to 65% by mass relative to the entire polyester resin (A). If the total content of the structural unit derived from the dimer acid (a2) and the structural unit derived from the dimer alcohol (b2) is too small, there is a tendency that the adhesive force and the moist heat resistance become insufficient, and if it is too large, there is a tendency that the compatibility with the polyepoxy compound (B) is reduced, the optical properties become insufficient, or the solvent dissolution stability becomes insufficient.

[0120] [Trifunctional or higher polycarboxylic acids, and trifunctional or higher polyols]

[0121] The aforementioned polyester resin (A) preferably contains structural units derived from trifunctional or higher polycarboxylic acids and / or structural units derived from trifunctional or higher polyols as branched backbones. In particular, when the polyester resin (A) is reacted with a crosslinking agent to form a crosslinked structure, the polyester resin (A) contains a branched backbone, and the crosslinking points of the polyester resin (A) are increased, and an adhesive with high cohesive force can be efficiently obtained with a small amount of crosslinking. It should be noted that the aforementioned trifunctional or higher polycarboxylic acids used to introduce a branched backbone into the polyester resin (A) are different from the polycarboxylic acids used in the depolymerization reaction described later.

[0122] Examples of the trifunctional or higher polycarboxylic acids include trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tri(anhydrotrimellitate), trimellitic anhydride, pyromellitic acid dianhydride, oxydiphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)phthalic acid dianhydride, and compounds such as 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride.

[0123] Examples of the trifunctional or higher polyols include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.

[0124] These trifunctional or higher polycarboxylic acids and trifunctional or higher polyols can be used alone or in combination of two or more.

[0125] When the polyester resin (A) contains structural units derived from trifunctional or higher polycarboxylic acids and / or structural units derived from trifunctional or higher polyols as branched backbones, the content of trifunctional or higher polycarboxylic acids is preferably 0.1 to 5 mol%, more preferably 0.3 to 4 mol%, further preferably 0.5 to 3 mol%, and particularly preferably 1 to 2.5 mol% relative to 100 mol% of structural units derived from polycarboxylic acids (a). In addition, the content of trifunctional or higher polyols is preferably 0.1 to 5 mol%, more preferably 0.3 to 4 mol%, further preferably 0.5 to 3 mol%, and particularly preferably 1 to 2.5 mol% relative to 100 mol% of structural units derived from polyols (b). If the content of either or both is too high, there is a tendency that mechanical properties such as elongation at break of the coating film formed by applying the adhesive are reduced, resulting in reduced adhesive strength, and there is also a tendency that gelation occurs during polymerization.

[0126] [Structural unit derived from cyclic ester]

[0127] The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b), and may further contain a structural unit derived from a cyclic ester.

[0128] Examples of the cyclic ester include propiolactone, β-propiolactone, β-butyrolactone, γ-butyrolactone, γ-caprolactone, γ-octalactone, δ-valerolactone, δ-caprolactone, δ-octalactone, ε-caprolactone, δ-dodecalactone, α-methyl-γ-butyrolactone, β-methyl-valerolactone, and aliphatic lactones such as glycolide. One or more of these cyclic ester monomers may be used.

[0129] The content of the structural unit derived from the cyclic ester in the polyester resin (A) is preferably less than 140 mol%, more preferably less than 100 mol%, particularly preferably less than 60 mol%, further preferably less than 30 mol%, particularly preferably less than 15 mol%, and most preferably 0 mol%, relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a). If the content of the structural unit derived from the cyclic ester is too high, heat resistance, moist heat resistance, and solvent dissolution stability tend to be insufficient.

[0130] [Production of polyester resin (A)]

[0131] The polyester resin (A) can be produced by a known method.

[0132] For example, the polyester resin can be produced by subjecting polycarboxylic acids (a) and polyols (b) to an esterification reaction in the presence of a catalyst as required to obtain a prepolymer, followed by polycondensation to obtain the polyester resin, and then introducing an acid value as required.

[0133] The temperature in the esterification reaction of the polycarboxylic acid (a) and the polyol (b) is usually 180 to 280° C., and the reaction time is usually 60 minutes to 8 hours.

[0134] The temperature during the polycondensation is usually 220 to 280° C., and the reaction time is usually 20 minutes to 4 hours. The polycondensation is preferably performed under reduced pressure.

[0135] Examples of a method for introducing an acid value into a polyester resin include a method of introducing a carboxyl group into the polyester resin by an acid addition method or a depolymerization method after an esterification reaction or after polycondensation under reduced pressure.

[0136] Among them, when introducing carboxyl groups into the main chain terminals of the polyester resin, the depolymerization method is particularly preferred from the viewpoints of efficiently introducing carboxyl groups, increasing the molecular weight between crosslinking points with the polyepoxy compound (B), and achieving excellent adhesion, heat resistance, and molding stability.

[0137] Furthermore, when introducing a carboxyl group into a side chain of a polyester-based resin, an acid addition method is preferred.

[0138] When a carboxyl group is introduced into the main chain terminal of the polyester resin by the depolymerization method, for example, a polycarboxylic acid (a) and a polyol (b) are subjected to an esterification reaction in the presence of a catalyst as required to obtain a prepolymer, followed by polycondensation and further depolymerization.

[0139] From the viewpoint of adhesive strength, it is preferred to use a trivalent or higher polycarboxylic acid having an anhydride group of 0 or 1 for depolymerization. Examples of the trivalent or higher polycarboxylic acid having an anhydride group of 0 or 1 include compounds such as trimellitic acid, trimellitic anhydride, hydrogenated trimellitic anhydride, and trimesic acid. From the viewpoint of suppressing a decrease in molecular weight, a trivalent or higher polycarboxylic acid having an anhydride group of 1 is preferred, and examples thereof include trimellitic anhydride, hydrogenated trimellitic anhydride, and the like, and trimellitic anhydride is particularly preferred.

[0140] The temperature during depolymerization is usually 200 to 260° C., and the reaction time is usually 10 minutes to 3 hours.

[0141] When the polyester resin (A) is produced by a depolymerization method, if the content of the structural units derived from trivalent or higher polycarboxylic acids having 0 or 1 anhydride groups exceeds 20 mol % relative to 100 mol % of the structural units derived from the polycarboxylic acid (a), the molecular weight of the resin tends to decrease significantly.

[0142] Therefore, the content of the structural units derived from trivalent or higher polycarboxylic acids having 0 or 1 anhydride groups is preferably 20 mol% or less, more preferably 1 to 15 mol%, particularly preferably 2 to 10 mol%, and further preferably 3 to 8 mol%, relative to 100 mol% of the structural units derived from the polycarboxylic acid (a).

[0143] In the case of introducing carboxyl groups into the side chains of the polyester resin by the acid addition method, for example, a polycarboxylic acid (a) other than a polycarboxylic acid anhydride and a polyol (b) can be subjected to an esterification reaction to obtain a prepolymer, and then the obtained carboxyl group-containing prepolymer is reacted with a polycarboxylic acid anhydride to perform acid addition. It should be noted that in the acid addition method, if a monocarboxylic acid, a dicarboxylic acid, or a polyfunctional carboxylic acid compound is used, there is a possibility that the molecular weight is reduced due to ester exchange, so it is preferred to use a compound having at least one carboxylic acid anhydride.

[0144] Examples of the method for acid addition and depolymerization include a method of directly adding the acid in a bulk state and a method of adding the acid by solubilizing the polyester resin.

[0145] The reaction speed in the bulk state is high, but if a large amount is added, gelation will occur. In addition, the reaction will be at a high temperature, so care must be taken to block oxygen to prevent oxidation.

[0146] On the other hand, although the addition reaction in a solution state is slow, a large number of carboxyl groups can be stably introduced.

[0147] Examples of the carboxylic anhydride include succinic anhydride, maleic anhydride, phthalic anhydride, 2,5-norbornene dicarboxylic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, oxydiphthalic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyltetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride, and compounds such as 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride.

[0148] When the polyester resin (A) is produced by the acid addition method, if 15 mol % or more of the acid is added to 100 mol % of the structural units derived from the polycarboxylic acid (a), gelation occurs. Therefore, the acid addition is preferably performed at less than 15 mol %.

[0149] [Composition ratio of polyester resin (A)]

[0150] In the present invention, the ratio of the structural parts (composition ratio) of the components derived from the polyester resin (A) can be determined by a known method using NMR, for example, a resonance frequency of 400 MHz. 1H-NMR measurement (proton nuclear magnetic resonance spectroscopy measurement), 13 The method can be determined by C-NMR measurement (carbon nuclear magnetic resonance spectroscopy measurement) or the like.

[0151] [Glass transition temperature of polyester resin (A)]

[0152] The glass transition temperature of the polyester resin (A) used in the present invention is -75 to -20°C, preferably -70 to -22°C, more preferably -65 to -24°C, particularly preferably -60 to -26°C, further preferably -55 to -28°C, particularly preferably -50 to -30°C, and most preferably -45 to -35°C. If the glass transition temperature is too high, the viscosity and adhesive force will be insufficient, or the tensile properties will be reduced, and the processing suitability and molding stability will tend to be insufficient. If the glass transition temperature is too low, the heat resistance and moist heat resistance will tend to be insufficient.

[0153] The method for measuring the glass transition temperature is as follows.

[0154] The glass transition temperature can be determined by measuring using a differential scanning calorimeter. The measurement conditions are a measurement temperature range of -90 to 100°C and a temperature increase rate of 10°C / min.

[0155] [Acid value of polyester resin (A)]

[0156] In the present invention, the polyester resin (A) is cross-linked by the polyepoxy compound (B) and has a carboxyl group as a cross-linking point.

[0157] The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g, preferably 2 to 20 mgKOH / g, particularly preferably 2.5 to 15, further preferably 3 to 12 mgKOH / g, particularly preferably 3.5 to 10 mgKOH / g, and most preferably 4 to 8 mgKOH / g. If the acid value is too low, the heat resistance tends to be insufficient due to the decrease in crosslinking points, and if the acid value is too high, the adhesion and molding stability tend to be insufficient due to the increase in crosslinking points, or the amount of the polyepoxy compound (B) required for crosslinking tends to be insufficient, resulting in insufficient optical properties.

[0158] The definition and measurement method of the acid value are as follows.

[0159] The acid value (mgKOH / g) can be determined by dissolving 1 g of the polyester resin (A) in 30 g of a mixed solvent of toluene / methanol (for example, a volume ratio of toluene / methanol = 7 / 3), and performing neutralization titration in accordance with JIS K 0070.

[0160] In addition, in this invention, the acid value of a polyester resin (A) is derived from the content of the carboxyl group in a resin.

[0161] [Hydroxyl value of polyester resin (A)]

[0162] In addition, the hydroxyl value of the polyester resin (A) is preferably 10 mgKOH / g or less, particularly preferably 5 mgKOH / g or less, further preferably 3 mgKOH / g or less, more preferably 2 mgKOH / g or less, particularly preferably 1 mgKOH / g or less, and most preferably 0.5 mgKOH / g or less. If the hydroxyl value is too high, there is a tendency that the number of crosslinking points with the polyepoxy compound (B) decreases, and heat resistance and moist heat resistance become insufficient.

[0163] The hydroxyl value of the polyester resin (A) can be determined by neutralization titration in accordance with JIS K 0070.

[0164] [Ester bond concentration of polyester resin (A)]

[0165] The ester bond concentration of the polyester resin (A) used in the present invention is preferably 1.5 to 8 mmol / g, more preferably 2 to 7.5 mmol / g, further preferably 2.5 to 7 mmol / g, particularly preferably 3 to 6.5 mmol / g, particularly preferably 3.5 to 6 mmol / g, and most preferably 4 to 5.5 mmol / g.

[0166] If the ester bond concentration is too high, heat resistance and moist heat resistance tend to be insufficient, while if the ester bond concentration is too low, compatibility with the polyepoxy compound (B) tends to decrease, resulting in insufficient optical properties.

[0167] The definition and measurement method of the ester bond concentration are as follows.

[0168] The ester bond concentration (mmol / g) refers to the number of moles of ester bonds in 1 g of the polyester resin (A), and is obtained, for example, by a calculated value based on the feed amount. The calculation method is a value obtained by dividing the smaller number of moles of each feed amount of the polycarboxylic acid (a) and the polyol (b) by the total mass of the polyester resin (A). An example of the calculation formula is shown below.

[0169] In addition, when each charging amount of polycarboxylic acid (a) and polyol (b) is the same molar amount, any of the following calculation formulas can be used.

[0170] In addition, when a compound having both a carboxyl group and a hydroxyl group is used as a monomer, or when a polyester is produced from caprolactone or the like, the calculation method is appropriately changed.

[0171] (When the amount of polycarboxylic acid (a) is less than that of polyol (b))

[0172] Ester group concentration (mmol / g) = [(A1 / a1×m1+A2 / a2×m2+A3 / a3×m3…) / Z]×1000

[0173] A: Amount of polycarboxylic acid (a) (g)

[0174] a: Molecular weight of polycarboxylic acid (a)

[0175] m: the number of carboxyl groups per molecule of the polycarboxylic acid (a)

[0176] Z: Finished mass (g)

[0177] (When the amount of polyols (b) is less than that of polycarboxylic acids (a))

[0178] Ester group concentration (mmol / g) = [(B1 / b1×n1+B2 / b2×n2+B3 / b3×n3…) / Z]×1000

[0179] B: Feeding amount of polyol (b) (g)

[0180] b: Molecular weight of polyol (b)

[0181] n: number of hydroxyl groups per molecule of the polyol (b)

[0182] Z: Finished mass (g)

[0183] The ester bond concentration can also be determined by a known method using NMR or the like, for example, by using a resonance frequency of 400 MHz. 1 H-NMR measurement (proton nuclear magnetic resonance spectroscopy measurement), 13 The measurement was carried out by C-NMR measurement (carbon nuclear magnetic resonance spectroscopy measurement).

[0184] [Peak Top Molecular Weight (Mp) and Weight Average Molecular Weight (Mw) of Polyester Resin (A)]

[0185] The peak top molecular weight (Mp) of the polyester resin (A) is preferably 5,000 to 150,000, more preferably 10,000 to 120,000, particularly preferably 20,000 to 100,000, further preferably 30,000 to 90,000, and particularly preferably 40,000 to 80,000.

[0186] If the peak top molecular weight (Mp) is too low, the cohesive force is insufficient, and the heat resistance and wet heat durability tend to be insufficient. In addition, if the peak top molecular weight (Mp) is too high, the adhesive force is insufficient, or the compatibility with the polyepoxy compound (B) is reduced, and the optical properties tend to be insufficient.

[0187] The weight average molecular weight (Mw) of the polyester resin (A) is preferably 5,000 to 500,000, more preferably 10,000 to 300,000, particularly preferably 20,000 to 200,000, further preferably 30,000 to 150,000, and particularly preferably 50,000 to 130,000.

[0188] If the weight average molecular weight (Mw) is too low, the cohesive force is insufficient, and the heat resistance and wet heat durability tend to be insufficient. In addition, if the weight average molecular weight (Mw) is too high, the adhesive force is insufficient, or the compatibility with the polyepoxy compound (B) is reduced, and the optical properties tend to be insufficient.

[0189] The peak top molecular weight (Mp) and the weight average molecular weight (Mw) are measured as follows.

[0190] The peak molecular weight (Mp) and weight average molecular weight (Mw) can be determined by high performance liquid chromatography (manufactured by Tosoh Corporation, “HLC-8320GPC”) using two pillars (TSKgel SuperMultipore HZ-M (exclusion limit molecular weight: 2×10 6 , theoretical plate number: 16000 plates / plate, filler material: styrene-divinylbenzene copolymer, filler particle size: 4 μm)) are measured in series and calculated using standard polystyrene molecular weight.

[0191] In the present invention, the polyester resin (A) is preferably a non-crystalline polyester resin from the viewpoints of solvent solubility, solution stability, viscosity, optical properties, etc. It should be noted that if the polyester resin (A) is crystalline, solvent solubility, solution stability, viscosity, molding stability, optical properties, etc. tend to be insufficient.

[0192] The amorphous property can be confirmed by a differential scanning calorimeter, for example, when no endothermic peak due to crystal melting is observed when the measurement is performed at a measurement temperature range of -90 to 400°C and a temperature increase rate of 10°C / min. It should be noted that the measurement temperature range and the temperature increase rate may be appropriately changed depending on the sample.

[0193] The crystal fusion heat of the polyester resin (A) is 35 J / g or less, preferably 20 J / g or less, particularly preferably 10 J / g or less, particularly preferably 5 J / g or less, more preferably 3 J / g or less, and most preferably 1 J / g or less during crystallization. When the crystal fusion heat is 0 J / g, the polyester resin (A) is amorphous, which is preferred from the viewpoints of solvent solubility, solution stability, viscosity, optical properties, etc.

[0194] Furthermore, the polyester resin (A) preferably has a biomass content consisting of plant-derived raw materials in order to reduce the burden on the global environment.

[0195] The biomass degree of the polyester resin (A) is preferably 10% or more, more preferably 20% or more, particularly preferably 30% or more, further preferably 40% or more, particularly preferably 50% or more, and most preferably 60% or more. It should be noted that the upper limit is 100%. If the biomass degree is low, there is a tendency that the reduction of the burden on the global environment becomes insufficient.

[0196] Here, the biomass degree of the aforementioned polyester resin (A) refers to the mass ratio of the portion of the plant-derived raw material used in the manufacture of the aforementioned polyester resin (A) incorporated into the resin relative to the total mass of the polyester resin (A), and the calculation method thereof is as described below. It should be noted that the biomass degree of polycarboxylic acids (a) and polyols (b) is a value obtained by weighted average of their respective biomass degrees. In addition, in the following calculation method, the value obtained by any method may be within the aforementioned range.

[0197] (Calculation method)

[0198] Biomass content (%) = [(the number of moles of carbon atoms of the plant-derived monomer calculated from the molar ratio of the polycarboxylic acid (a) and the polyol (b) in the polyester resin (A)) / (the number of moles of carbon atoms of all constituent monomers in the polyester resin (A))] × 100

[0199] The biomass degree can be determined by analyzing the composition ratio by NMR and calculating the number of carbon atoms in the plant-derived monomer / the number of carbon atoms in the whole plant.

[0200] Furthermore, the aforementioned biomass degree can also be measured by the method described in Tokyo Metropolitan Industrial Technology Research Center Research Report No. 4, 2009, "Technology for Identifying the Origin of Biomass Fuels Using Natural Radioactive Carbon C-14".

[0201] In addition, from the viewpoint of VOC emission regulation, in the present invention, the polyester resin (A) is preferably soluble in a non-petroleum organic solvent and a non-aldehyde organic solvent. If the solubility in the organic solvent is insufficient, the burden on the human body and the global environment will increase, the preparation of the present adhesive composition will become difficult, or the stability of the solution after dissolution will tend to be insufficient.

[0202] The non-petroleum organic solvent and the non-aldehyde organic solvent include, for example, ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohol solvents such as methanol, ethanol, isopropyl alcohol, and isobutyl alcohol, ester solvents such as ethyl acetate and n-butyl acetate, acetate ester solvents such as cellosolve acetate and methoxyacetate, or a mixture of two or more of these solvents. Among them, ketone solvents and ester solvents are preferred, and methyl ethyl ketone, cyclohexanone, and ethyl acetate are particularly preferred. From the viewpoint of low boiling point and excellent drying efficiency, methyl ethyl ketone and ethyl acetate are more preferred.

[0203] <Polyepoxy compound (B)>

[0204] The present adhesive composition further contains a polyepoxy compound (B) as a crosslinking agent.

[0205] The adhesive composition contains a polyepoxy compound (B), and the epoxy group in the polyepoxy compound (B) reacts with the carboxyl group in the polyester resin (A) to crosslink (cure), thereby obtaining an adhesive having not only excellent adhesive strength but also excellent heat resistance. It should be noted that the polyepoxy compound (B) refers to a compound having at least two epoxy groups in the molecule.

[0206] Examples of the polyepoxy compound (B) include glycidylamines such as tetraglycidyl diaminodiphenylmethane, triglycidyl p-aminophenol, tetraglycidyl bisaminomethylcyclohexane, and N,N,N',N'-tetraglycidyl-m-xylenediamine; bifunctional glycidyl ethers such as bisphenol A diglycidyl ether, bisphenol S diglycidyl ether, and brominated bisphenol A diglycidyl ether; polyfunctional glycidyl ethers such as phenol novolac glycidyl ether and cresol novolac glycidyl ether; glycidyl esters such as hexahydrophthalic acid glycidyl ester and dimer acid glycidyl ester; alicyclic or aliphatic epoxides such as triglycidyl isocyanurate, 3,4-epoxycyclohexylmethylcarboxylate, epoxidized polybutadiene, and epoxidized soybean oil. One or more of the polyepoxy compounds (B) may be used.

[0207] From the viewpoint of being able to cure the coating film of the adhesive composition at a relatively low temperature, the present adhesive composition preferably contains a polyepoxy compound containing a nitrogen atom (polyepoxy compound containing a nitrogen atom) as the polyepoxy compound (B). Particularly preferred are aromatic glycidylamine-type polyepoxy compounds such as tetraglycidyldiaminodiphenylmethane and triglycidylparaaminophenol, and aliphatic glycidylamine-type polyepoxy compounds such as 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane and N,N,N',N'-tetraglycidyl-m-phenylenediamine. From the viewpoint of excellent low-temperature curing properties, preferred are aliphatic glycidylamine-type polyepoxy compounds such as 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane and N,N,N',N'-tetraglycidyl-m-phenylenediamine.

[0208] The equivalent of the epoxy group of the polyepoxy compound (B) relative to the carboxyl group of the polyester resin (A) is preferably 0.3 to 5 equivalents, more preferably 0.5 to 4 equivalents, even more preferably 0.7 to 3.5 equivalents, further preferably 0.9 to 3.0 equivalents, particularly preferably 1.0 to 2.8 equivalents, particularly preferably 1.2 to 2.6 equivalents, particularly preferably 1.4 to 2.4 equivalents, and most preferably 1.6 to 2.2 equivalents.

[0209] If the equivalent weight is too large, the polyepoxy compound (B) not incorporated into the crosslinking will remain, and the optical properties and heat resistance will tend to be insufficient. If it is too small, the crosslinking density will be low, and the heat resistance, wet heat resistance, and adhesive strength will tend to be insufficient.

[0210] The equivalent weight of the epoxy group to the carboxyl group (COOH) can be determined by the following formula based on the acid value of the polyester resin (A) and the epoxy equivalent weight (g / eq) of the blended polyepoxy compound (B).

[0211] Equivalent weight of epoxy group to COOH = (e÷WPE) / (AV÷56.1÷1000×P)

[0212] e: Mass (g) of the polyepoxy compound (B) used for compounding

[0213] WPE: Epoxy equivalent of polyepoxy compound (B) (g / eq)

[0214] AV: Acid value of polyester resin (A) (mgKOH / g)

[0215] P: Mass of polyester resin (A) used for compounding (g)

[0216] It should be noted that the epoxy equivalent (WPE) of the polyepoxy compound (B) is preferably 500 g / eq or less, more preferably 350 g / eq or less, further preferably 250 g / eq or less, particularly preferably 200 g / eq or less, and particularly preferably 150 g / eq or less. If the epoxy equivalent of the polyepoxy compound (B) is too large, there is a tendency that the crosslinking density after curing decreases and the heat resistance becomes insufficient, or a large amount of polyepoxy compound (B) needs to be added to increase the crosslinking density, so the optical properties become insufficient. It should be noted that the lower limit of the epoxy equivalent (WPE) of the polyepoxy compound (B) is usually 50 g / eq or more.

[0217] The "epoxy equivalent (WPE)" in the present invention is defined as "the mass of an epoxy resin containing 1 equivalent of epoxy groups", and can be measured in accordance with JIS K 7236.

[0218] The amount of the epoxy compound (B) is preferably 0.1 to 15 parts by mass, more preferably 0.2 to 10 parts by mass, further preferably 0.3 to 5 parts by mass, particularly preferably 0.5 to 4.5 parts by mass, particularly preferably 0.7 to 4 parts by mass, and most preferably 1 to 3.5 parts by mass relative to 100 parts by mass of the polyester resin (A). If the amount of the polyepoxy compound (B) is too much, there is a tendency that the polyepoxy compound (B) that is not incorporated into the crosslinking remains, and the optical properties and heat resistance become insufficient. In addition, if it is too little, there is a tendency that the crosslinking density becomes low, and the heat resistance, wet heat resistance, and adhesive force become insufficient.

[0219] <Polyisocyanate compound (C)>

[0220] From the viewpoint of moisture and heat resistance, the present adhesive composition may contain a polyisocyanate compound (C) as a crosslinking agent. The polyisocyanate compound (C) refers to a compound having at least two isocyanate groups in the molecule.

[0221] Examples of the polyisocyanate compound (C) include aromatic diisocyanate compounds such as 2,4-toluene diisocyanate and 2,6-toluene diisocyanate, toluene diisocyanate compounds such as 1,3-xylylene diisocyanate, diphenylmethane compounds such as diphenylmethane-4,4-diisocyanate, and naphthalene diisocyanate crosslinking agents such as 1,5-naphthalene diisocyanate; aromatic diisocyanate compounds such as isophorone diisocyanate, 1,4-cyclohexane diisocyanate, 4,4'-dicyclohexane diisocyanate, and the like; Hexylmethane diisocyanate, methylcyclohexane diisocyanate, isopropylidene dicyclohexyl-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, norbornane diisocyanate and other alicyclic diisocyanate compounds; hexamethylene diisocyanate, trimethylhexamethylene diisocyanate and other aliphatic diisocyanate compounds; adducts, biuret bodies, isocyanurate bodies and the like of the aforementioned aromatic diisocyanate compounds, alicyclic diisocyanate compounds and aliphatic diisocyanate compounds. It should be noted that the aforementioned polyisocyanate compounds (C) can also use compounds in which the isocyanate moiety is blocked by phenol, lactam and the like. These polyisocyanate compounds (C) can be used alone or in combination of two or more. Among them, from the viewpoint of optical properties and heat resistance, alicyclic diisocyanate compounds and aliphatic diisocyanate compounds are preferred, aliphatic diisocyanate compounds are particularly preferred, and isocyanurate of hexamethylene diisocyanate is further preferred.

[0222] The equivalent of the isocyanate group of the polyisocyanate compound (C) to the hydroxyl group of the polyester resin (A) is preferably 3 equivalents or less, more preferably 2 equivalents or less, further preferably 1.5 equivalents or less, particularly preferably 1 equivalent or less, and particularly preferably 0.5 equivalent or less.

[0223] If the equivalent weight is too large, the polyisocyanate compound (C) which is not incorporated into the crosslinking tends to remain and the optical properties tend to be insufficient, or the urethane bond concentration tends to be high and the heat resistance tends to be insufficient.

[0224] When the present adhesive composition contains a polyisocyanate compound (C), the content thereof is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, further preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, particularly preferably 1.5 parts by mass or less, and most preferably 1 part by mass or less, relative to 100 parts by mass of the polyester resin (A). If the amount of the polyisocyanate compound added is too much, there is a tendency that the polyisocyanate compound (C) not incorporated into the crosslinking remains, the optical properties become insufficient, or the heat resistance decreases due to the increase in the urethane bond concentration.

[0225] <Carbodiimide compounds>

[0226] From the viewpoint of moisture and heat resistance, the present adhesive composition may contain a carbodiimide compound.

[0227] As the aforementioned carbodiimide compound, a known carbodiimide having one or more carbodiimide groups (-N=C=N-) in the molecule can be used. From the viewpoint of improving durability under higher temperature and humidity, a compound containing two or more carbodiimide groups in the molecule, i.e., a polycarbodiimide compound, is preferably a compound containing three or more carbodiimide groups in the molecule, further preferably containing five or more, and especially containing seven or more. It should be noted that the number of carbodiimide groups in the molecule is usually less than 50. If there are too many carbodiimide groups, there is a tendency that the molecular structure becomes too large, so the compatibility is reduced and the optical properties become insufficient. In addition, a high molecular weight polycarbodiimide generated by decarboxylation condensation reaction of diisocyanate in the presence of a carbodiimidization catalyst can also be used.

[0228] As such a high molecular weight polycarbodiimide, a high molecular weight polycarbodiimide obtained by subjecting the following diisocyanates to a decarboxylation condensation reaction can be cited. As such a diisocyanate, for example, 4,4'-diphenylmethane diisocyanate, 3,3'-dimethoxy-4,4'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 3,3'-dimethyl-4,4'-diphenylether diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1-methoxyphenyl-2,4-diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, etc. can be cited, and these can be used alone or in combination of two or more.

[0229] When the adhesive composition contains a carbodiimide compound, the content thereof is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, further preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, especially preferably 1 part by mass or less, and most preferably 0.5 parts by mass or less, relative to 100 parts by mass of the polyester resin (A). If the amount of the carbodiimide compound added is too much, there is a tendency that an excess of the carbodiimide compound that is not incorporated into the crosslinking remains and the optical properties become insufficient, or that the crosslinking between the polyester resin (A) and the polyepoxy compound (B) is hindered and the heat resistance becomes insufficient.

[0230] <Metal chelate compounds>

[0231] From the viewpoint of moisture and heat resistance, the present adhesive composition may also contain a metal chelate compound as a crosslinking agent. Examples of the metal chelate compound include metal alkoxides such as tetraethyl titanate, tetraethyl zirconate, and aluminum isopropionate, metal chelate compounds of acetylacetone, acetoacetate, and ethylenediaminetetraacetic acid coordination compounds of polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, and zirconium, acetic acid-ammonium complex salts, ammonium-carbonate complex salts, and the like. One or more of these metal chelate compounds may be used.

[0232] When the present adhesive composition contains a metal chelate compound, the content thereof is preferably 5 parts by mass or less, more preferably 4 parts by mass or less, further preferably 3 parts by mass or less, particularly preferably 2 parts by mass or less, especially preferably 1 part by mass or less, and most preferably 0.5 parts by mass or less, relative to 100 parts by mass of the polyester resin (A). If the amount of the metal chelate compound added is too much, there is a tendency that the metal chelate compound not incorporated into the crosslinking remains and the optical properties become insufficient, or that the crosslinking of the polyester resin (A) and the polyepoxy compound (B) is hindered and the heat resistance becomes insufficient.

[0233] <Tackifying resin>

[0234] The present adhesive composition may also contain a tackifying resin in order to improve adhesive properties.

[0235] The tackifier resin is not particularly limited, and a conventionally known tackifier resin can be used.

[0236] Examples of the tackifying resin include hydrocarbon resins, terpene resins, phenolic resins, rosin resins, xylene resins, epoxy resins, polyamide resins, ketone resins, and elastic resins. These resins may be used alone or in combination of two or more. Among them, hydrocarbon tackifying resins and terpene resins are preferred from the viewpoint of compatibility with the polyester resin (A) and excellent heat resistance.

[0237] Examples of the hydrocarbon-based tackifying resin include various hydrocarbon-based resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins.

[0238] Examples of the terpene resin include terpene resins, terpene phenolic resins, and aromatic modified terpene resins. Specifically, α-pinene polymers, β-pinene polymers, dipentene polymers, or terpene resins obtained by phenol modification, aromatic modification, hydrogenation modification, or hydrocarbon modification of these can be used. In addition, terpene phenolic resins are preferred from the viewpoint of excellent compatibility with the polyester resin (A) and excellent heat resistance.

[0239] As the phenolic resin, for example, various phenols such as phenol, m-cresol, 3,5-xylenol, p-alkylphenol, and resorcinol, and condensates of formaldehyde can be used. Furthermore, resol-type phenolic resins obtained by subjecting the phenols to an addition reaction with formaldehyde in the presence of an alkali catalyst, novolacs obtained by subjecting the phenols to a condensation reaction with formaldehyde in the presence of an acid catalyst, and rosin-modified phenolic resins obtained by subjecting phenol to an addition reaction with rosins such as unmodified or modified rosins or derivatives thereof in the presence of an acid catalyst and thermal polymerization can be used.

[0240] Examples of the rosin-based resin include rosin resin, polymerized rosin resin, hydrogenated rosin resin, rosin ester resin, hydrogenated rosin ester resin, rosin phenolic resin, polymerized rosin ester, and the like. Specifically, unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin, and modified rosins obtained by hydrogenation, disproportionation, polymerization, or other chemical modifications thereof, and derivatives thereof can be used.

[0241] From the viewpoint of moisture and heat resistance, the acid value of the tackifying resin is preferably 30 mgKOH / g or less, particularly preferably 15 mgKOH / g or less, further preferably 10 mgKOH / g or less, particularly preferably 6 mgKOH / g or less, and most preferably 3 mgKOH / g. When a plurality of tackifying resins are used in combination, it is preferred that the average thereof is within the above range.

[0242] The softening point of the tackifier resin (measured by, for example, a ring and ball method) is preferably 60 to 170° C., particularly 80 to 160° C., and more preferably 100 to 150° C. The softening point within the above range is preferred because tack and adhesive strength can be improved.

[0243] In addition, for the purpose of protecting the global environment, the tackifier resin is preferably a plant-derived tackifier resin. Examples of the plant-derived tackifier resin include terpene-based resins and rosin-based resins.

[0244] When the adhesive composition contains a tackifying resin, the content thereof is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, further preferably 15 parts by mass or less, particularly preferably 10 parts by mass or less, and particularly preferably 5 parts by mass or less, relative to 100 parts by mass of the polyester resin (A). If the content is within the aforementioned range, it is preferred because the viscosity and adhesive force can be improved. If the content is too high, the glass transition temperature of the adhesive becomes high, and the viscosity, adhesive force, and molding stability tend to become insufficient.

[0245] [catalyst]

[0246] The present adhesive composition may contain a catalyst in order to allow the crosslinking (curing) of the polyepoxy compound (B) to proceed at a relatively low temperature.

[0247] Examples of the catalyst include imidazole compounds such as 2-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, and 1-cyanoethyl-2-ethyl-4-methylimidazole; tertiary amines such as triethylamine, triethylenediamine, N'-methyl-N-(2-dimethylaminoethyl)piperazine, 1,8-diazabicyclo[5,4,0]undecene-7, 1,5-diazabicyclo[4.3.0]non-5-ene, and 6-dibutylamino-1,8-diazabicyclo[5.4.0]-7-undecene; and compounds obtained by converting these tertiary amines into ammonium salts using phenol, octyl acid, quaternary tetraphenylborate, and the like; cationic catalysts such as triarylsulfonium hexafluoroantimonate and diaryliodonium hexafluoroantimonate; and triphenylphosphine. Among these, tertiary amines such as 1,8-diazabicyclo[5,4,0]undecene-7, 1,5-diazabicyclo[4.3.0]non-5-ene, and 6-dibutylamino-1,8-diazabicyclo[5,4,0]undecene-7, and compounds obtained by converting these tertiary amines into ammonium salts with phenol, octyl acid, quaternized tetraphenylborate, etc. are preferred from the viewpoints of thermosetting properties, heat resistance, adhesion to metals, and storage stability after compounding. One or more of these catalysts may be used.

[0248] When the adhesive composition contains a catalyst, the amount thereof is preferably 0.01 to 1 part by mass relative to 100 parts by mass of the polyester resin (A). If the content is within the above range, the reaction of the polyester resin (A) and the polyepoxy compound (B) can obtain an adhesive with a high degree of crosslinking at a low temperature and in a short time.

[0249] <Antioxidant (D)>

[0250] From the viewpoint of improving the heat resistance of the polyester resin (A), the present adhesive composition more preferably contains an antioxidant (D).

[0251] Examples of the antioxidant (D) include hindered phenol antioxidants, amine antioxidants, sulfur antioxidants, and phosphoric acid antioxidants. Among them, at least one selected from hindered phenol antioxidants, amine antioxidants, and phosphoric acid antioxidants is preferred, and an antioxidant (D) containing a hindered phenol compound is particularly preferred.

[0252] Examples of the hindered phenol antioxidant include antioxidants having a hindered phenol structure in which a group having a large steric hindrance such as a tert-butyl group is bonded to at least one of carbon atoms adjacent to a carbon atom on an aromatic ring to which a hydroxyl group of a phenol is bonded.

[0253] When the present adhesive composition contains an antioxidant (D), the amount thereof is preferably 0.001 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, further preferably 0.02 to 2 parts by mass, particularly preferably 0.03 to 1 part by mass, and particularly preferably 0.05 to 0.5 parts by mass, relative to 100 parts by mass of the polyester resin (A).

[0254] If the content is too small, heat resistance tends to be insufficient, and if too large, optical properties tend to be insufficient.

[0255] <Adhesive composition>

[0256] In the range that does not impair the effect of the present invention, in addition to the aforementioned polyester resin (A), polyepoxy compound (B), polyisocyanate compound (C), carbodiimide compound, metal chelate compound, catalyst, tackifying resin, antioxidant (D), this adhesive composition can also be mixed with additives such as plasticizer, ultraviolet absorber, stabilizer, antistatic agent, silane coupling agent, flux, flame retardant, dispersant, emulsifier, defoamer, leveling agent, ion capture agent, inorganic or organic filler, metal powder, pigment powder, granular etc. as other ingredients. These can be used alone or in combination of two or more. In addition, this adhesive composition can also contain impurities etc. contained in the manufacturing raw materials etc. of the constituent components of this adhesive composition in small amounts.

[0257] When the adhesive composition contains the above-mentioned additives, the content thereof is preferably 70% by mass or less, more preferably 0.001 to 50% by mass, particularly preferably 0.005 to 30% by mass, and further preferably 0.01 to 10% by mass, based on the entire adhesive composition.

[0258] The content of the polyester resin (A) in the adhesive composition is usually 70% by mass or more, more preferably 80 to 99.5% by mass, particularly preferably 85 to 99% by mass, further preferably 90 to 98.5% by mass, and particularly preferably 95 to 98% by mass.

[0259] Such an adhesive composition can be obtained by, for example, preparing the aforementioned polyester resin (A), the polyepoxy compound (B) and any necessary components, and mixing and dispersing them during the production of the polyester resin (A), or mixing them into a solution of the polyester resin (A) dissolved in an organic solvent and dispersing them using a mixing roll, etc.

[0260] <Solvent>

[0261] In order to properly adjust the viscosity of the adhesive composition and facilitate handling when forming a coating film, a solvent may be added to the adhesive composition. The solvent is used to ensure the operability and workability during molding of the adhesive composition, and the amount used is not particularly limited.

[0262] Examples of the aforementioned solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate; ethers such as ethylene glycol monomethyl ether; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; alcohols such as methanol and ethanol; alkanes such as hexane and cyclohexane; aromatics such as toluene and xylene. Among these, from the perspective of VOC emission regulations, ketone solvents and ester solvents are preferred, and methyl ethyl ketone, cyclohexanone, and ethyl acetate are particularly preferred. Furthermore, from the perspective of low boiling point and excellent drying efficiency, methyl ethyl ketone and ethyl acetate are preferred. The above-mentioned solvents may be used alone or in any combination and ratio.

[0263] <Adhesive>

[0264] The polyester-based adhesive (hereinafter sometimes referred to as "the present adhesive") in one embodiment of the present invention is obtained by crosslinking the present adhesive composition described above, and has excellent adhesive strength, heat resistance, moisture and heat resistance, and optical properties.

[0265] The term "crosslinking" in the present invention means intentionally crosslinking the adhesive composition by heat and / or light, etc. The degree of crosslinking can be controlled according to the desired physical properties and application.

[0266] The degree of crosslinking can be confirmed by the gel fraction of the present adhesive, and the gel fraction is preferably 20 to 100%, more preferably 30 to 98%, further preferably 40 to 95%, particularly preferably 50 to 90%, particularly preferably 55 to 85%, and most preferably 60 to 80%. If the gel fraction is too low, there is a tendency for heat resistance, holding power, adhesive strength, and wet heat durability to become insufficient, and if it is too high, there is a tendency for tackiness and adhesive strength to become insufficient.

[0267] It should be noted that the gel fraction is an index of the degree of crosslinking, and is calculated, for example, by the following method. That is, an adhesive sheet (an adhesive sheet without a release sheet) formed by forming an adhesive layer on a polymer sheet (such as a PET film) serving as a substrate is covered with a 200-mesh SUS metal mesh, immersed in toluene at 23°C for 24 hours, and the mass percentage of the undissolved adhesive component remaining in the metal mesh after the immersion relative to the mass of the adhesive component before the immersion is taken as the gel fraction. The mass of the substrate is subtracted.

[0268] Therefore, a pressure-sensitive adhesive layer formed from the present pressure-sensitive adhesive can be obtained, and a pressure-sensitive adhesive sheet having the pressure-sensitive adhesive layer can be obtained.

[0269] It should be noted that the "sheet" described in the present invention also includes the meaning of "film" and "tape".

[0270] <Adhesive Sheet>

[0271] The pressure-sensitive adhesive sheet according to one embodiment of the present invention (hereinafter also referred to as “the present pressure-sensitive adhesive sheet”) can be produced, for example, in the following manner.

[0272] The adhesive sheet can be produced according to a commonly known method for producing an adhesive sheet. For example, the adhesive composition is applied to a substrate and dried and cross-linked, a release sheet is attached to the adhesive layer on the opposite side of the substrate, and the adhesive layer is aged as needed to obtain the adhesive sheet having an adhesive layer containing an adhesive on the substrate.

[0273] The adhesive layer is preferably formed on one or both sides of the substrate.

[0274] Alternatively, the present adhesive sheet can be obtained by coating the present adhesive composition on a release sheet, drying and crosslinking the composition, laminating a substrate on the adhesive layer opposite to the release sheet, and aging the composition as required.

[0275] Alternatively, a double-sided PSA sheet without a substrate can be produced by forming a PSA layer on a release sheet and bonding a release sheet to the PSA layer on the opposite side.

[0276] When the obtained PSA sheet or substrate-free double-sided PSA sheet of the present invention is used, the release sheet is peeled off from the PSA layer, and the PSA layer is bonded to an adherend.

[0277] Examples of the substrate include polyester resins such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymers; polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; polyvinyl fluoride resins such as polyvinylidene fluoride and polytetrafluoroethylene; polyamides such as nylon 6 and nylon 6,6; vinyl polymers such as polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymers, ethylene-vinyl acetate copolymers, ethylene-vinyl alcohol copolymers, polyvinyl alcohol, and vinylon; cellulose triacetate, cellulose styrene, and polyvinyl chloride. Cellulose resins such as Lupyron; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; fluorine resins; polystyrene; polycarbonate; acrylonitrile-butadiene-styrene copolymer; acrylonitrile-styrene-acrylate copolymer; polyarylate; polyimide; cycloolefin polymer: a sheet consisting of at least one synthetic resin selected from the group consisting of urethane acrylate resins, etc.; metal foils of aluminum, copper, and iron; paper such as high-quality paper and cellophane; fabrics and nonwoven fabrics consisting of glass fibers, natural fibers, synthetic fibers, etc. These substrates can be used as a single layer or as a multilayer body formed by laminating two or more types.

[0278] Among these, particularly preferred are substrates composed of polyethylene terephthalate, acrylic resins, polycarbonate, acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene-acrylate copolymers, polyimide, and urethane acrylate resins. In particular, from the viewpoint of excellent heat resistance and molding processability, preferred are acrylic resins, fluorine resins, and urethane acrylate resins.

[0279] In addition, as the aforementioned substrate, for example, a foam sheet consisting of a foam substrate, for example, a foam of a synthetic resin such as polyurethane foam, polyethylene foam, polyacrylate foam, etc. can be used. Among these, polyurethane foam and polyacrylate foam are preferred from the viewpoint of excellent balance in heat resistance, followability to adherends, and bonding strength.

[0280] The thickness of the substrate is, for example, preferably 1 to 1000 μm, particularly preferably 10 to 800 μm, further preferably 25 to 600 μm, and particularly preferably 50 to 400 μm.

[0281] As the release sheet, for example, a sheet, paper, cloth, nonwoven fabric, etc. made of various synthetic resins exemplified in the above substrates, subjected to a release treatment, can be used. As the release sheet, a silicone-based release sheet is preferably used.

[0282] As a coating method of the present adhesive composition, for example, a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater or the like can be used.

[0283] The aging treatment may be carried out under conditions of 0 to 80° C. and 1 to 30 days, specifically, for example, 1 to 20 days at 23° C., preferably 2 to 14 days at 23° C., particularly preferably 3 to 7 days at 23° C., 1 to 10 days at 40° C., etc. If the aging treatment is carried out at a temperature higher than 80° C., the optical properties of the adhesive sheet may be insufficient or the production efficiency may be reduced due to the thermal history.

[0284] Furthermore, as drying conditions, the drying temperature is preferably 60 to 140° C., particularly preferably 80 to 120° C., and the drying time is preferably 0.5 to 30 minutes, particularly preferably 1 to 5 minutes.

[0285] The thickness of the adhesive layer of the aforementioned adhesive sheet and the double-sided adhesive sheet without substrate is preferably 1 to 500 μm, particularly preferably 3 to 200 μm, further preferably 5 to 100 μm, and particularly preferably 10 to 50 μm. If the thickness of the adhesive layer is too thin, there is a tendency for the adhesive force to decrease, and if it is too thick, there is a tendency for the uniformity of the coating to decrease and the appearance to be poor, or bubbles to be incorporated into the coating and the optical properties to become insufficient.

[0286] The thickness of the PSA layer was determined by subtracting the thickness of the constituent members other than the PSA layer from the thickness of the entire PSA sheet using "ID-C112B" manufactured by Mitutoyo Corporation.

[0287] The haze of the pressure-sensitive adhesive sheet is preferably 3% or less, more preferably 2.5% or less, and particularly preferably 2% or less. When the haze is below the above values, the optical properties tend to be excellent.

[0288] The haze can be determined by pressing the adhesive sheet onto a polyethylene terephthalate (PET) film and an alkali-free glass plate to produce a test piece consisting of a PET film / adhesive layer / alkali-free glass plate, and measuring the test piece at 23°C and 50% RH using a HAZE MATER NDH2000 (manufactured by Nippon Denshoku Industries).

[0289] The molding stability of the PSA sheet can be confirmed by the elongation of the PSA sheet.

[0290] The elongation is preferably 100 to 2000%, more preferably 200 to 1500%, further preferably 300 to 1400%, particularly preferably 400 to 1300%, and particularly preferably 500 to 1200%.

[0291] If the elongation is too low, the adhesive layer will not be able to follow the molded body and the molding stability will tend to be insufficient. If the elongation is too high, the holding power and the wet heat durability will tend to be insufficient.

[0292] The elongation can be determined by subjecting the PSA sheet to a tensile test in accordance with JIS K 7127.

[0293] For example, a substrate-free adhesive sheet having an adhesive layer thickness of 200 μm can be cut into a size of 15 mm in width and 75 mm in length, and the release films on both sides can be peeled off to prepare a test piece. The tensile test can be carried out at 23° C. and 50% RH using an Autograph (manufactured by Shimadzu Corporation, Autograph AG-X) with a width of 15 mm, a distance between clamps of 25 mm, and a tensile speed of 10 mm / min to determine the value.

[0294] And then, as required, this adhesive sheet also can be provided with release sheet in the outside of adhesive layer for protection.In addition, the adhesive sheet that adhesive layer is formed on one side of base material is implemented peeling process by the face of the opposite side with the adhesive layer of base material, and this peeling process face can also be utilized to protect adhesive layer.

[0295] The adhesive can be used for laminating various components and has excellent adhesive strength, heat resistance, moisture and heat resistance, and optical properties. Therefore, it is particularly useful for laminating decorative films, single-sided or double-sided adhesive sheets used in molding, and films for electronic components.

[0296] <Decorative film>

[0297] A decorative film according to one embodiment of the present invention (hereinafter also referred to as “the present decorative film 1 ” in some cases) includes the present pressure-sensitive adhesive sheet.

[0298] Furthermore, a decorative film according to another embodiment of the present invention (hereinafter sometimes referred to as "the present decorative film 2") is a decorative film having an adhesive layer formed of a polyester adhesive composition containing a polyester resin (A) and a polyepoxy compound (B).

[0299] The polyester resin (A) satisfies all of the following conditions (1) to (4).

[0300] (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b).

[0301] (2) The content of the structural unit derived from the cyclic structure-containing polycarboxylic acid (a1) is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a).

[0302] (3) The structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1).

[0303] (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g.

[0304] The polyester resin (A) and the polyepoxy compound (B) used in the above-mentioned present decorative film 2 are the same as those described in the above-mentioned present adhesive composition. In addition, the polyester adhesive composition used in the present decorative film 2 may also contain the polyisocyanate compound (C), carbodiimide compound, metal chelate compound, tackifying resin, antioxidant (D) and additives described in the above-mentioned present adhesive composition.

[0305] Hereinafter, the present decorative films 1 and 2 (hereinafter sometimes simply referred to as “present decorative films”) will be described.

[0306] The present decorative film is a film for imparting design properties to a resin layer formed of a thermoplastic resin or a metal, and the present decorative film comprises at least a substrate and an adhesive layer.

[0307] As the base material in the present decorative film, for example, a resin layer formed of a thermoplastic resin can be cited. As the aforementioned thermoplastic resin, for example, polyethylene terephthalate, acrylic resin, polycarbonate, acrylonitrile-butadiene-styrene copolymer, acrylonitrile-styrene-acrylate copolymer, polyimide acrylic resin, fluorine resin, urethane acrylate resin, etc. can be cited. These can be used alone or in combination of two or more. Among them, acrylic resin, fluorine resin, and urethane acrylate resin are preferred from the viewpoint of excellent ductility, bendability, and shape tracking during molding.

[0308] The base material in the present decorative film may be colorless or colored. When the base material is colored, a known colorant may be added to the resin.

[0309] Furthermore, the base material in the present decorative film may be transparent, translucent or opaque.

[0310] Generally, the thickness of the substrate is preferably 1 to 1000 μm, particularly preferably 10 to 800 μm, further preferably 25 to 600 μm, and particularly preferably 50 to 400 μm. If the thickness of the substrate is within the above range, there is a tendency for the processability, shape followability, and operability to be improved when manufacturing the decorative molded article.

[0311] The present decorative film may also have a decorative layer on the substrate and / or between the substrate and the adhesive layer. The decorative layer is a layer provided to give the decorative film an appearance, and is a pattern layer that expresses patterns, text, and pattern-like patterns. The decorative layer can be provided, for example, by a known printing method such as inkjet printing, screen printing, and gravure printing, or by vapor deposition of metals such as aluminum, chromium, nickel, gold, tin, indium, and copper, or metal oxides.

[0312] The substrate in the decorative film is located at the outermost layer of the decorative molded product after the molded product described below is decorated by the decorative film, and functions as a protective layer of the decorative molded product. By using acrylic resin or urethane acrylate resin to form the substrate, a decorative molded product with excellent durability such as abrasion resistance, chemical resistance, and weather resistance can be obtained.

[0313] <Decorative molding>

[0314] The decorative molded body according to one embodiment of the present invention (hereinafter sometimes referred to as "the present decorative molded body") is formed by laminating the present decorative film on a molded body by vacuum forming, pressure forming (preferably vacuum forming), etc. That is, the present decorative molded body is formed by laminating the present decorative film on a molded body, and more specifically, by laminating an adhesive layer, a decorative layer as required, and a substrate on a molded body.

[0315] Examples of the molded article include a resin layer formed of a thermoplastic resin, and examples of the thermoplastic resin include polyethylene terephthalate, acrylic resin, polycarbonate, acrylonitrile-butadiene-styrene copolymer, and acrylonitrile-styrene-acrylate copolymer.

[0316] <Film for electronic components>

[0317] The film for electronic components according to one embodiment of the present invention is usually composed of the present pressure-sensitive adhesive sheet and a substrate.

[0318] The aforementioned thin film for electronic components is used in the manufacturing process of electronic components, for example, in the semiconductor manufacturing process, it is used for masking, fixing, component protection, and part transportation of electronic components.

[0319] As the substrate in the aforementioned film for electronic components, for example, polyethylene terephthalate resin, polyimide resin, polyphenylene sulfide resin, polyethylene naphthalate resin, polyetheretherketone resin, polyethersulfone resin, polycyclohexane dimethylene terephthalate resin, polyetherimide resin, aromatic polyamide resin, liquid crystal polymer resin, etc. can be listed. These can be used alone or in combination of two or more. Among them, polyethylene terephthalate resin, polyimide resin, and polyphenylene sulfide are preferred from the viewpoint of excellent heat resistance and processability.

[0320] Generally, the thickness of the substrate is preferably 1 to 1000 μm, particularly preferably 3 to 500 μm, further preferably 5 to 300 μm, and particularly preferably 10 to 100 μm. When the thickness of the substrate is within the above range, the heat resistance and processability of the thin film for electromagnetic components tend to be good.

[0321] Example

[0322] The present invention will be described in more detail below by giving examples, but the present invention is not limited to the following examples without departing from the gist of the present invention. It should be noted that "parts" and "%" in the examples are based on mass.

[0323] In addition, the glass transition temperature (°C), acid value (mgKOH / g), content of structural units derived from polycarboxylic acids (a1) containing a cyclic structure relative to structural units derived from polycarboxylic acids (a) (mol%), content of structural units derived from aliphatic polyols (b1) relative to structural units derived from polyols (b) (mol%), content of structural units derived from dimer acids (a2) and / or structural units derived from dimer alcohols (b2) in the polyester resin (A) (mass%), ester bond concentration (mmol / g), crystal fusion heat (J / g), peak top molecular weight (Mp), weight average molecular weight (Mw), and biomass degree (%) were measured according to the description of the present specification.

[0324] <Production of polyester resins (A) and (A')>

[0325] The compositions described in Table 1 below are the composition ratios of the finished products (resin composition ratios), and the relative ratios (molar ratios) and mass % of the amounts of the constituent monomers of the obtained polyester resins (A) and (A').

[0326] [Production of polyester resin (A-1)]

[0327] In a reactor equipped with a thermometer, a stirrer, a distillation tower, and a nitrogen inlet pipe, 124 parts of isophthalic acid (IPA), 104.3 parts of terephthalic acid (TPA), 4 parts of trimellitic anhydride (TMAn) as polycarboxylic acids (a), 39 parts of ethylene glycol (EG) as polyols, 664.2 parts of dimer alcohol "Pripol 2033" (P2033) (manufactured by Croda), 56.6 parts of 2-methyl-1,3-propanediol (2MPG), and 0.1 part of tetrabutyl titanate as a catalyst were added, and the temperature was raised over 2.5 hours until the internal temperature reached 260°C, and an esterification reaction was carried out at 260°C for 1.5 hours.

[0328] Then, 0.1 parts of tetrabutyl titanate was added as a catalyst, and the pressure in the reaction system was reduced to 2.5 hPa, and a polymerization reaction was carried out over 2 hours.

[0329] Furthermore, the temperature was lowered until the internal temperature reached 235°C, 8 parts of trimellitic anhydride (TMAn) was added, and a depolymerization reaction was carried out over 1 hour to obtain a polyester resin (A-1).

[0330] [Production of polyester resins (A-2 to 5, A'-2)]

[0331] Except having changed the resin composition as described in Table 1, it carried out similarly to A-1, and obtained the polyester resin (A-2-5, A'-2).

[0332] [Production of polyester resin (A'-1)]

[0333] Into a reactor equipped with a thermometer, a stirrer, a distillation tower, and a nitrogen inlet pipe, 225.5 parts of terephthalic acid (TPA) as a polycarboxylic acid (a), 126.4 parts of ethylene glycol (EG) as a polyol (b), 646.4 parts of dimer "Pripol 2033" (P2033) (manufactured by Croda), 1.8 parts of trimethylolpropane (TMP), and 0.1 part of tetrabutyl carbonate as a catalyst were added, and the temperature was increased over 2.5 hours until the internal temperature reached 260°C, and an esterification reaction was carried out at 260°C for 1.5 hours.

[0334] Then, 0.1 parts of tetrabutyl carbonate was added as a catalyst, the pressure in the reaction system was reduced to 2.5 hPa, and a polymerization reaction was carried out over 2 hours to obtain a polyester resin (A'-1).

[0335] The resin composition (structural units derived from components) of each obtained polyester-based resin is shown in the following Table 1, and the physical properties are shown in the following Table 2. In addition, in Table 1, each abbreviation is as follows.

[0336] [Polycarboxylic acids (a)]

[0337] [Polycarboxylic acids containing a cyclic structure (a1)]

[0338] "IPA": Isophthalic acid

[0339] "TPA": terephthalic acid

[0340] "TMAn": trimellitic anhydride

[0341] [Dimer acids (a2)]

[0342] ・"P1009": dimer acid "Pripol 1009" (manufactured by Croda) ※Biomass-derived raw material

[0343] [Aliphatic polycarboxylic acids]

[0344] ・"SebA": Sebacic acid ※Biomass-derived raw materials

[0345] [Polyols (b)]

[0346] [Aliphatic polyols (b1)]

[0347] ・"EG": Ethylene glycol ※Biomass-derived raw materials

[0348] "2MPG": 2-methyl-1,3-propanediol

[0349] "3MPG": 3-methyl-1,5-pentanediol

[0350] "TMP": trimethylolpropane

[0351] [Dimer alcohols (b2)]

[0352] · "P2033": dimer alcohol "Pripol 2033" (manufactured by Croda) ※Biomass-derived raw material

[0353] [Table 1]

[0354]

[0355] [Table 2]

[0356]

[0357] <PET resin sheet with release film on one side>

[0358] Each of the obtained polyester resins (A) and (A') was applied to a polyethylene terephthalate (PET) film (manufactured by Toray Industries, Inc., Lumirror T60, thickness 38 μm) so as to have a thickness of about 25 μm after drying, and then dried at 100° C. for 3 minutes to form an adhesive layer. Then, a release-treated PET film (release film) (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-01-BU, thickness 38 μm) was attached to the adhesive layer to protect the surface, thereby obtaining a PET resin sheet with a release film attached to one side.

[0359] <Cross-linking agent>

[0360] As a cross-linking agent, the following compound was prepared.

[0361] (B-1): N,N,N',N'-tetraglycidyl-m-xylenediamine (manufactured by Mitsubishi Gas Chemical Co., Ltd., "TETRADX")

[0362] (C-1): Trimer of isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, "Coronate HX")

[0363] <Antioxidants>

[0364] As antioxidants, the following compounds were prepared.

[0365] (D-1): Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (manufactured by BASF Japan, hindered phenol antioxidant "Irganox 1010")

[0366] <Production of polyester-based adhesive composition>

[0367] The polyester-based adhesive composition was produced as follows using the polyester-based resins (A) and (A′) obtained above and the crosslinking agent.

[0368] (Example 1)

[0369] The polyester resin (A-1) obtained above is diluted with ethyl acetate to a solid content concentration of 50%, and 1.3 parts of a polyepoxy compound (B-1) (solid content) is added to the polyester resin (A-1) solution (100 parts in terms of solid content), and the mixture is stirred and mixed to obtain a polyester adhesive composition.

[0370] (Examples 2 to 5, Comparative Examples 1 to 3)

[0371] In Example 1, except that each component was blended as shown in Table 3, a polyester-based adhesive composition was obtained in the same manner as in Example 1.

[0372] <PET adhesive sheet with release film on one side>

[0373] Each of the obtained polyester-based adhesive compositions was applied to a polyethylene terephthalate (PET) film (manufactured by Toray Industries, Inc., Lumirror T60, thickness 38 μm) so that the thickness after drying was about 25 μm, and then dried at 100° C. for 3 minutes to form an adhesive layer. Then, a release-treated PET film (release film) (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-01-BU, thickness 38 μm) was attached to the adhesive layer to protect its surface, and the adhesive layer was aged for 4 days at a temperature of 40° C. to obtain a PET adhesive sheet with a release film attached to one side.

[0374] The following evaluations were performed on the obtained PET pressure-sensitive adhesive sheet with a release film on one side. The evaluation results are shown in Table 3 described below.

[0375] [Gel ratio]

[0376] The PET adhesive sheet with a release film on one side obtained above was cut into a size of 4 cm×4 cm, and the release film was peeled off. It was covered with a 200-mesh SUS metal mesh and immersed in toluene at 23°C for 24 hours. The mass of the undissolved adhesive component remaining in the metal mesh after deducting the mass of the PET substrate was measured relative to the mass of the adhesive component before immersion, and the mass percentage was calculated as the following calculation formula as the gel fraction (%).

[0377] Gel rate (%)

[0378] =Mass of the undissolved binder component remaining in the metal mesh after immersion / Mass of the binder component before immersion × 100

[0379] [Adhesion (peel strength) (for SUS-BA)]

[0380] Prepare SUS-BA plate as adherend. Cut the PET adhesive sheet with release film on one side obtained above into 25mm×200mm under 23℃, 50%RH environment, peel off the release film, and make 2kg roller reciprocate twice to pressurize the adhesive layer side to the SUS-BA plate. Then, after standing for 30 minutes under the same environment, use Autograph (made by Shimadzu Corporation, AutographAG-X 50N) to measure 180 degree peel strength (N / 25mm) at a peeling speed of 300mm / min.

[0381] (Evaluation Criteria)

[0382] ◎(excellent)…The adhesive force is above 5N / 25mm, and there is no residual adhesive left on the adherend

[0383] 〇(very good)…The adhesive force is 3N / 25mm or more and less than 5N / 25mm, and there is no residual adhesive left on the adherend

[0384] △(good)…The adhesive force is 1N / 25mm or more and less than 3N / 25mm, and there is no residual adhesive left on the adherend.

[0385] ×(poor)…The adhesive force is less than 1N, or there is residual adhesive on the adherend

[0386] [Adhesion (peel strength) (for ABS)]

[0387] The PET adhesive sheet with a release film on one side obtained above was cut into 25 mm×200 mm at 23°C and 50% RH, the release film was peeled off, and the adhesive layer side was pressed and bonded to the SUS-BA plate by rolling back and forth twice with a 2 kg roller.

[0388] Then, after leaving it to stand for 30 minutes under the same environment, the 180-degree peel strength (N / 25 mm) was measured at a peeling speed of 300 mm / min using Autograph (Autograph AG-X 50N manufactured by Shimadzu Corporation).

[0389] (Evaluation Criteria)

[0390] ◎(excellent)…The adhesive force is above 5N / 25mm, and there is no residual adhesive left on the adherend

[0391] 〇(very good)…The adhesive force is 3N / 25mm or more and less than 5N / 25mm, and there is no residual adhesive left on the adherend

[0392] △(good)…The adhesive force is 1N / 25mm or more and less than 3N / 25mm, and there is no residual adhesive left on the adherend.

[0393] ×(poor)…The adhesive force is less than 1N, or there is residual adhesive on the adherend

[0394] [Optical properties (H1: haze of resin sheet)]

[0395] The PET resin sheet with a release film on one side obtained above was cut into a size of 30 mm × 50 mm under an environment of 23°C and 50% RH, and then the release film was peeled off and a 2 kg roller was reciprocated twice to press the adhesive layer side onto an alkali-free glass (EAGLE XG manufactured by Corning Incorporated) to prepare a test piece consisting of a PET film / polyester resin layer / alkali-free glass plate.

[0396] The haze (H1) of the test piece was measured in an environment of 23° C. and 50% RH using HAZE MATER NDH2000 (manufactured by Nippon Denshoku Industries Co., Ltd.).

[0397] [Optical properties (H2: Haze of adhesive sheet)]

[0398] The PET adhesive sheet with a release film on one side obtained above was cut into a size of 30 mm × 50 mm under an environment of 23°C and 50% RH, and then the release film was peeled off. The adhesive layer side was pressed and adhered to an alkali-free glass (EAGLE XG manufactured by Corning Incorporated) by rolling back and forth twice with a 2 kg roller to prepare a test piece consisting of a PET film / adhesive layer / alkali-free glass plate.

[0399] The haze (H2) of the test piece was measured under an environment of 23° C. and 50% RH using HAZE MATER NDH2000 (manufactured by Nippon Denshoku Industries, Ltd.).

[0400] [Optical properties (ΔH)]

[0401] The optical properties were evaluated by calculating the haze shift of the polyester resin (A) or (A') and the adhesive prepared by mixing the polyester resin (A) or (A') with a polyepoxy compound (B) or a polyisocyanate compound (C) using the following formula.

[0402] Haze displacement (ΔH) = adhesive sheet haze (H2) - resin sheet haze (H1)

[0403] (Evaluation Criteria)

[0404] ◎(excellent)…Haze displacement is less than 0.1

[0405] 0(very good)…haze shift greater than 0.1 and less than 0.5

[0406] △(good)…haze shift is greater than 0.5 and less than 1.0

[0407] ×(poor)…haze shift greater than 1.0

[0408] <PI adhesive sheet with release film on one side>

[0409] Each of the obtained polyester adhesive compositions was applied to a polyimide (PI) film (manufactured by DU PONT-TORAY CO., LTD., Kapton 200H, thickness 50 μm) in a manner to have a thickness of about 25 μm after drying, and then dried at 100° C. for 3 minutes to form an adhesive layer. Then, a release-treated PET film (release film) (manufactured by Mitsui Chemicals Tohcello, Inc., SP-PET-01-BU, thickness 38 μm) was attached to the adhesive layer to protect its surface, and the adhesive layer was aged for 4 days at a temperature of 40° C. to obtain a PI adhesive sheet with a release film attached to one side.

[0410] The following evaluations were performed on the obtained PI pressure-sensitive adhesive sheet with a release film on one side. The evaluation results are shown in Table 3 described below.

[0411] [Heat resistance]

[0412] The release film of the PI adhesive sheet with a release film on one side obtained above was peeled off, and the sheet was attached to a copper foil at 23°C and 50% RH. The sheet was cut into a size of 2.0×2.0 cm and then heat treated at 130°C for 1 hour to prepare a test piece consisting of copper foil / adhesive layer / PI.

[0413] The test piece was floated in a solder bath at a predetermined temperature (300° C., 320° C.) for 60 seconds with the PI film facing upward to measure heat resistance.

[0414] (Evaluation Criteria)

[0415] ◎(excellent)…No appearance change

[0416] ×(poor)…There are changes in appearance such as floating or peeling

[0417] [Moisture and heat resistance]

[0418] Prepare SUS-BA plate as adherend. Cut the PET adhesive sheet with release film on one side obtained above into 25mm×200mm under 23℃, 50%RH environment, peel off the release film, and make 2kg roller reciprocate twice to pressurize and stick the adhesive layer side to SUS-BA plate. Then, let it stand for 500 hours under 85℃, 85%RH environment, and then let it stand for 1 hour under 23℃, 50%RH environment, and then use Autograph (made by Shimadzu Corporation, AutographAG-X 50N) to measure 180 degree peel strength (N / 25mm) at a peeling speed of 300mm / min.

[0419] (Evaluation Criteria)

[0420] ◎(excellent)…The adhesive force is above 10N / 25mm, and there is no residual adhesive left on the adherend

[0421] 〇(very good)…The adhesive force is 5N / 25mm or more and less than 10N / 25mm, and there is no residual adhesive left on the adherend

[0422] △(good)…The adhesive force is 3N / 25mm or more and less than 5N / 25mm, and there is no residual adhesive left on the adherend.

[0423] ×(poor)…The adhesive force is less than 3N, or there is residual adhesive on the adherend

[0424] [Table 3]

[0425]

[0426] According to the results in Table 3, in the present invention, the polyester-based adhesive compositions and adhesive sheets of Examples 1 to 5 have excellent adhesive strength, heat resistance, and moisture-heat resistance in the adhesive layers, and also have excellent optical properties.

[0427] In contrast, although the adhesive layers of the adhesive compositions and adhesive sheets of Comparative Examples 1 to 3 were excellent in optical properties, they were inferior in at least one of adhesive strength, heat resistance, and moist heat resistance and could not satisfy the purpose of the present invention.

[0428] It should be noted that the above embodiments show specific aspects of the present invention, but the above embodiments are merely examples and are not to be construed as limiting. Various changes that are obvious to those skilled in the art are within the scope of the present invention.

[0429] Industrial Applicability

[0430] The polyester adhesive composition of the present invention is excellent in adhesive strength, heat resistance, moisture and heat resistance, and optical properties when used as an adhesive, and is particularly effective as an adhesive for decorative films and films for electronic components.

Claims

1. A polyester adhesive composition comprising a polyester resin (A) and a polyepoxy compound (B), The polyester resin (A) satisfies all of the following conditions (1) to (6): (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b); (2) the content of the structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a); (3) the structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1); (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g; (5) The glass transition temperature of the polyester resin (A) is -75 to -20°C; (6) The structural unit derived from the cyclic ester in the polyester resin (A) accounts for less than 140 mol % based on 100 mol % of the structural unit derived from the polycarboxylic acid (a).

2. The polyester adhesive composition according to claim 1, in, The structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is a structural unit derived from a monocyclic polycarboxylic acid (a1-1).

3. The polyester adhesive composition according to claim 1 or 2, in, The structural unit derived from the aliphatic polyol (b1) includes a structural unit derived from a polyol having a hydrocarbon group in at least one side chain.

4. The polyester adhesive composition according to any one of claims 1 to 3, in, The polyester resin (A) has a structural unit derived from dimer acids (a2) and / or a structural unit derived from dimer alcohols (b2).

5. The polyester adhesive composition according to any one of claims 1 to 4, in, The content of the structural unit derived from the aliphatic polyol (b1) is 5 to 80 mol% relative to 100 mol% of the structural unit derived from the polyol (b).

6. The polyester adhesive composition according to any one of claims 1 to 5, in, The structural unit derived from the polyols (b) includes a structural unit derived from the dimer alcohols (b2).

7. The polyester adhesive composition according to any one of claims 1 to 6, in, The total content of the structural unit derived from the dimer acid (a2) and the structural unit derived from the dimer alcohol (b2) is 20 to 90% by mass based on the entire polyester resin (A).

8. The polyester adhesive composition according to any one of claims 1 to 7, in, The polyester resin (A) has an ester bond concentration of 1.5 to 8.0 mmol / g.

9. The polyester adhesive composition according to any one of claims 1 to 8, in, The crystal fusion heat of the polyester resin (A) is 3 J / g or less.

10. The polyester adhesive composition according to any one of claims 1 to 9, in, The polyepoxy compound (B) includes a nitrogen atom-containing polyepoxy compound.

11. The polyester adhesive composition according to any one of claims 1 to 10, in, The equivalent weight of the epoxy group of the polyepoxy compound (B) relative to the carboxyl group of the polyester resin (A) is 0.3 to 5 equivalents.

12. The polyester adhesive composition according to any one of claims 1 to 11, in, The content of the polyepoxy compound (B) is 0.1 to 15 parts by mass based on 100 parts by mass of the polyester resin (A).

13. A polyester-based adhesive obtained by crosslinking the adhesive composition according to any one of claims 1 to 12.

14. The polyester adhesive according to claim 13, in, The gel fraction is 20 to 100%. 15 . A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive according to claim 13 or 14 . 16 . The pressure-sensitive adhesive sheet according to claim 15 , which has a haze of 3% or less. 17 . A pressure-sensitive adhesive sheet comprising a substrate and a pressure-sensitive adhesive layer comprising the polyester pressure-sensitive adhesive according to claim 13 , wherein the pressure-sensitive adhesive layer is provided on at least one surface of the substrate. 18 . A decorative film comprising the pressure-sensitive adhesive sheet according to claim 17 .

19. A thin film for electronic components, comprising the pressure-sensitive adhesive sheet according to claim 17.

20. A decorative molded body, comprising: laminating the decorative film according to claim 18 on a molded body.

21. A decorative film comprising an adhesive layer formed from a polyester adhesive composition containing a polyester resin (A) and a polyepoxy compound (B), The polyester resin (A) satisfies all of the following conditions (1) to (4): (1) The polyester resin (A) has a structural unit derived from a polycarboxylic acid (a) and a structural unit derived from a polyol (b); (2) the content of the structural unit derived from the polycarboxylic acid (a1) containing a cyclic structure is 30 mol% or more relative to 100 mol% of the structural unit derived from the polycarboxylic acid (a); (3) the structural unit derived from the polyol (b) contains a structural unit derived from the aliphatic polyol (b1); (4) The acid value of the polyester resin (A) is 1.5 to 30 mgKOH / g.

Citation Information

Patent Citations

  • Thermoplastic polyester elastomer

    JP1994128363A

  • Polyester-based adhesive composition, polyester-based adhesive, adhesive film, adhesive composition for heat resistant adhesive film, heat resistant adhesive film for masking, and use method of heat resistant adhesive film for masking

    JP2019119872A

  • Biofuel battery sensor

    JP2020134344A

  • Adhesive composition and adhesive sheet, laminate, and printed wiring board

    WO2021200713A1