Electronic device manufacturing liquid, method for manufacturing resist pattern, and method for manufacturing device

By using an electronic device manufacturing solution containing anionic surfactants and quaternary ammonium compounds to clean the photosensitive resin layer, the problems of defects and collapse in fine resist patterns were solved, thereby improving the stability and safety of the resist patterns.

CN118891587APending Publication Date: 2024-11-01MERCK PATENT GMBH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380025970.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-09
Filing Date
2023-03-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing technologies suffer from defects, bridging, collapse, uneven width, residues, high surface tension, significant environmental impact, high handling risks, and poor storage stability in fine resist patterns.

Method used

An electronic device manufacturing solution containing anionic surfactants, solvents, and quaternary ammonium compounds is used to form a resist pattern by cleaning and developing the photosensitive resin layer.

Benefits of technology

It reduces defects and collapse in the resist pattern, lowers surface tension, reduces residues, reduces environmental impact and handling hazards, and improves preservation stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891587A_ABST
    Figure CN118891587A_ABST
Patent Text Reader

Abstract

The invention provides an electronic device manufacturing liquid, a method for manufacturing a resist pattern, and a method for manufacturing a device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electronic device manufacturing liquid, a method for manufacturing a resist pattern, and a method for manufacturing a device. Background Art

[0002] In recent years, as the demand for high integration of LSI increases, the refinement of patterns is required. In order to cope with such demand, the lithography process using short-wavelength KrF excimer laser (248nm), ArF excimer laser (193nm), extreme ultraviolet (EUV; 13nm), X-rays, electron beams, etc. is becoming increasingly practical. In order to cope with the refinement of such resist patterns, during fine processing, high resolution is also required for the photosensitive resin composition used as a resist. By exposing with short-wavelength light, a finer pattern can be formed, but due to the production of very fine structures, the yield rate such as the collapse of fine patterns becomes a problem.

[0003] Based on such a situation, Patent Document 1 studies a rinsing liquid for lithography which, like a conventional system containing a surfactant, has excellent performances such as pattern collapse margin, defect, and LWR, and also has excellent characteristics in terms of melting.

[0004] In addition, as another attempt, the use of a fluorine-containing surfactant has also been studied (Patent Documents 2 and 3).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-219577

[0008] Patent Document 2: International Publication No. 2018 / 095885

[0009] Patent Document 3: International Publication No. 2017 / 220479 Summary of the invention

[0010] Technical Problems to be Solved by the Invention

[0011] The inventors of the present invention believe that there are still one or more issues that need to be improved. These issues can be listed as follows: reducing defects in fine resist patterns; suppressing the occurrence of bridges in resist patterns; preventing resist pattern collapse in fine resist patterns; suppressing unevenness in resist pattern width; reducing residues after removing electronic device manufacturing liquid; reducing the surface tension of electronic device manufacturing liquid; providing electronic device manufacturing liquid with less environmental impact; providing electronic device manufacturing liquid with low handling risk; providing electronic device manufacturing liquid with excellent storage stability (e.g., long-term storage); providing electronic device manufacturing liquid with less impact on resist patterns.

[0012] The present invention is completed based on the above-mentioned technical background, and thus provides an electronic device manufacturing liquid.

[0013] Solutions for solving technical problems

[0014] The electronic device manufacturing liquid of the present invention at least comprises:

[0015] Anionic surfactant (A), solvent (B), and quaternary ammonium compound (C).

[0016] The method for producing a resist pattern of the present invention uses the above-mentioned electronic device manufacturing liquid.

[0017] The method for manufacturing a resist pattern of the present invention comprises the following steps:

[0018] (1) applying a photosensitive resin composition onto a substrate via one or more intermediate layers or without an intermediate layer to form a photosensitive resin layer;

[0019] (2) exposing the photosensitive resin layer to radiation;

[0020] (3) developing the exposed photosensitive resin layer; and

[0021] (4) The developed layer is washed with the above-mentioned electronic device manufacturing liquid.

[0022] The method for manufacturing a device of the present invention includes the above-mentioned method for manufacturing a resist pattern.

[0023] Effects of the Invention

[0024] By using the electronic device manufacturing liquid of the present invention, one or more of the following effects can be expected.

[0025] In fine resist patterns, defects can be reduced. Bridging can be suppressed in resist patterns. In fine resist patterns, collapse of resist patterns can be prevented. Unevenness in the width of resist patterns can be suppressed. Residues can be reduced after removing electronic device manufacturing liquid. Surface tension of electronic device manufacturing liquid can be reduced. Environmental impact of electronic device manufacturing liquid can be reduced. Danger of handling electronic device manufacturing liquid can be reduced. Storage stability of electronic device manufacturing liquid can be improved. Impact of electronic device manufacturing liquid on resist patterns can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram showing the state where the resist wall is washed away. DETAILED DESCRIPTION

[0027] The embodiments of the present invention are described in detail below.

[0028] definition

[0029] In this specification, unless otherwise specified or mentioned, the definitions and examples described in this paragraph shall apply.

[0030] The singular includes the plural, and “a” and “the” mean “at least one.” An element of a certain concept may be expressed in plural forms, and when the amount (eg, mass % or mol %) thereof is described, the amount means the total of the plural types.

[0031] "And / or" includes all combinations of elements and also includes individual uses.

[0032] When "to" or "- / to" is used to express a numerical range, both endpoints are included and the units are common. For example, 5 to 25 mol% means 5 mol% or more and 25 mol% or less.

[0033] “C x-y ”, “C x ~C y ” and “C x " refers to the number of carbon atoms in a molecule or substituent. For example: C 1-6 The alkyl group means an alkyl chain having 1 to 6 carbon atoms (such as methyl, ethyl, propyl, butyl, pentyl, and hexyl).

[0034] In the case where the polymer has multiple repeating units, these repeating units are copolymerized. These copolymerizations can be alternating copolymerization, random copolymerization, block copolymerization, graft copolymerization, or any of these mixed forms. When the polymer or resin is represented by a structural formula, n, m, etc. outside the brackets represent the number of repetitions.

[0035] The unit of temperature is Celsius. For example, 20 degrees means 20 degrees Celsius.

[0036] The additive refers to the compound itself having the function (for example, if it is a base generator, it is the compound itself that generates the base). It can also be a method in which the compound is dissolved or dispersed in a solvent and added to the composition. As one embodiment of the present invention, these solvents are preferably contained in the composition of the present invention as solvent (B) or other components.

[0037] <Electronic equipment manufacturing fluid>

[0038] The electronic device manufacturing liquid of the present invention contains at least an anionic surfactant (A), a solvent (B), and a quaternary ammonium compound (C).

[0039] Among them, the electronic device manufacturing liquid is used in the manufacturing process of the electronic device. As long as it can be used in the manufacturing process of the electronic device, it can also be removed or disappear during the process. As electronic devices, display devices, LEDs or semiconductor devices can be listed.

[0040] The electronic device manufacturing liquid is preferably an electronic device manufacturing aqueous solution, more preferably a semiconductor substrate manufacturing aqueous solution, more preferably a semiconductor substrate manufacturing process cleaning liquid, further preferably a photolithography cleaning liquid, and further preferably a resist pattern cleaning liquid. In one embodiment of the present invention, the electronic device manufacturing liquid is a rinsing composition used to rinse the exposed and developed resist pattern.

[0041] Anionic surfactant (A)

[0042] The electronic device manufacturing liquid of the present invention contains an anionic surfactant (A) (hereinafter referred to as component (A); the same applies to other components). Component (A) is not particularly limited as long as it is a compound having a lipophilic group and a hydrophilic group and the hydrophilic part is dissociated into anions.

[0043] One of the effects of the component (A) is that it contributes to preventing pattern collapse after the development of the resist pattern. This is considered to be because the surface activity of the component (A) increases the contact angle between the resist pattern and the electronic device manufacturing liquid.

[0044] (A) As a hydrophilic group of a component, a carboxylate, a sulfonate, a sulfate ester salt, a phosphate ester salt etc. are mentioned, for example, A carboxylate is preferable.

[0045] The component (A) is preferably a carboxyl group-containing compound, more preferably an alkyl carboxylic acid compound, and still more preferably a compound represented by the formula (a).

[0046] Formula (a) is as follows.

[0047] R a1 -COOH(a)

[0048] In formula (a),

[0049] R a1 C 3-12 Alkyl, preferably a linear or branched C 3-10 Alkyl, more preferably a linear or branched C 3-9 Alkyl, more preferably a straight chain or branched C 3-8 alkyl.

[0050] It is believed that the alkyl group in formula (a) can reduce the surface tension of the electronic device manufacturing liquid, and the carboxyl group can improve the solubility of the electronic device manufacturing liquid, thereby achieving a better balance between solubility and low surface tension.

[0051] Specific examples of the component (A) include 2-methylpropionic acid, n-butyric acid, 2-methylbutyric acid, n-pentanoic acid, n-hexanoic acid, n-heptanoic acid, n-octanoic acid, 2-methylpentanoic acid, 2-methylhexanoic acid, 5-methylhexanoic acid, 2-methylheptanoic acid, 4-methyl-n-octanoic acid, 2-ethylhexanoic acid, 2-propylpentanoic acid, 2,2-dimethylpentanoic acid, and 3,5,5-trimethylhexanoic acid.

[0052] The content of the component (A) is preferably 0.01 to 10% by mass, more preferably 0.02 to 5% by mass, and even more preferably 0.02 to 1% by mass based on the electronic device manufacturing liquid.

[0053] Solvent (B)

[0054] The electronic device manufacturing liquid of the present invention contains a solvent (B). The solvent (B) preferably contains water. The water is preferably deionized water.

[0055] Considering the use in the manufacturing process of electronic devices, the solvent (B) preferably has less impurities. The impurity concentration of the solvent (B) is preferably 1 ppm or less, more preferably 100 ppb or less, and even more preferably 10 ppb or less.

[0056] The content of water based on solvent (B) is preferably 90 to 100 mass %, more preferably 98 to 100 mass %, further preferably 99 to 100 mass %, and further preferably 99.9 to 100 mass %. As a preferred embodiment of the present invention, solvent (B) substantially only contains water. However, the mode contained in the electronic device manufacturing liquid of the present invention under the state that the additive is dissolved and / or dispersed in a solvent other than water is allowed as a preferred mode of the present invention. As a further preferred mode of the present invention, the content of water contained in solvent (B) is 100 mass %.

[0057] As a specific example of the solvent (B) other than water, for example, preferably cyclohexanone, cyclopentanone, propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol 1-monomethyl ether 2-acetate (PGMEA), propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, γ-butyrolactone, ethyl lactate, or a mixture thereof. These solvents are preferred in terms of the storage stability of the solution. These solvents may also be used in combination of two or more.

[0058] The content of the component (B) is preferably 80 to 99.99% by mass, more preferably 90 to 99.99% by mass, further preferably 95 to 99.99% by mass, and further preferably 98 to 99.99% by mass based on the electronic device manufacturing liquid.

[0059] The content of water in the solvent (B) is preferably 80 to 99.99% by mass, more preferably 90 to 99.99% by mass, further preferably 95 to 99.99% by mass, and further preferably 98 to 99.99% by mass based on the electronic device manufacturing liquid.

[0060] Quaternary ammonium compounds (C)

[0061] The electronic device manufacturing liquid of the present invention contains a quaternary ammonium compound (C).

[0062] (C) As a component, a quaternary ammonium hydroxide is mentioned, for example.

[0063] It is believed that the electronic device manufacturing liquid can significantly improve the defect prevention effect or collapse prevention effect by including the component (C). Although not being limited by theory, it is believed that the component (C) has a strong alkalinity and thus has a large effect of ionizing the component (A).

[0064] The component (C) is preferably a quaternary ammonium hydroxide, and more preferably represented by the following formula (c).

[0065]

[0066] In formula (c),

[0067] R c1 , R c2 , R c3 , and R c4 Each independently is:

[0068] -halogen;

[0069] - unsubstituted or substituted by halogen, C 3-25 Cycloalkyl, C 4-25 Aryl or hydroxy substituted straight or branched chain C 1-25alkyl;

[0070] - unsubstituted or substituted with halogen, straight-chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl, C 4-25 Aryl or hydroxy substituted straight or branched chain C 2-25 alkenylene;

[0071] - unsubstituted or substituted with halogen, straight-chain or branched C 1-25 Alkyl, C 4-25 Aryl or hydroxy substituted C 3-25 Cycloalkyl; or

[0072] - unsubstituted or substituted with halogen, straight-chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl or hydroxy substituted C 4-25 In the present invention, an alkenylene group refers to a divalent hydrocarbon group having one or more double bonds.

[0073] Preferred R c1 , R c2 , R c3 , and R c4 Each independently is:

[0074] - unsubstituted or substituted with phenyl or hydroxyl straight chain or branched C 1-18 alkyl;

[0075] - unsubstituted, or replaced by straight-chain or branched C 1-5 Alkyl or hydroxy substituted C 5-15 Cycloalkyl; or

[0076] - unsubstituted, or replaced by straight-chain or branched C 1-5 Alkyl or hydroxy substituted C 6-12 Aryl.

[0077] More preferably R c1 , R c2 , R c3 , and R c4 Each is independently methyl, ethyl, propyl, butyl, hexadecyl, hydroxyethyl, benzyl, adamantyl, or phenyl.

[0078] R c1 , R c2 , R c3 , and R c4 The total number of carbon atoms contained in is preferably 4-25, more preferably 4-20.

[0079] R c1 , R c2 , R c3 , and R c4Although all of them may be different, preferably 3 or 4 are the same and the rest are different.

[0080] Specific examples of the component (C) include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrahexylammonium hydroxide, hexadecyltrimethylammonium hydroxide, 2-hydroxyethyltrimethylammonium hydroxide, trimethylphenylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, and N,N,N-trimethyl-1-adamantylammonium hydroxide.

[0081] The content of the component (C) is preferably 0.00001 to 1% by mass, more preferably 0.0001 to 0.1% by mass, and even more preferably 0.0002 to 0.01% by mass based on the electronic device manufacturing liquid.

[0082] The electronic device manufacturing liquid of the present invention mainly contains the above-mentioned (A), (B) and (C) components, but may contain other components as needed, which are described in detail below. It should be noted that the components other than (A), (B) and (C) (in the case of multiple components, the sum) in the composition as a whole are preferably 0 to 10% by mass, more preferably 0 to 5% by mass, further preferably 0 to 3% by mass, and further preferably 0 to 1% by mass, based on the electronic device manufacturing liquid. The electronic device manufacturing liquid of the present invention does not contain components other than (A), (B) and (C) (0% by mass) is also a mode of the present invention.

[0083] Compounds containing hydroxyl groups (D)

[0084] The electronic device manufacturing liquid of the present invention may further contain a hydroxyl group-containing compound (D). The hydroxyl group-containing compound (D) is a compound different from the components (A) and (B). The compound may have one or more hydroxyl groups, but preferably has 1 to 3 hydroxyl groups and may be substituted with fluorine. 3-30 The fluorine substitution is to replace H of the compound with F, but the substitution is not to replace H in the hydroxyl group.

[0085] It is considered that the critical size without collapse can be further reduced by further including the component (D).

[0086] The component (D) is preferably represented by the following formula (d):

[0087]

[0088] In formula (d),

[0089] R d1 , R d2 , R d3 , and R d4are independently hydrogen, fluorine, or C 1-5 The alkyl groups are preferably each independently hydrogen, fluorine, methyl, ethyl, tert-butyl, isopropyl or isopentyl, and more preferably each independently hydrogen, methyl or ethyl.

[0090] L d1 and L d2 Each independently is C 1-20 Alkylene, C 1-20 Cycloalkylene, C 2-4 Alkenylene, C 2-4 Alkyne, or C 6-20 Arylene. These groups can also be fluorinated, C 1-5 Alkyl or hydroxyl groups are substituted. Among them, alkenylene refers to a divalent hydrocarbon group having one or more double bonds, and alkynylene refers to a divalent hydrocarbon group having one or more triple bonds. d1 and L d2 Each is independently C which may be substituted with fluorine 1-5 Alkylene, C 2-4 Alkyne group, or phenylene group (C6 arylene group). d1 and L d2 Each independently is more preferably C substituted by fluorine 2-4 Alkylene, ethynyl (C2 alkynyl) or phenylene, more preferably C2 substituted by fluorine 2-4 Alkylene, ethynyl.

[0091] In another embodiment of the present invention, L d1 and L d2 Also preferably not substituted by fluorine, each independently is C 1-5 Alkylene, C 2-4 alkynylene, or phenylene, more preferably each independently is C 2-4 The alkylene, ethynyl or phenylene groups are each independently C 2-4 Alkylene, ethynyl.

[0092] h is 0, 1, or 2, preferably 0 or 1, and more preferably 0.

[0093] Specific examples of the component (D) include 3-hexyne-2,5-diol, 2,5-dimethyl-3-hexyne-2,5-diol, 3,6-dimethyl-4-octyne-3,6-diol, 1,4-butynediol, 2,4-hexadiyne-1,6-diol, 1,4-butanediol, 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,2,3,3-tetrafluoro-1,4-butanediol, 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol, cis-1,4-dihydroxy-2-butene, and 1,4-benzenedimethanol.

[0094] The content of the component (D) is preferably 0.001 to 10% by mass, more preferably 0.002 to 5% by mass, and even more preferably 0.005 to 1% by mass based on the electronic device manufacturing liquid.

[0095] It is also a preferred embodiment of the present invention that the component (D) is not contained.

[0096] Additives (E)

[0097] The electronic device manufacturing liquid of the present invention may further contain an additive (E) different from components (A) to (D). In the present invention, the additive (E) contains one or more selected from the group consisting of a second surfactant, an acid, an alkali, a bactericide, an antibacterial agent, a preservative, and a mildewcide.

[0098] The second surfactant is a surfactant other than anionic surfactant, for example, nonionic surfactant can be cited. In order to improve the coating property and solubility, the second surfactant can be included in the electronic device manufacturing liquid. Not including the second surfactant is also a preferred embodiment of the present invention.

[0099] In order to adjust the pH value of the treatment liquid or to increase the solubility of each component, an acid or an alkali may be used.

[0100] Bactericides, antimicrobial agents, preservatives, and antifungal agents are used to prevent bacteria or fungi from multiplying over time, and examples thereof include alcohols such as phenoxyethanol and isothiazolone.

[0101] The content of the component (E) is preferably 0.0001 to 10% by mass, more preferably 0.0003 to 0.1% by mass, and even more preferably 0.0005 to 0.01% by mass based on the electronic device manufacturing liquid. Not containing the component (E) is also a preferred embodiment of the present invention.

[0102] The electronic device manufacturing liquid of the present invention is produced by dissolving each component in a solvent and then filtering the solution with a filter to remove impurities and / or insoluble matter.

[0103] <Method for producing resist pattern>

[0104] The present invention also provides a method for manufacturing a resist pattern using the above-mentioned electronic device manufacturing liquid. The photosensitive resin composition (resist composition) used in the method can be either positive or negative, preferably positive. A representative method for manufacturing a resist pattern to which the electronic device manufacturing liquid of the present invention can be applied includes the following steps:

[0105] (1) applying a photosensitive resin composition onto a substrate via one or more intermediate layers or without an intermediate layer to form a photosensitive resin layer;

[0106] (2) exposing the photosensitive resin layer to radiation;

[0107] (3) developing the exposed photosensitive resin layer; and

[0108] (4) The developed layer is washed with the above-mentioned electronic device manufacturing liquid.

[0109] The following is a detailed description.

[0110] First, a photosensitive resin composition is applied (e.g., laminated) on top of a substrate such as a silicon substrate or a glass substrate that has been pre-treated as needed to form a photosensitive resin layer. The lamination can be performed using a known method, but a coating method such as spin coating is preferred. The photosensitive resin composition can also be laminated directly on the substrate, or it can be laminated via one or more intermediate layers (e.g., BARC). In addition, an anti-reflection film (e.g., TARC) can also be laminated on top of the photosensitive resin layer (on the opposite side of the substrate). Layers other than the photosensitive resin layer are described below. By pre-forming an anti-reflection film above or below the photosensitive resin layer, the cross-sectional shape and exposure margin can be improved.

[0111] Representative examples of positive or negative photosensitive resin compositions used in the resist pattern manufacturing method of the present invention include, for example, photosensitive resin compositions comprising quinonediazide-based photosensitizers and alkali-soluble resins, chemically amplified photosensitive resin compositions, and the like. From the viewpoint of forming a high-resolution fine resist pattern, chemically amplified photosensitive resin compositions are preferred, and for example, chemically amplified PHS-acrylate hybrid EUV resist compositions can be cited. These are more preferably positive photosensitive resin compositions.

[0112] Examples of the quinonediazide-based photosensitizer used in the positive-type photosensitive resin composition comprising the quinonediazide-based photosensitizer and the alkali-soluble resin include 1,2-benzoquinonediazide-4-sulfonic acid, 1,2-naphthoquinonediazide-4-sulfonic acid, 1,2-naphthoquinonediazide-5-sulfonic acid, sulfonates or sulfonamides thereof, and examples of the alkali-soluble resin include novolac resins, polyvinylphenol, polyvinyl alcohol, copolymers of acrylic acid or methacrylic acid, etc. Preferred novolac resins include novolac resins produced from one or more phenols such as phenol, o-cresol, m-cresol, p-cresol, and xylenol and one or more aldehydes such as formaldehyde and paraformaldehyde.

[0113] Examples of chemically amplified photosensitive resin compositions include positive chemically amplified photosensitive resin compositions, which include a compound that generates an acid by irradiation with radiation (photoacid generator), and a resin whose polarity increases due to the action of the acid generated by the photoacid generator and whose solubility in a developer changes between an exposed portion and an unexposed portion; or negative chemically amplified photosensitive resin compositions, which include an alkali-soluble resin, a photoacid generator, and a crosslinking agent, wherein crosslinking of the resin based on the crosslinking agent is induced by the action of the acid, and whose solubility in a developer changes between an exposed portion and an unexposed portion.

[0114] As the resin whose polarity increases due to the action of an acid and whose solubility in a developer changes between an exposed portion and an unexposed portion, there can be mentioned a resin having a group that "is decomposed by the action of an acid to generate an alkali-soluble group" in the main chain or side chain of the resin, or in both the main chain and the side chain. Representative examples thereof include a polymer obtained by introducing an acetal group or a ketal group as a protective group into a hydroxystyrene-based polymer (PHS), and a similar polymer obtained by introducing a tert-butoxycarbonyloxy group or a p-tetrahydropyranyloxy group as an acid-decomposable group.

[0115] As the photoacid generator, any substance may be used as long as it is a compound that generates an acid by irradiation with radiation, and examples thereof include: onium salts such as diazonium salts, ammonium salts, phosphonium salts, iodonium salts, sulfonium salts, selenonium salts, and arsenic salts; organic halogen compounds; organic metal / organic halides; photoacid generators having an o-nitrobenzyl type protective group; compounds that generate sulfonic acid by photolysis represented by iminosulfonates, etc.; disulfone compounds; diazoketosulfone; diazodisulfone compounds, etc. In addition, compounds obtained by introducing these groups or compounds that generate an acid by light into the main chain or side chain of a polymer may also be used.

[0116] The chemically amplified photosensitive resin composition may further contain an acid-decomposable dissolution inhibitory compound, a dye, a plasticizer, a surfactant, a photosensitizer, an organic basic compound, and a compound that promotes solubility in a developer, as required.

[0117] The photosensitive resin composition can be coated on a substrate by a suitable coating device or coating method such as a spinner or a coater, and heated on a hot plate to remove the solvent in the photosensitive resin composition to form a photosensitive resin layer. The heating temperature varies depending on the solvent or resist composition used, but is generally 70 to 150° C., preferably 90 to 150° C., and can be carried out for 10 to 180 seconds, preferably 30 to 120 seconds, when a hot plate is used, and can be carried out for 1 to 30 minutes when a clean oven is used.

[0118] In the method for manufacturing the resist pattern of the present invention, the presence of a film or layer other than the photosensitive resin layer may also be allowed. The substrate and the photosensitive resin layer may not be in direct contact, but may be sandwiched by an intermediate layer. The intermediate layer is a layer formed between the substrate and the photosensitive resin layer, also referred to as a lower film. As the lower film, a substrate modified film, a planarization film, a lower anti-reflection film (BARC), an inorganic hard mask intermediate layer (silicon oxide film, silicon nitride film and silicon oxide nitride film) or a close contact film may be cited. Regarding the formation of the inorganic hard mask intermediate layer, reference may be made to Japanese Patent No. 5336306. The intermediate layer may be composed of one or more layers. In addition, an upper anti-reflection film (TARC) may also be formed on the photosensitive resin layer.

[0119] In the method for producing a resist pattern of the present invention, a known method can be used for the layer configuration in accordance with the process conditions, and for example, the following layer configuration can be mentioned.

[0120] Substrate / underlayer film / photosensitive resin layer

[0121] Substrate / planarization film / BARC / photosensitive resin layer

[0122] Substrate / planarization film / BARC / photosensitive resin layer / TARC

[0123] Substrate / planarization film / inorganic hard mask intermediate layer / photosensitive resin layer / TARC

[0124] Substrate / planarization film / inorganic hard mask intermediate layer / BARC / photosensitive resin layer / TARC

[0125] Substrate / planarization film / adhesion film / BARC / photosensitive resin layer / TARC

[0126] Substrate / Substrate modification layer / Planarization film / BARC / Photosensitive resin layer / TARC

[0127] Substrate / Substrate modification layer / Planarization film / Adhesion film / BARC / Photosensitive resin layer / TARC

[0128] These layers can be cured by heating and / or exposure after coating, or can be formed into a film by a known method such as CVD method. These layers can be removed by a known method (etching, etc.), and patterning can be performed using the upper layer as a photomask.

[0129] The photosensitive resin layer is exposed through a prescribed photomask. When other layers are also included (TARC, etc.), they can be exposed together. The wavelength of the radiation (light) used for exposure is not particularly limited, but it is preferably exposed with light with a wavelength of 13.5 to 248 nm. Specifically, KrF excimer laser (wavelength 248 nm), ArF excimer laser (wavelength 193 nm), and extreme ultraviolet light (wavelength 13.5 nm) can be used, and extreme ultraviolet light is more preferred. Their wavelengths allow a range of ±5%, preferably an allowable range of ±1%. After exposure, post-exposure heating (PEB) can also be performed as needed. The temperature of post-exposure heating is 70 to 150°C, preferably 80 to 120°C, and the heating time is 0.3 to 5 minutes, preferably 0.5 to 2 minutes, which can be appropriately selected.

[0130] Next, development is performed using a developer. The development of the resist pattern manufacturing method of the present invention preferably uses a 2.38 mass % (±1% is allowed) tetramethylammonium hydroxide (TMAH) aqueous solution. Surfactants and the like may also be added to these developers. The temperature of the developer is generally 5 to 50° C., preferably 25 to 40° C., and the development time is generally 10 to 300 seconds, preferably 20 to 60 seconds, which can be appropriately selected. The development method may use a known method such as spin immersion (puddle) development.

[0131] As described above, the resist pattern of the present invention includes not only a pattern obtained by exposing and developing a resist film but also a pattern in which the wall is thickened by further coating with another layer or film.

[0132] The resist pattern (photosensitive resin layer after development) prepared up to the above-mentioned process is in an unwashed state. The resist pattern can be cleaned with the electronic device manufacturing liquid of the present invention. The time for the electronic device manufacturing liquid to contact the resist pattern, i.e., the processing time, is preferably more than 1 second. In addition, the processing temperature can be arbitrary. The method for contacting the electronic device manufacturing liquid with the resist can also be arbitrary, for example, by immersing the resist substrate in the electronic device manufacturing liquid, or dripping the electronic device manufacturing liquid onto the surface of the rotating resist substrate.

[0133] In the method for manufacturing resist pattern of the present invention, before and / or after the cleaning treatment using electronic equipment manufacturing liquid, the developed resist pattern can be cleaned with other cleaning liquids. Other cleaning liquids are preferably water, more preferably pure water (DW, deionized water, etc.). The cleaning before the treatment is useful because the developer attached to the resist pattern is cleaned. The cleaning after the treatment is useful because the electronic equipment manufacturing liquid is cleaned. By injecting pure water into the developed resist pattern so as to replace the developer while cleaning the pattern, and then by injecting the electronic equipment manufacturing liquid while maintaining the pattern impregnated with pure water, the method for cleaning the pattern while replacing the developer while cleaning the pattern is a preferred mode of the manufacturing method of the present invention.

[0134] The washing of the electronic device with the aqueous solution can be performed by a known method.

[0135] For example, the resist substrate may be immersed in the electronic device manufacturing liquid, or the electronic device manufacturing liquid may be dropped onto the surface of the rotating resist substrate. These methods may be appropriately combined.

[0136] The narrowest interval between the walls of the resist pattern is one of the conditions where pattern collapse is likely to occur. It becomes a strict condition where the walls of the resist pattern are parallel to each other. In this specification, the distance of the interval at the smallest interval on a circuit unit is taken as the minimum spatial dimension. A circuit unit is preferably a semiconductor in the process described later. In addition, a semiconductor containing one circuit unit in the horizontal direction and a plurality of circuit units in the vertical direction is also preferred. Of course, unlike the test sample, as long as the frequency of occurrence of the narrow interval between the walls is low, the frequency of defects is reduced, thereby reducing the frequency of defective products.

[0137] In the present invention, the minimum space size of the resist pattern in one circuit unit is preferably 10 to 30 nm, more preferably 10 to 20 nm, and further preferably 10 to 17 nm.

[0138] <Method of manufacturing device>

[0139] The method for manufacturing a device of the present invention includes a method for manufacturing a resist pattern using an electronic device manufacturing liquid. Preferably, the method for manufacturing a device of the present invention includes processing a substrate by etching the resist pattern manufactured by the above method as a photomask. After processing, the resist film is peeled off as needed.

[0140] In the manufacturing method of the present invention, by etching with a resist pattern as a photomask, the intermediate layer and / or substrate can be processed. Etching can use known methods such as dry etching or wet etching, and dry etching is more preferred. For example, the resist pattern can be used as an etching mask to etch the intermediate layer, and the obtained intermediate layer pattern can be used as an etching mask to etch the substrate to process the substrate. In addition, the resist pattern can also be used as an etching mask to etch the layer (such as the intermediate layer) below the resist layer while directly etching the substrate. The processed substrate becomes, for example, a patterned substrate. The formed pattern can be used to form wiring on the substrate.

[0141] These layers can be removed preferably by dry etching using O2, CF4, CHF3, Cl2 or BCl3, preferably O2 or CF4. As a preferred embodiment, the method for manufacturing a device of the present invention further includes forming wiring on the processed substrate.

[0142] <Stress applied to the resist wall>

[0143] As described in Namatsu et al. Appl. Phys. Lett. 1995 (66), p2655-2657, or as Figure 1 As schematically shown, the stress applied to the resist pattern wall 1 during rinsing and drying can be expressed by the following equation.

[0144] σ max =(6γcosθ / D)×(H / W) 2

[0145] σ max : Maximum stress applied to the resist wall, γ: Surface tension of the rinse

[0146] θ: contact angle, D: distance between walls

[0147] H: height of the wall, W: width of the wall.

[0148] Their length can be determined by known methods, for example, by SEM photographs.

[0149] From the above formula, it can be seen that short D or short W will cause more stress. In this specification, the spacing dimension 3 is as follows Figure 1 As described, it refers to one unit in the resist pattern unit sequence having W and D.

[0150] This means that the finer the resist pattern required (the narrower the pitch size), the greater the stress applied to the resist pattern. Thus, the finer the pattern becomes, the more severe the conditions become, and more improvements are required for the electronic device manufacturing liquid 2 (such as the rinse composition).

[0151] Preferred embodiments are listed below.

[0152] [Implementation Method 1]

[0153] An electronic device manufacturing liquid comprises at least an anionic surfactant (A), a solvent (B), and a quaternary ammonium compound (C).

[0154] The surfactant (A) is preferably a carboxyl group-containing compound, more preferably an alkyl carboxylic acid compound, and further preferably represented by the formula (a).

[0155] R a1 -COOH formula (a)

[0156] In formula (a), R a1 C 3-12 Alkyl, preferably R a1 C is a straight chain or branched chain 3-10 Alkyl, more preferably a linear or branched C 3-9 Alkyl, more preferably a straight chain or branched C 3-8 alkyl.

[0157] The surfactant (A) is preferably selected from the group consisting of 2-methylpropionic acid, n-butyric acid, 2-methylbutyric acid, n-pentanoic acid, n-hexanoic acid, n-heptanoic acid, n-octanoic acid, 2-methylpentanoic acid, 2-methylhexanoic acid, 5-methylhexanoic acid, 2-methylheptanoic acid, 4-methyl-n-octanoic acid, 2-ethylhexanoic acid, 2-propylpentanoic acid, 2,2-dimethylpentanoic acid, and 3,5,5-trimethylhexanoic acid.

[0158] The solvent (B) preferably contains water, more preferably contains substantially only water, and further preferably contains water in an amount of 100% by mass.

[0159] The electronic device manufacturing liquid is preferably an electronic device manufacturing aqueous solution.

[0160] [Implementation Method 2]

[0161] The electronic device manufacturing liquid according to Embodiment 1, wherein the quaternary ammonium compound (C) is a quaternary ammonium hydroxide.

[0162] The quaternary ammonium compound (C) is preferably represented by formula (c).

[0163]

[0164] In formula (c),

[0165] R c1 , R c2 , R c3 , and R c4 are independently halogen, unsubstituted or substituted with halogen, C 3-25 Cycloalkyl, C4-25 Aryl or hydroxy substituted straight or branched chain C 1-25 Alkyl; unsubstituted or halogenated, straight chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl, C 4-25 Aryl or hydroxy substituted straight or branched chain C 2-25 Alkenylene; unsubstituted or halogenated, straight-chain or branched C 1-25 Alkyl, C 4-25 Aryl or hydroxy substituted C 3-25 Cycloalkyl; or unsubstituted or halogen, straight chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl or hydroxy substituted C 4-25 Aryl, preferably a straight or branched C 1-18 Alkyl; unsubstituted or with straight chain or branched C 1-5 Alkyl or hydroxy substituted C 5-15 Cycloalkyl; or unsubstituted or linear or branched C 1-5 Alkyl or hydroxy substituted C 6-12 The aryl group is more preferably selected from the group consisting of methyl, ethyl, propyl, butyl, hexadecyl, hydroxyethyl, benzyl, adamantyl, and phenyl.

[0166] The quaternary ammonium compound (C) is preferably selected from the group consisting of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, tetrahexylammonium hydroxide, hexadecyltrimethylammonium hydroxide, 2-hydroxyethyltrimethylammonium hydroxide, trimethylphenylammonium hydroxide, benzyltrimethylammonium hydroxide, benzyltriethylammonium hydroxide, and N,N,N-trimethyl-1-adamantylammonium hydroxide.

[0167] [Implementation method 3]

[0168] The electronic device manufacturing liquid according to embodiment 1 or 2, wherein the content of the anionic surfactant (A) is 0.01 to 10% by mass, preferably 0.02 to 5% by mass, and more preferably 0.02 to 1% by mass, based on the electronic device manufacturing liquid.

[0169] Preferably, the content of the solvent (B) is 80 to 99.99% by mass based on the electronic device manufacturing liquid.

[0170] Preferably, the content of water contained in the solvent (B) is 80 to 99.99% by mass based on the electronic device manufacturing liquid.

[0171] Preferably, the content of the quaternary ammonium compound (C) is 0.00001 to 1% by mass, more preferably 0.0001 to 0.1% by mass, and even more preferably 0.0002 to 0.01% by mass, based on the electronic device manufacturing liquid.

[0172] [Implementation Method 4]

[0173] The electronic device manufacturing liquid according to any one of Embodiments 1 to 3, further comprising a hydroxyl group-containing compound (D).

[0174] The hydroxyl group-containing compound (D) is preferably represented by the following formula (d):

[0175]

[0176] In formula (d),

[0177] R d1 , R d2 , R d3 , and R d4 are each independently hydrogen, fluorine, or C 1-5 Alkyl; preferably each independently is hydrogen, fluorine, methyl, ethyl, tert-butyl, isopropyl or isopentyl; more preferably each independently is hydrogen, methyl, or ethyl.

[0178] L d1 and L d2 Each independently is C 1-20 Alkylene, C 1-20 Cycloalkylene, C 2-4 Alkenylene, C 2-4 Alkyne, or C 6-20 Arylene. These groups can be fluorinated, C 1-5 Alkyl or hydroxyl groups are substituted. Among them, alkenylene refers to a divalent hydrocarbon group having one or more double bonds, and alkynylene refers to a divalent hydrocarbon group having one or more triple bonds. d1 and L d2 Each is independently C which may be substituted with fluorine 1-5 Alkylene, C 2-4 More preferably L d1 and L d2 are each independently C substituted by fluorine 2-4 Alkylene, ethynyl (C2 alkynyl) or phenylene, more preferably C2 substituted by fluorine 2-4 Alkylene, ethynyl.

[0179] In another embodiment of the present invention, it is also preferred that L is not substituted with fluorine. d1 and L d2 Each independently is C 1-5 Alkylene, C2-4 More preferably, each independently is C 2-4 alkylene, ethynyl or phenylene; further preferably each independently is C 2-4 Alkylene, ethynyl.

[0180] h is 0, 1, or 2, preferably 0 or 1, and more preferably 0.

[0181] [Implementation method 5]

[0182] The electronic device manufacturing liquid according to any one of Embodiments 1 to 4, further comprising an additive (E).

[0183] in,

[0184] The additive (E) includes one or more selected from the group consisting of a second surfactant, an acid, an alkali, a bactericide, an antibacterial agent, a preservative, and an antifungal agent.

[0185] Preferably, the content of the additive (E) is 0.0001 to 10% by mass, more preferably 0.0003 to 0.1% by mass, and even more preferably 0.005 to 0.01% by mass, based on the electronic device manufacturing liquid.

[0186] [Implementation Method 6]

[0187] The electronic device manufacturing liquid according to any one of Embodiments 1 to 5, which is a semiconductor manufacturing aqueous solution:

[0188] Preferably, the electronic device manufacturing liquid is a semiconductor substrate manufacturing aqueous solution;

[0189] Preferably, the electronic device manufacturing fluid is a semiconductor substrate manufacturing process cleaning fluid;

[0190] Preferably, the electronic device manufacturing fluid is a photolithography cleaning fluid;

[0191] Preferably, the electronic device manufacturing liquid is a resist pattern cleaning liquid; or

[0192] Preferably, the electronic device manufacturing fluid is a rinse composition.

[0193] [Implementation method 7]

[0194] A method for producing a resist pattern, the method comprising using the electronic device manufacturing liquid according to any one of Embodiments 1 to 6.

[0195] [Embodiment 8]

[0196] A method for manufacturing a resist pattern, comprising the following steps:

[0197] (1) applying a photosensitive resin composition onto a substrate via one or more intermediate layers or without an intermediate layer to form a photosensitive resin layer;

[0198] (2) exposing the photosensitive resin layer to radiation;

[0199] (3) developing the exposed photosensitive resin layer; and

[0200] (4) The developed layer is washed with the electronic device manufacturing solution described in any of Embodiments 1 to 6.

[0201] [Implementation Method 9]

[0202] According to the method for producing a resist pattern according to Embodiment 8, the photosensitive resin composition is a chemically amplified photosensitive resin composition, and the exposure is preferably performed using extreme ultraviolet rays.

[0203] [Implementation 10]

[0204] The method for manufacturing a resist pattern according to any one of Embodiments 7 to 9, wherein a minimum space size of the resist pattern in one circuit unit is 10 to 30 nm.

[0205] [Implementation 11]

[0206] A method for manufacturing a device, comprising the method for manufacturing a resist pattern according to any one of Embodiments 7 to 10.

[0207] [Implementation 12]

[0208] The method for manufacturing a device according to Embodiment 11 further comprises etching using the resist pattern manufactured by the method according to any one of Embodiments 7 to 10 as a photomask and processing the substrate.

[0209] [Implementation 13]

[0210] The method for manufacturing a device according to Embodiment 11 or 12, further comprising forming a wiring on the processed substrate.

[0211] The present invention will be described below using various examples, but it should be noted that the present invention is not limited to these examples.

[0212] <Preparation of electronic device manufacturing liquid of Example 101>

[0213] In deionized water, 2-methylbutyric acid was added as component (A) to a concentration of 0.7 mass %, and hexadecyltrimethylammonium hydroxide was added as component (C) to a concentration of 0.005 mass %, and the mixture was stirred. Complete dissolution was confirmed visually. The mixture was filtered (pore size = 10 nm) to obtain the electronic device manufacturing liquid of Example 101.

[0214] <Preparation of electronic device manufacturing liquid of Examples 102 to 109 and Comparative Examples 101 and 102>

[0215] Using the components (A) and (C) described in Table 1, the electronic device manufacturing liquids of Examples 102 to 109 and Comparative Examples 101 and 102 were prepared in the same manner as in the preparation of Example 101 so as to have the concentrations described in Table 1.

[0216] Comparative Example 101 was obtained by filtering deionized water without any addition, and Comparative Example 102 did not contain the component (A).

[0217] [Table 1]

[0218] Table 1

[0219]

[0220] <Evaluation substrate preparation 1>

[0221] A BARC composition (AZ Kr-F17B, Merck Electronics Co., Ltd. (hereinafter referred to as ME)) was applied to a silicon substrate by spin coating and heated on a hot plate at 180°C for 60 seconds to obtain a BARC with a film thickness of 80 nm. A PHS-acrylate chemically amplified resist (DX6270P, ME) was applied thereon and heated on a hot plate at 120°C for 90 seconds to obtain a resist film with a film thickness of 620 nm. The substrate was exposed using a KrF exposure device (FPA3000 EX5, Canon) through a photomask (250 nm line / space 1:1). At this time, the exposure amount was changed to 25 mJ / cm 2 ~40mJ / cm 2 , so that the resulting line width changes.

[0222] Then, PEB was performed on a hot plate at 100°C for 60 seconds, and after a 2.38% by mass TMAH aqueous solution of the developer was flowed in, it was maintained for 60 seconds (inverted and immersed). While the developer was inverted and immersed, water began to flow in, and the developer was replaced with water while the substrate was rotated, and the developer was stopped while it was inverted and immersed with water, and the substrate was allowed to stand for 60 seconds. Then, while the developer was inverted and immersed with water, the aqueous solution of Example 101 prepared above was flowed in, and the electronic device manufacturing liquid of Example 101 was replaced with water while the substrate was rotated, and the electronic device manufacturing liquid of Example 101 was stopped while it was inverted and immersed with the electronic device manufacturing liquid of Example 101, and the substrate was allowed to stand for 10 seconds. The substrate was dried by spin drying for 30 seconds.

[0223] Regarding Examples 102 to 109 and Comparative Example 102, each electronic device manufacturing liquid was used to prepare an evaluation substrate in the same manner as described above.

[0224] Comparative Example 101 is the same as the above-mentioned Example 101 except that the substrate is spin-dried immediately after being spin-covered and immersed in water.

[0225] <Evaluation of Collapse Prevention>

[0226] The evaluation substrate of Preparation 1 was used to evaluate the performance of preventing pattern collapse. The resist pattern was observed using SEM device S-9220 (Hitachi High-Tech) to observe whether there was pattern collapse. The following was used as the evaluation standard. In Comparative Example 101, if the line width was thinner than 190nm, pattern collapse of the resist pattern was confirmed. The results are recorded in Table 1.

[0227] A: In the resist pattern having a line width of 150 nm to 177 nm, pattern collapse was not observed.

[0228] B: Pattern collapse was observed in the resist pattern having a line width of 150 nm to 197 nm.

[0229] C: Pattern collapse was observed in a resist pattern having a line width larger than 200 nm.

[0230] <Preparation of electronic device manufacturing liquid of Examples 201 to 206 and Comparative Examples 201 to 204>

[0231] Using the components (A), (C) and (D) as described in Table 2 at the concentrations described in Table 2, electronic device manufacturing liquids of Examples 201 to 206 and Comparative Examples 201 to 204 were prepared in the same manner as the electronic device manufacturing liquid of Example 101 described above.

[0232] It should be noted that Comparative Example 203 is an example of filtering deionized water without any addition.

[0233] [Table 2]

[0234] Table 2

[0235]

[0236] <Evaluation substrate preparation 2>

[0237] A silicon substrate was treated with hexamethyldisilazane (HMDS) at 90°C for 30 seconds. A PHS-acrylate chemically amplified resist for EUV was applied thereon by spin coating, and heated on a hot plate at 110°C for 60 seconds to obtain a resist film with a thickness of 50 nm. The substrate was exposed via a photomask (16nm line / space 1:1) using an EUV exposure device (NXE: 3400, ASML). At this time, the exposure amount was changed to change the resulting line width. Then, PEB was performed on a hot plate at 100°C for 60 seconds, and after a 2.38% by mass TMAH aqueous solution of the developer was flowed in, it was kept for 30 seconds (spin-up immersion). When the developer was already swirled and immersed, water began to flow in, and the developer was replaced with water while the substrate was rotated, and it was stopped when it was swirled and immersed with water, and it was left to stand for 60 seconds. Then, the electronic device manufacturing liquid of Example 201 was poured into the substrate while the substrate was being submerged in water, and the water was replaced with the electronic device manufacturing liquid of Example 201 while the substrate was being rotated, and the substrate was stopped for 10 seconds while the substrate was being submerged in water. The substrate was spun dry to dry the substrate.

[0238] Regarding the electronic device manufacturing liquids of Examples 202 to 206 and Comparative Examples 201, 202, and 204, evaluation substrates were prepared in the same manner as described above using the respective aqueous solutions.

[0239] Comparative Example 201 is the same as the above-mentioned Example 201 except that the developer is replaced with water and the substrate is spin-dried immediately after being spin-immersed in water.

[0240] <Evaluation of Limiting Pattern Size (16nm Line / Space)>

[0241] The resist pattern formed on the evaluation substrate of Preparation 2 was observed using a length measuring SEM CG5000 (Hitachi High-Tech) to observe whether there was line width or pattern collapse. If the exposure amount increased, the line width became smaller. The minimum line width dimension without pattern collapse was taken as the "limit pattern dimension". The results are recorded in Table 2.

[0242] <Evaluation of LWR (16nm Line / Space)>

[0243] The LWR of the resist pattern formed on the evaluation substrate of Preparation 2 was evaluated. The LWR (Line Width Roughness) of the resist pattern having a line width of 16 nm was measured using a length measurement SEM CG5000. The results are shown in Table 2.

[0244] Description of Reference Numerals

[0245] 1: Resist pattern wall

[0246] 2: Electronic equipment manufacturing fluid

[0247] 3: Spacing size.

Claims

1. An electronic device manufacturing liquid, comprising at least: Anionic surfactant (A), solvent (B), and quaternary ammonium compound (C); in, The surfactant (A) is preferably a compound containing a carboxyl group, more preferably an alkyl carboxylic acid compound, and further preferably represented by formula (a): R a1 -COOH formula (a) In formula (a), R a1 C 3-12 Alkyl, preferably R a1 C is a straight chain or branched chain 3-10 alkyl; The solvent (B) preferably comprises water; or The electronic device manufacturing liquid is preferably an electronic device manufacturing aqueous solution.

2. The electronic device manufacturing liquid according to claim 1, wherein: The quaternary ammonium compound (C) is a quaternary ammonium hydroxide; Preferably, the quaternary ammonium compound (C) is represented by formula (c): In formula (c), R c1 , R c2 , R c3 , and R c4 are independently halogen, unsubstituted or substituted with halogen, C 3-25 Cycloalkyl, C 4-25 Aryl or hydroxy substituted straight or branched chain C 1-25 Alkyl; unsubstituted or halogenated, straight chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl, C 4-25 Aryl or hydroxy substituted straight or branched chain C 2-25 Alkenylene; unsubstituted or halogenated, straight-chain or branched C 1-25 Alkyl, C 4-25 Aryl or hydroxy substituted C 3-25 Cycloalkyl; or unsubstituted or halogen, straight chain or branched C 1-25 Alkyl, C 3-25 Cycloalkyl or hydroxy substituted C 4-25 Aryl.

3. The electronic device manufacturing liquid according to claim 1 or 2, wherein: Based on the electronic device manufacturing liquid, the content of the anionic surfactant (A) is 0.01 to 10% by mass; Preferably, based on the electronic device manufacturing liquid, the content of the solvent (B) is 80 to 99.99% by mass. Preferably, the water content of the solvent (B) is 80 to 99.99% by mass based on the electronic device manufacturing liquid, or Preferably, the content of the quaternary ammonium compound (C) is 0.00001 to 1% by mass, more preferably 0.0001 to 0.1% by mass, based on the electronic device manufacturing liquid. 4 . The electronic device manufacturing liquid according to claim 1 , further comprising a hydroxyl group-containing compound (D).

5. The electronic device manufacturing liquid according to any one of claims 1 to 4, further comprising an additive (E): in, The additive (E) comprises one or more selected from the group consisting of a second surfactant, an acid, a base, a bactericide, an antibacterial agent, a preservative, and an antifungal agent; Preferably, the content of the additive (E) is 0.0001 to 10% by mass based on the electronic device manufacturing liquid.

6. The electronic device manufacturing liquid according to any one of claims 1 to 5, which is a semiconductor manufacturing aqueous solution; Preferably, the electronic device manufacturing liquid is a semiconductor substrate manufacturing aqueous solution; Preferably, the electronic device manufacturing liquid is a semiconductor substrate manufacturing process cleaning liquid; Preferably, the electronic device manufacturing liquid is a photolithography cleaning liquid; or Preferably, the electronic device manufacturing liquid is a resist pattern cleaning liquid. 7 . A method for producing a resist pattern, comprising using the electronic device manufacturing liquid according to claim 1 .

8. A method for manufacturing a resist pattern, comprising the following steps: (1) applying a photosensitive resin composition onto a substrate via one or more intermediate layers or without an intermediate layer to form a photosensitive resin layer; (2) exposing the photosensitive resin layer to radiation; (3) developing the exposed photosensitive resin layer; and (4) The developed layer is washed with the electronic device manufacturing liquid according to any one of claims 1 to 6.

9. The method for producing a resist pattern according to claim 8, wherein: The photosensitive resin composition is a chemically amplified photosensitive resin composition. Preferably, the exposure is performed using extreme ultraviolet rays.

10. The method for producing a resist pattern according to any one of claims 7 to 9, wherein: The minimum space size of the resist pattern in one circuit unit is 10 to 30 nm.

11. A method for manufacturing a device, comprising the method for manufacturing a resist pattern according to any one of claims 7 to 10.

12. The method for manufacturing a device according to claim 11, wherein: Further including: The substrate is processed by etching using the resist pattern produced by the method according to any one of claims 7 to 10 as a photomask.

13. The method for manufacturing a device according to claim 11 or 12, wherein: The method further includes forming wiring on the processed substrate.

Citation Information

Patent Citations

  • Rinse liquid for lithography and pattern formation method using the same

    JP2014219577A

  • A rinse composition, a method for forming resist patterns and a method for making semiconductor devices

    WO2017220479A1

  • A lithography composition, a method for forming resist patterns and a method for making semiconductor devices

    WO2018095885A1