Energy storage device
By using a high aspect ratio carbon network and polyamide binders in lithium-ion batteries, the problems of environmental unfriendliness and unstable contact of traditional binders are solved, and an electrode structure with non-toxic solvent treatment and high conductivity is achieved.
Patent Information
- Application Number
- CN202280077194.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-12
- Filing Date
- 2022-11-14
- Publication Date
- 2024-11-01
AI Technical Summary
The binders used in traditional lithium-ion batteries often require toxic or environmentally unfriendly solvents for processing, and it is difficult to effectively maintain the contact between the active material and the current collector during charging and discharging.
A high aspect ratio carbon network and polyamides or modified polyamides are used as binders to form the active layers of the anode and cathode. The carbon nanotube network provides mechanical support and electrical conductivity pathways, and water-soluble or alcohol-soluble polyamides are used as binder materials.
This technology enables lithium-ion batteries to operate without the need for toxic solvent treatment and maintains good contact between the active material and the current collector during charging and discharging, thereby improving the mechanical properties and conductivity of the electrodes.
Smart Images

Figure CN118891684A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Application Serial No. 63 / 278,782, filed on November 12, 2021, the entire disclosure of which is incorporated herein by reference. Technical Field
[0003] The invention relates to an energy storage device, in particular to a super capacitor and a lithium ion battery and electrodes used therein. Background Art
[0004] Lithium batteries are used in many products, including medical devices, electric vehicles, aircraft, and consumer products such as laptops, cell phones, and cameras. Lithium-ion batteries have dominated the secondary battery market due to their high energy density, high operating voltage, and low self-discharge, and continue to find new uses in products and developing industries.
[0005] Typically, a lithium ion battery ("LIB" or "LiB") comprises an anode, a cathode, and an electrolyte material, such as an organic solvent containing a lithium salt. More specifically, the anode and cathode (collectively referred to as "electrodes") are formed by mixing an anode active material or a cathode active material with a binder and a solvent to form a paste or slurry, which is then coated on a current collector (such as aluminum or copper) and dried to form a film on the current collector. The anode and cathode are then layered or wound and subsequently housed in a pressurized casing containing an electrolyte material, which together form a lithium ion battery.
[0006] The binder is used to adhere the active material to the current collector with a suitable coating. It is important that the binder helps maintain adequate contact between the active material and the current collector. In addition, it is important to select a binder that is mechanically compatible with the electrode active material so that the binder can withstand the degree of expansion and contraction of the electrode active material during charging and discharging of the battery. The binder must also be sufficient to withstand the handling of the electrode when it is installed in the battery housing.
[0007] Therefore, binders such as cellulose binders or cross-linked polymer binders have been used to provide good mechanical properties. However, in conventional electrodes, the selected binders often require environmentally unfriendly or toxic solvents for processing. Summary of the invention
[0008] Disclosed herein is an anode comprising: an active layer comprising a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles disposed in the void spaces within the network, wherein the active material particles contain silicon; and a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative.
[0009] The present invention also discloses a cathode, comprising: an active layer comprising a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles, the plurality of electrode active material particles being arranged in the void spaces within the network; and a polymer additive, the polymer additive being (i) selected from the polyamide family or (ii) at least one of a modified polyamide or a polyamide derivative. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The following is a brief description of the drawings, in which like elements are similarly numbered, and which are presented for the purpose of illustrating exemplary embodiments disclosed herein and not for the purpose of limiting the same.
[0011] Figure 1 is a diagram of an example of an electrode as disclosed herein;
[0012] Figure 2A is a flow chart showing an example of a method that can be used to make an electrode disclosed herein;
[0013] Figure 2B A flowchart depicting an exemplary method of making an anode for an energy storage device;
[0014] Figure 3 is a diagram of an electrode arrangement in a pouch cell device; and
[0015] Figure 4 is an illustration of a schematic cross-sectional view showing the appearance of an energy storage device (ESD). DETAILED DESCRIPTION
[0016] A more complete understanding of the components, methods, and devices disclosed herein may be obtained by reference to the accompanying drawings. These figures are merely schematic illustrations based on convenience and ease of display of the present disclosure, and are therefore not intended to indicate the relative size and dimensions of the device or its components and / or to define or limit the scope of the exemplary embodiments. Although specific terms are used in the following description for clarity, these terms are intended to refer only to the specific structures of the embodiments selected for illustration in the accompanying drawings, and are not intended to define or limit the scope of the present disclosure. In the accompanying drawings and the following description below, it should be understood that the same reference numerals refer to components with the same functions.
[0017] An electrolytic cell is disclosed herein, comprising a housing comprising electrodes (anode and cathode). The housing comprises an electrolyte contacting the anode and cathode. Both electrodes (anode and cathode) comprise a current collector on which an active layer is disposed. The active layer may be disposed on an optional adhesive layer contacting the electrodes.
[0018] Figure 1 1 is a diagram of an example of an electrode (anode or cathode) as disclosed herein. In the example shown, the electrode 100 includes a current collector 102 and an active layer 106. The electrode 100 may optionally include an adhesion layer 104. As an example, the adhesion layer 104 includes a material that promotes adhesion between the current collector 102 and the active layer 106. The active layer 106 includes an electrode active material 110 in a binder, and a conductive element 108. The conductive element may include a high aspect ratio element.
[0019] The current collector 102 is a conductive element. The current collector may include a metal (e.g., a substantially pure metal or a metal alloy). As another example, the current collector 102 may be in the form of a metal strip or a metal foil. For example, the current collector 102 may be an aluminum foil or strip, an aluminum alloy foil or strip, a copper foil or strip, or a copper alloy foil or strip. The thickness of the current collector 102 may be no greater than 15 μm (micrometer), no greater than 10 μm, no greater than 8 μm, or no greater than 5 μm. In some embodiments, the thickness of the current collector may be at least 3 μm at the same time. For example, the thickness of the current collector 102 may be 3 to 15 μm, preferably 6 μm to 10 μm. As another example, the current collector 102 is an aluminum foil or an aluminum alloy foil having a thickness of 5 to 7 μm.
[0020] Active layer 106 comprises a conductive material, a binder material and an electrode active material. The active layer can be manufactured by mixing the conductive material, the binder material and the electrode active material with a solvent to form a mixture. The mixture can be applied directly to the current collector, or applied to an adhesive layer, which can adhere to the current collector. If an adhesive layer is used, it can be conductive. The mixture can be dried to remove the solvent, leaving a solid active layer. The active layers 106 of the anode and cathode will now be described in detail.
[0021] The binder material for both the anode active layer and the cathode active layer is polyamide, preferably water-soluble or alcohol-soluble polyamide. The active material of the anode comprises silicon, while the active material of the cathode is NMC, NCA, NCMA or a combination thereof.
[0022] anode
[0023] As noted above, the anode includes a conductive element, a binder, and an electrode active material mixed together to form a mixture. The mixture is placed on a current collector and dried to form an active layer. The components of the anode active material layer are described in detail below.
[0024] The conductive element (also referred to as the conductive material) may comprise carbon. For example, the conductive element may be a high aspect ratio carbon element. The term "high aspect ratio carbon element" refers to a carbonaceous element whose size in one or more dimensions ("major dimensions") is significantly greater than the size of the element in a lateral dimension ("minor dimension"). The high aspect ratio carbon element may comprise a substantially cylindrical network of carbon atoms. The conductive material may comprise a carbon nanotube or a plurality of carbon nanotube bundles.
[0025] In one embodiment, the conductive material used in the anode may include a graphite sheet. This will be described later.
[0026] The conductive material can form a conductive percolation network (also referred to herein as a network of high aspect ratio carbon elements) that can transmit current between any two separated points on the surface of a solid active layer (wherein there is no solvent). In other words, the current can be transmitted from one surface or end of the active layer to the opposite surface or end by means of physical contact or electronic hopping between the conductive elements in the electrode active layer. The percolation network may include voids between high aspect ratio carbon elements that may contain or accommodate electrode active materials. The high aspect ratio conductive material can be generally oriented in the electrode active layer 106 in a direction substantially parallel to the current collector to facilitate conducting current from one end of the electrode to the other end while still maintaining a certain smaller orientation through the thickness of the active layer.
[0027] The network of high aspect ratio carbon elements includes: a first set of carbon nanotubes, wherein the first set of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; and a second set of carbon nanotubes, wherein the second set of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and the second set of carbon nanotubes has one or more properties different from the first set of carbon nanotubes. In one embodiment, the first set of carbon nanotubes includes multi-walled nanotubes, and the second set of carbon nanotubes includes single-walled nanotubes; and the ratio of the amount by weight of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:1.
[0028] In one embodiment, the first average aspect ratio of the first set of carbon nanotubes is greater than the second average aspect ratio of the second set of carbon nanotubes. In another embodiment, the network of high aspect ratio carbon elements includes a plurality of multi-walled carbon nanotubes, and the length distribution of the plurality of multi-walled carbon nanotubes is biased toward a nominal length of the multi-walled carbon nanotubes. In another embodiment, the nominal length of the multi-walled carbon nanotubes is at least 15 microns.
[0029] In yet another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes and at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 8 microns. In yet another embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes and at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 12 microns. In one embodiment, when both the first set of carbon nanotubes and the second set of carbon nanotubes are swollen by the electrolyte, the first set of carbon nanotubes swells more than the second set of carbon nanotubes.
[0030] The conductive material may be present in the mixture in an amount of 0.1 to 2.0, or 0.15 to 1.2, or 0.3 to 1 weight percent (wt%), based on the total weight of the mixture (the mixture includes the conductive material, the electrode active material, the binder material, and the solvent). The conductive material may be present in the active layer in an amount of 0.2 to 3.5, or 0.3 to 3, or 0.5 to 2 weight percent, based on the total weight of the solids in the active layer (the total weight of the solids includes the conductive material, the binder material, and the electrode active material without the solvent).
[0031] The high aspect ratio carbon element may be single-walled carbon nanotube (SWCNT), double-walled carbon nanotube (DWNT), multi-walled carbon nanotube (MWNT), or a mixture thereof.
[0032] The outer diameter of the single-walled carbon nanotube may be 0.5 to 5.0 nanometers, preferably 1.0 to 3.5 nanometers. The aspect ratio (length to diameter ratio) of the single-walled carbon nanotube may be greater than about 2.0, preferably greater than 5.0, preferably greater than 10.0, greater than 50, and more preferably greater than 100. In an exemplary embodiment, the average aspect ratio of the single-walled carbon nanotube may be 5 to 200.
[0033] The length of the single-walled carbon nanotubes may be greater than 6 nanometers, preferably greater than 10 nanometers, preferably greater than 15 nanometers, preferably greater than 30 nanometers, preferably greater than 50 nanometers, more preferably greater than 100 nanometers, preferably greater than 1 micrometer, preferably greater than 5 micrometers, preferably greater than 10 micrometers, and more preferably greater than 15 micrometers up to at least 200 micrometers. In an exemplary embodiment, the average length of the single-walled carbon nanotubes may be 10 nanometers to 20 micrometers, preferably 20 nanometers to 15 micrometers.
[0034] The single-walled carbon nanotubes may be present in the mixture of the conductive material, the binder material, the electrode active material and the solvent in an amount of 0.1 to 0.3 wt %, preferably 0.15 to 0.25 wt %, based on the total weight of the mixture.
[0035] The single-walled carbon nanotubes are present in the electrode active layer in an amount of 0.2 to 0.6 wt %, preferably 0.3 to 0.5 wt %, based on the total weight of the electrode active layer (conductive material, binder material and electrode active material excluding solvent).
[0036] The number of carbon walls in the multi-walled carbon nanotubes may be 2 or more, 5 or more, 10 or more, 50 or more. The multi-walled carbon nanotubes may include an average of 3 to 15 layers, 4 to 12 layers, 5 to 10 layers, 6 to 8 layers.
[0037] The active layer 106 may include multi-walled carbon nanotubes and single-walled carbon nanotubes. When wetted with an electrolyte in an energy storage device where the electrode 100 is located, the multi-walled carbon nanotubes swell more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte in an energy storage device where the electrode 100 is located, the multi-walled carbon nanotubes can swell at least 15%, or at least 25%, or at least 50% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes can expand at least 15%, or at least 25%, or at least 50% more than the length of the single-walled carbon nanotubes. As another example, the multi-walled carbon nanotubes swell up to 50% when wetted (e.g., the length of the multi-walled carbon nanotubes increases by 50% after being wetted with the electrolyte, and / or the diameter of the multi-walled carbon nanotubes increases by 50% after being wetted, etc.).
[0038] The outer diameter of the multi-walled carbon nanotube may be 2.0 to 50 nanometers, 5.0 to 40 nanometers, or 6 to 10 nanometers. The length of the multi-walled carbon nanotube may be greater than 10 nanometers, greater than 15 nanometers, greater than 30 nanometers, greater than 50 nanometers, greater than 100 nanometers, greater than 500 nanometers, greater than 1 micron, greater than 5 microns, greater than 10 microns, or greater than 15 microns. At the same time, the average length of the multi-walled carbon nanotube may be up to 25 microns or up to 20 microns. In an exemplary embodiment, the average length of the multi-walled carbon nanotube is 10 nanometers to 20 microns or 20 nanometers to 15 microns. The aspect ratio (length to diameter ratio) of the multi-walled carbon nanotube may be greater than 5.0, greater than 10.0, greater than 50, greater than 100, or greater than 500. In one embodiment, the multi-walled carbon nanotube may be a branched nanotube.
[0039] Compared with the multi-walled carbon nanotubes included in the electrodes of the related art, the electrodes including multi-walled carbon nanotubes can be relatively long. It is found that the use of relatively long multi-walled carbon nanotubes in electrodes has beneficial mechanical and / or electrical properties. For example, multi-walled carbon nanotubes provide relatively good power at low density. As another example, shorter multi-walled carbon nanotubes generally do not swell (e.g., expand) like longer multi-walled carbon nanotubes. Therefore, the use of shorter multi-walled carbon nanotubes will lose (or reduce) some beneficial properties related to the swelling of carbon nanotubes. As an extreme example, carbon black will not show swelling because carbon black is only carbon particles without entanglement, such as the entanglement shown by the collection of multi-walled carbon nanotubes. During the calendering process, it is observed that the length of a certain amount of multi-walled carbon nanotubes has a length exceeding the threshold length and therefore has sufficient swelling characteristics. The calendering process is to calender the slurry with a relatively large amount of pressure or force when applied to the foil, which indicates that the collective swelling (e.g., average swelling) of the multi-walled carbon nanotubes in the active layer will meet a specific performance threshold. However, multi-walled carbon nanotubes are generally difficult to process.
[0040] The multi-walled carbon nanotube processing related to the preparation / formation of active layers and / or electrodes is gentler than the processing for the electrodes of the related art. Therefore, the method according to various embodiments can maintain longer multi-walled carbon nanotubes (e.g., fewer multi-walled carbon nanotubes are crushed, fragmented, broken, etc.). In some embodiments, the active layer of the electrode includes a collection of multi-walled carbon nanotubes, and the average length of the collection of multi-walled carbon nanotubes is greater than the average length of the multi-walled carbon nanotubes in the electrodes of the related art. According to various embodiments, the length distribution of the collection of multi-walled carbon nanotubes is biased towards the nominal length of the multi-walled carbon nanotubes. As an example, the nominal length of the multi-walled carbon nanotubes is about 16 microns. For example, multi-walled carbon nanotubes are processed and / or applied in a manner to reduce or minimize the rupture or fracture of multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more biased towards the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 8 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the network of high aspect ratio carbon elements have a length of at least 13 microns.
[0041] According to various embodiments, the length distribution of the collection of multi-walled carbon nanotubes is biased toward the nominal length of the multi-walled carbon nanotubes. For example, the multi-walled carbon nanotubes are processed and / or applied in a manner that reduces or minimizes the cracking or breaking of the multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the network of high aspect ratio carbon elements is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more biased toward the nominal length.
[0042] In some embodiments, at least 75% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are at least 12 microns in length. In some embodiments, at least 75% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are at least 13 microns in length. In some embodiments, at least 50% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are at least 12 microns in length. In some embodiments, at least 50% of the multi-walled carbon nanotubes within a network of high aspect ratio carbon elements are at least 13 microns in length.
[0043] The multi-walled carbon nanotubes may be present in the mixture (the mixture comprises a conductive material, an electrode active material, a binder material and a solvent or a combination of solvents) in an amount of 0.3 to 1.0 wt %, preferably 0.4 to 0.9 wt %, based on the total weight of the mixture. The multi-walled carbon nanotubes are present in the solid anode active layer (the solid active layer comprises a conductive material, a binder material, and an electrode active material without a solvent) in an amount of 0.8 to 2.6 wt %, preferably 1.0 to 1.8 wt %, based on the total weight of the solid anode active material.
[0044] In examples where both multi-walled carbon nanotubes and single-walled carbon nanotubes are used, the ratio of the weight of multi-walled carbon nanotubes to the weight of single-walled carbon nanotubes in the mixture or in the solid active material layer may be at least 2:1.
[0045] In one example, the three-dimensional network of high aspect ratio carbon elements 108 includes carbon nanotubes, and the carbon nanotubes are only multi-walled carbon nanotubes and / or fragments of such carbon nanotubes.
[0046] In another example, the multi-walled carbon nanotubes are present in the mixture or in the solid anode active material layer in an amount at least twice the amount of the single-walled carbon nanotubes, based on the weight of the conductive material.
[0047] The network of the three-dimensional network of high aspect ratio carbon elements 108 may comprise at least 99% carbon by weight.
[0048] In addition to high aspect ratio carbon elements (carbon nanotubes), the conductive material may optionally include graphite flakes, carbon black, or a combination thereof.
[0049] The graphite flakes are preferably high aspect ratio graphite flakes, where at least one dimension is greater than any other dimension. The graphite flakes may be naturally occurring or commercially synthesized flakes. The graphite flakes are particulate and may be oval in shape. The aspect ratio of these graphite flakes may range from 2:1 to 20:1, preferably 5:1 to 12:1. In one embodiment, the graphite flakes may be intercalated with metal ions. In another embodiment, the graphite flakes may be exfoliated flakes.
[0050] The graphite sheet may be present in the solid anode active layer (solid active layer comprises conductive material, binder material, electrode active material without solvent) in an amount of 5 to 65 wt %, preferably 8 to 50 wt %, based on the total weight of the solid anode active material.
[0051] In addition to carbon nanotubes, carbon black can also be used. Carbon black is generally a high specific surface area carbon black having a surface area greater than 50 square meters per gram (m2 / gm), preferably greater than 200m2 / gm, and more preferably greater than 500m2 / gm. An example of a high specific surface area carbon black is KELTJEN Black. Carbon black is optional, and based on the total weight of the solid anode active material, carbon black may be present in the solid anode active layer (solid active layer comprising conductive material, binder material, solvent-free electrode active material) in an amount of 0.5 to 2.0 wt%, preferably 0.8 to 1.6 wt%.
[0052] The three-dimensional network of high aspect ratio carbon elements 108 may include an electrically interconnected network of carbon elements that exhibits connectivity above a percolation threshold and wherein the network defines one or more highly conductive paths greater than 100 μm in length. The percolation threshold is the threshold at which conductive elements contact each other to provide a conductive network measured across any two points on any surface of the network.
[0053] Anode Binder
[0054] In one embodiment, the anode active layer comprises a polymer binder comprising nylon (i.e., polyamide), a polyamide family, or a polyamide derivative. In an exemplary embodiment, the polyamide is a water-soluble polyamide, an alcohol-soluble polyamide, or a combination thereof (i.e., soluble in a combination of water and alcohol). The anode active layer does not include a polymer material that is insoluble in water or alcohol. In other words, the anode active layer does not contain polyamide or any other non-water-soluble polymer binder.
[0055] The polyamide (used in the anode polymer binder and the cathode polymer binder) may include aliphatic polyamides, aromatic polyamides, or combinations thereof. In one embodiment, the polyamide includes the general family of resins known as nylons, characterized by the presence of amide groups (—C(O)NH—). Any amide-containing polymer may be used individually or in combination: nylon-6 and nylon-6,6 are suitable polyamide resins available from various commercial sources. However, other polyamides, such as nylon-4, nylon-4,6 (PA46), nylon-12, nylon-6,10, nylon-6,9, nylon-6,12, nylon-9T, copolymers of nylon-6,6 and nylon-6, nylon 610 (PA610), nylon 11 (PA11), nylon 12 (PA12), nylon 6-3-T (PA6-3-T), polyaramid (PAMXD6), polyphthalamide (PPA) and / or polyether block amides, and others (such as amorphous nylon), may also be useful. Mixtures of various polyamides and various polyamide copolymers are also useful.
[0056] Polyamides can be obtained by many well-known processes, such as those described in U.S. Pat. Nos. 2,071,250; 2,071,251; 2,130,523; 2,130,948; 2,241,322; 2,312,966; and 2,512,606. For example, nylon-6 is the polymerization product of caprolactam. Nylon-6,6 is the condensation product of adipic acid and 1,6-diaminohexane. Similarly, nylon 4,6 is the condensation product between adipic acid and 1,4-diaminobutane. In addition to adipic acid, other useful diacids for preparing nylon include azelaic acid, sebacic acid, dodecanedioic acid, as well as terephthalic acid and isophthalic acid, among others. Other useful diamines include meta-xylene diamine, bis-(4-aminophenyl)methane, bis-(4-aminocyclohexyl)methane; 2,2-bis-(4-aminophenyl)propane, 2,2-bis-(4-aminocyclohexyl)propane, etc. Copolymers of caprolactam with diacids and diamines are also useful.
[0057] Polyamides are generally derived from the polymerization of organic lactams having 4 to 12 carbon atoms. In one embodiment, the lactam is represented by formula (I):
[0058]
[0059] wherein n is 3 to 11. In one embodiment, the lactam is ε-caprolactam with n being equal to 5.
[0060] Polyamides can also be synthesized from amino acids having 4 to 12 carbon atoms. In one embodiment, the amino acid is represented by formula (II):
[0061]
[0062] wherein n is 3 to 11. In one embodiment, the amino acid is ε-aminocaproic acid wherein n is 5. Polyamides can also be obtained by polymerizing aliphatic dicarboxylic acids having 4 to 12 carbon atoms with aliphatic diamines having 2 to 12 carbon atoms. In one embodiment, the aliphatic diamine is represented by formula (III):
[0063] H2N-(CH2) n —NH2(III)
[0064] wherein n is from about 2 to about 12. In one embodiment, the aliphatic diamine is hexamethylenediamine (H2N(CH2)6NH2). In one embodiment, the molar ratio of dicarboxylic acid to diamine is from 0.66 to 1.5. Within this range, it is often advantageous to have a molar ratio greater than or equal to 0.81. In another embodiment, the molar ratio is greater than or equal to 0.96. In yet another embodiment, the molar ratio is less than or equal to 1.22. In yet another embodiment, the molar ratio is less than or equal to 1.04. Examples of polyamides useful in the present invention include nylon 6, nylon 6,6, nylon 4,6, nylon 6,12, nylon 10, or a combination comprising at least one of the foregoing polyamides.
[0065] The molecular weight of the polyamide is greater than 200 g / mol, preferably greater than 500,000 g / mol, preferably greater than 1,000,000 g / mol, and more preferably from 500,000 g / mol to 1,500,000 g / mol.
[0066] In one embodiment, the anode active layer comprises at least 0.5 wt %, preferably 0.5 to 1.5 wt % of the polymer additive. The wt % is based on the total weight of the active layer.
[0067] Anode active material
[0068] In one embodiment, the anode includes an active layer, the active layer including a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles, the plurality of electrode active material particles being disposed in the void spaces within the network, wherein the active material particles contain silicon; and a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) modified polyamide or polyamide derivatives.
[0069] In one embodiment, the silicon contained in the electrode active material particles is in the form of SiO. The silicon contained in the electrode active material is microsilicon. In one embodiment, the silicon contained in the electrode active material is greater than 50 percent by weight of the active layer. The silicon in the electrode active material is at least 80 percent by weight of the active layer.
[0070] Anode Overview
[0071] In one embodiment, the anode includes an active layer, the active layer including a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles, the plurality of electrode active material particles being disposed in the void spaces within the network, wherein the active material particles contain silicon; and a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) modified polyamide or polyamide derivatives.
[0072] In one embodiment, the silicon contained in the electrode active material particles is in the form of SiO. The silicon contained in the electrode active material is microsilicon. In one embodiment, the silicon contained in the electrode active material is greater than 50 percent by weight of the active layer. The silicon in the electrode active material is at least 80 percent by weight of the active layer.
[0073] The network of high aspect ratio carbon elements includes a network of carbon nanotubes; and the network of carbon nanotubes maintains electrical connections between at least a subset of the carbon nanotubes contained in the network during expansion of the silicon.
[0074] The network of high aspect ratio carbon elements includes a network of carbon nanotubes; and the network of carbon nanotubes maintains electrical connections between at least a subset of the carbon nanotubes present in the network during charging and discharging of a battery comprising the electrode. The network of high aspect ratio carbon elements has been described in detail above, and for the sake of brevity, most of which will not be repeated herein. However, some features of the network of high aspect ratio carbon nanotubes in the anode active layer that are different from the corresponding network present in the cathode will be described in detail here.
[0075] In one embodiment, the network of high aspect ratio carbon elements contains graphite particles in the interstices. Graphite is typically present in the anode active layer in an amount up to 10 wt%, preferably up to 5 wt%.
[0076] The multi-walled carbon nanotubes (the first group of carbon nanotubes) are present in the anode active layer in an amount of at least 3 wt%, preferably at least 4.5 wt%, based on the weight of the anode active layer. In one embodiment, the multi-walled carbon nanotubes are present in the anode active layer in an amount of 3 to 5 wt%, based on the weight of the anode active layer.
[0077] The single-walled carbon nanotubes (the second population of carbon nanotubes) are present in the anode active layer in an amount of at least 1.5 wt%, preferably at least 2 wt%, based on the weight of the anode active layer.
[0078] In one embodiment, the weight ratio of the first set of carbon nanotubes (multi-walled carbon nanotubes (including double-walled carbon nanotubes)) to the weight of the second set of carbon nanotubes (single-walled carbon nanotubes) is at least 5:1, preferably at least 9:1.
[0079] In one embodiment, the thickness of the active layer increases after swelling with the electrolyte. In one embodiment, the average amount of thickness increase of the active layer (of the anode or cathode) after wetting with the electrolyte is less than 15% (based on the initial size before wetting with the electrolyte), preferably less than 10%, and preferably less than 5%.
[0080] The first average aspect ratio of the first population of carbon nanotubes is greater than the second average aspect ratio of the second population of carbon nanotubes.The first population of carbon nanotubes has an average aspect ratio of at least 100 up to 1000, preferably 200 to 1000.
[0081] In one embodiment, the network of high aspect ratio carbon elements comprises a collection of multi-walled carbon nanotubes, the collection comprising a plurality of multi-walled carbon nanotubes; the average length of the plurality of multi-walled carbon nanotubes is greater than 5 microns, preferably greater than 10 microns.
[0082] In one embodiment, an energy storage device includes an anode and a cathode, wherein the anode or cathode includes an active layer, the active layer includes a network of high aspect ratio carbon elements, the network including: a first set of carbon nanotubes, the first set including multi-walled carbon nanotubes; a second set of carbon nanotubes, the second set including single-walled carbon nanotubes; and the active layer also includes graphite. The active layer indicates that when wetted with an electrolyte, the multi-walled nanotubes swell less than the single-walled carbon nanotubes.
[0083] The polymer additive in the anode active layer is polyamide, preferably water-soluble polyamide, alcohol-soluble polyamide or polyamide soluble in water and alcohol. Polyamide is described in detail below and will not be repeated here.
[0084] The average thickness of the anode active layer is 20 to 100 microns, preferably 30 to 50 microns. The anode active layer comprises anode active particles containing silicon such as, for example, silicate in an amount of 96 to 99 wt %, preferably 96 to 98.5 wt % of the anode active layer.
[0085] The anode active layer further includes a surface treatment agent on the surface of the high aspect ratio carbon element, which promotes adhesion between the high aspect ratio carbon element and the active material particles. The surface treatment agent may include a surfactant. The surfactant may be present in the active layer in an amount of at least 0.5wt% based on the weight of the active layer. The surfactant forms a surfactant layer that is bonded to the high aspect ratio carbon element and includes a plurality of surfactant elements, each surfactant element having a hydrophobic end and a hydrophilic end, wherein the hydrophobic end is arranged to be adjacent to the surface of one of the carbon elements, and the hydrophilic end is arranged to be away from the surface of one of the carbon elements. The surface treatment agent may include a polymer additive (i.e., it may be a polyamide).
[0086] The multi-walled carbon nanotubes may be generally aligned in a direction perpendicular to the surface of the active layer or alternatively perpendicular to a metal foil used as an electrode. The metal foil may include copper or aluminum.
[0087] In one embodiment, an energy storage device (i.e., a supercapacitor or a battery) includes: a cathode; an electrolyte; and an anode, the anode including an active layer, the active layer including a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles, the plurality of electrode active material particles being disposed in the void spaces within the network, wherein the active material particles comprise silicon; and a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative, wherein the active layer includes sufficient silicon such that at least a portion of the silicon is unused during charge and discharge cycles.
[0088] Anode preparation
[0089] The anode can be produced by first preparing a mixture of conductive elements, active materials and binders (sometimes referred to as slurry) in a solvent or solvent mixture. The method for making the anode can also be used to make the cathode. For the sake of brevity, the method will not be repeated during the manufacture of the cathode. The advantage of the binder as described herein is that water, alcohol or a combination thereof can be used as a solvent to form a useful slurry. The slurry can then be applied directly to the current collector or applied to the current collector using an intermediate adhesive layer.
[0090] The slurry can be prepared in a single step. Figure 2A and Figure 2B Depicts methods for making an anode or cathode. These figures describe methods for making the active layers of the anode and cathode and applying the active layers to the current collector. Alternatively, the active layers may be made according to Figure 2A The multi-step method for preparing the slurry is shown in the flow chart of Figure 1 An example of a method 200 is provided for an electrode 100 of a substrate. At 202, a conductive material (e.g., a high aspect ratio carbon element) and a surface treatment agent material (e.g., a surfactant, a binder material as described herein, or both) are combined with a solvent (e.g., water, an alcohol, or a combination thereof) to form an initial slurry. At 204, any additional binder may be added to the initial slurry to form a second slurry. At 206, the slurry is applied to a metal foil (current collector). The solvent present in the slurry is removed via vacuum or heating to form an active layer on the current collector.
[0091] Figure 2BAnother method 300 of manufacturing an anode (or cathode) of an energy storage device is depicted. At 302, a conductive material (e.g., a high aspect ratio carbon element) and a surface treatment material (e.g., a surfactant, a binder material as described herein, or both) are combined with a solvent (e.g., water, alcohol, or a combination thereof) to form an initial slurry. The materials may be mixed in a blade mixer 303.
[0092] At 304, the initial slurry is processed to ensure good dispersion of the solid materials in the slurry. The Li-SiO-C active material (or NMC material) may be added to the slurry. Graphite powder and optional dispersants may be added in step 306. Blade mixing may be performed in mixing step 305 and mixing step 307. The polymer solution may be added in step 308, and additional deionized water may be added in step 310. Blade and dispersive mixing may be used in steps 307 and 309. The slurry prepared in step 312 may then be added to the current collector.
[0093] The treatment may include introducing mechanical energy into the mixture of solvent and solid material (e.g., using an ultrasonic generator, which may also sometimes be referred to as a "sonicator") or other suitable mixing device (e.g., a high shear mixer). For example, the mechanical energy introduced into the mixture may be at least 0.4 kilowatt-hours / kilogram (kWh / kg), 0.5 kWh / kg, 0.6 kWh / kg, 0.7 kWh / kg, 0.8 kWh / kg, 0.9 kWh / kg, 1.0 kWh / kg or more. For example, the mechanical energy introduced into the mixture per kilogram of the mixture may be in the range of 0.4 kWh / kg to 1.0 kWh / kg or any sub-range thereof, such as 0.4 kWh / kg to 0.6 kWh / kg.
[0094] As an example, an ultrasonic bath mixer may be used in step 302, step 304, or step 306. As another example, a probe ultrasonic generator may be used. When compared to an ultrasonic bath for nanoparticle applications, probe ultrasonic treatment may be significantly stronger and more effective. The high shear forces generated by ultrasonic cavitation can destroy particle agglomerates and produce smaller and more uniform particle sizes. In addition to these, ultrasonic treatment can result in a stable and uniform suspension of the formation / solid in the slurry. Typically, this results in dispersion and disaggregation of solids and other decompositions. Examples of probe ultrasonic processing devices include the Q series probe ultrasonic generators available from QSonica LLC of Newtown, Connecticut. Another example includes the Branson Digital SFX-450 ultrasonic generator commercially available from Thomas Scientific of Swedesboro, New Jersey.
[0095] The local nature of each probe within the probe assembly may sometimes result in uneven mixing and suspension. This may be the case for large samples, for example. This can be addressed by using a setup with a continuous flow cell and proper mixing. For example, with such a setup, mixing of the slurry will achieve a fairly uniform dispersion.
[0096] The initial slurry once processed may have a viscosity in the range of 5,000 cps to 25,000 cps or any sub-range thereof (eg, 6,000 cps to 19,000 cps).
[0097] In an optional step, (e.g., used without adding a binder in step 302) a binder or additional binder may be applied, as the surface treatment may be formed completely or partially on the conductive material (e.g., high aspect ratio carbon element) in the initial slurry. In some embodiments, the surface treatment may self-assemble at this stage.
[0098] The resulting surface treatment agent may include functional groups or other features that may promote adhesion between the high aspect ratio carbon elements and the active material particles, as described in other steps below. For example, functional groups on a binder may provide the surface treatment described.
[0099] At 304 and 306 , the active material particles may be combined with the initial slurry to form a final slurry containing the active material particles and the high aspect ratio carbon elements having the surface treatment agent formed thereon.
[0100] The active material may be added directly to the initial slurry. Alternatively, the active material may first be dispersed in a solvent (e.g., water, alcohol, or a combination thereof, dispersed using the techniques described above for the initial solvent) to form an active material slurry. The active material slurry may then be combined with the initial slurry to form a final slurry.
[0101] Suitable solvents are water, alcohol or a combination thereof. Examples of alcohols are ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol or a combination thereof. In addition to water and alcohol, other solvents may also be added to promote the dissolution and / or dispersion of the polymer. Other solvents include polar solvents, non-polar solvents, etc. Adding other solvents should preferably not change the solubility of the polymer in water or alcohol. Liquid non-protonic polar solvents, such as propylene carbonate, ethylene carbonate, butyrolactone, acetonitrile, benzonitrile, nitromethane, nitrobenzene, cyclopentane, dimethylformamide, N-methylpyrrolidone, etc. or a combination thereof, may be added to water or alcohol to dissolve the polymer. Polar protic solvents may be used, such as acetonitrile, nitromethane, acetone, dimethyl sulfoxide, dimethylformamide, etc. or a combination thereof. Other non-polar solvents may also be used, such as benzene, toluene, methylene dichloride, carbon tetrachloride, hexane, diethyl ether, tetrahydrofuran, etc. or a combination thereof. It is also possible to use a co-solvent comprising at least one aprotic polar solvent and at least one non-polar solvent to alter the solubility capacity of the solvent.
[0102] When water and alcohol are used as solvents for the anode active layer (used in the anode), the ratio of water to alcohol is 80:20 to 95:5, preferably 88:12 to 92:8. In an exemplary embodiment, the ratio of water to alcohol is 90:10.
[0103] The solvent may be added to the mixture of the binder, the conductive material and the active material in an amount of 10 to 1000 wt %, preferably 50 to 500 wt %, and more preferably 100 to 200 wt % of the total weight of the solids used to form the active layer. The solids include materials (e.g., binder, conductive material and active material) that do not evaporate and eventually enter the active material layer disposed on the current conductor.
[0104] At 312, the final slurry is processed to ensure good dispersion of the solid material in the final slurry. Any suitable mixing method known in the art can be used. For example, the process can use the techniques described above with respect to 303, 305, 307, 309 and 311, etc. Alternatively, a planetary mixer can be used, such as a multi-axis (e.g., three-axis or more) planetary mixer. The planetary mixer can have multiple blades, such as two or more mixing blades and one or more (e.g., two, three or more) dispersion blades, such as disc dispersion blades.
[0105] During 312 , the matrix engaging the active material may fully or partially self-assemble as the interaction between the surface treatment (eg, binder) and the active material promotes the self-assembly process.
[0106] In some embodiments, the final slurry once processed will have a viscosity in the range of 1,000 cps to 10,000 cps or any sub-range thereof (eg, 2,500 cps to 6000 cps).
[0107] At 312, an active layer 106 is formed from the final slurry. In some embodiments, the final slurry may be wet cast directly onto the current collector conductive layer 102 (or optional adhesion layer 104) and dried. As an example, the active layer 106 may be formed by applying at least one of heat and vacuum until substantially all solvents and any other liquids have been removed. It may be desirable to protect portions of the underlying layers. For example, where the electrode 100 is intended for single-sided operation, it may be desirable to protect the underside of the conductive layer 102. Protection may include preventing the effects of solvents, such as by shielding certain areas or providing drains to divert the solvent away.
[0108] In another example, the final slurry can be at least partially dried elsewhere before being transferred to the adhesion layer 104 or the conductive layer 102 using any suitable technique (e.g., roll-to-roll application) to form the active layer 106. As another example, the wet combined slurry can be placed on an intermediate material with a suitable surface and dried to form a layer (e.g., active layer 106). Although any material with a suitable surface can be used as an intermediate material, an exemplary intermediate material includes polytetrafluoroethylene (PTFE) because its properties facilitate subsequent removal from the surface. The layer can be formed in a press to provide a layer exhibiting a desired thickness, area, and density.
[0109] In yet another example, the final slurry can be formed into a sheet and applied to the adhesion layer 104 or the conductive layer 102 as appropriate. For example, the final slurry can be applied through a slot die to control the thickness of the applied layer. As another example, the slurry can be applied and then leveled to the desired thickness, for example, using a scraper. A variety of other techniques can be used to apply the slurry. For example, the coating technique may include, but is not limited to: comma coating; comma reverse coating; scraper coating; slot die coating; direct gravure coating; air scraper coating (air knife); chamber scraper coating; offset gravure coating; one roll kiss coating; reverse kiss coating using a small diameter gravure roller; rod coating; three reverse roll coating (top feed); three reverse roll coating (fountain die); reverse roll coating, etc.
[0110] The viscosity of the final slurry can vary depending on the application technique. For example, for comma coating, the viscosity can be in the range of about 1,000 cps to about 200,000 cps. Lip die coating provides coating with a slurry exhibiting a viscosity between about 500 cps and about 300,000 cps. Reverse kiss coating provides coating with a slurry exhibiting a viscosity between about 5 cps and 1,000 cps. In some applications, the corresponding layer can be formed by multiple passes.
[0111] When desired, the active layer 106 formed from the final slurry can be compressed (e.g., using a calendering device) before or after being applied to the electrode 100. The slurry can be partially or completely dried before or during the compression process (e.g., by applying heat, vacuum, or a combination thereof). For example, in some embodiments, the active layer can be compressed to a final thickness (e.g., in a direction perpendicular to the current collector layer 102) that is less than 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of its pre-compression thickness.
[0112] When a partially dried layer is formed during the coating or compression process, the layer can be subsequently fully dried (eg, by applying heat, vacuum, or a combination thereof). In some embodiments, substantially all of the solvent is removed from the active layer 106 .
[0113] The solvent used to form the slurry may be recovered and recycled into the slurry preparation process.
[0114] The active layer 106 may be compressed, for example to break some of the constituent high aspect ratio carbon elements or other carbonaceous materials, thereby increasing the surface area of the corresponding layer. Such compression treatment may increase one or more of the adhesion between layers, the ion transport rate within the layer, and the surface area of the layer. In various embodiments, compression may be applied before or after the corresponding layer is applied to or formed on the electrode 100.
[0115] In the case of using calendaring to compress the active layer 106, the calendaring equipment can be set to a gap spacing equal to or less than 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of the pre-compression thickness of the layer (for example, set to about 33% of the pre-compression thickness of the layer). The calendaring rollers can be configured to provide a suitable pressure, for example, greater than 1 ton per centimeter of roller length, greater than 1.5 tons per centimeter of roller length, greater than 2.0 tons per centimeter of roller length, greater than 2.5 tons per centimeter of roller length or more. The density of the active layer after compression can be in the range of 1g / cc to 10g / cc or any sub-range thereof (such as 2.0g / cc to 4.0g / cc). It should be noted that the density of the cathode active layer is 2 to 4g / cc. The density of the anode active layer is typically 1.0 to 1.8g / cc. The calendaring process can be carried out at a temperature in the range of 20°C to 140°C or any sub-range thereof. In some embodiments, the active layer 106 may be preheated prior to calendaring, for example at a temperature in the range of 20° C. to 100° C. or any sub-range thereof.
[0116] Figure 2B The method 300 may include any of the following features (alone or in any suitable combination):
[0117] The initial slurry has a solids content in the range of 0.1% to 20.0% by weight (or any sub-range thereof), and / or the final slurry has a solids content in the range of 10.0% to 80% by weight (or any sub-range thereof).
[0118] As noted, the scaffold or matrix of conductive material and binder can hold the active material particles together to form a cohesive layer that is also firmly attached to the metal current collector. Such active material structures can be produced during slurry preparation and subsequently in a roll-to-roll ("R2R") coating and drying process. One of the main advantages of this technology is its scalability and "drop-in" nature, as various embodiments are compatible with conventional electrode manufacturing processes.
[0119] The matrix can be formed during slurry preparation using the techniques described herein: using, for example, the above reference Figure 2A and Figure 2B The methods described in methods 200 and 300 are to appropriately disperse the high aspect ratio carbon material and chemically functionalize it as needed. Chemical functionalization is intended to form an organized self-assembled structure with the surface of the active material particles, such as NMC particles for the cathode (as described in detail below) or silicon particles ("Si") or silicon dioxide ("SiOx") particles in the case of the anode. The slurry so formed can be based on water and / or alcohol solvents for the cathode and water for the anode, and such solvents are very easy to evaporate and dispose of during the manufacturing process. Electrostatic interactions promote self-organized structures in the slurry, and after the drying process, the bonding between the carbon matrix with active material particles so formed and the collector surface is promoted by the surface treatment agent (e.g., functional groups on the matrix) and the strong entanglement of the active material in the carbon matrix.
[0120] By tuning the surface functionalization and entanglement effects, the mechanical properties of the electrode can be modified according to the application and mass loading requirements.
[0121] After coating and drying, the electrode can be subjected to a calendering step to control the density and porosity of the active material. In NMC cathode electrodes, densities of >=3.5 g / cc or higher and 20% porosity or higher can be achieved. Porosity can be optimized depending on mass loading and lithium-ion battery cell requirements. For silicon oxide or silicon-based anodes, porosity can be specifically controlled to accommodate the expansion of the active material during the lithiation process.
[0122] The teachings herein can provide up to 20% reduction in $ / kWh. By using water, alcohol, or mixed water / alcohol as solvents, which evaporate easily, electrode production can be higher, and more importantly, long-term dryer energy consumption can be significantly reduced. The conventional recovery system required when using NMP or similar compounds as solvents is also greatly simplified when using water, alcohol, or a combination thereof.
[0123] The teachings herein provide an active layer with a 3D matrix that can significantly increase the electrode conductivity by a factor of 10 to 100 compared to electrodes using conventional binders such as PVDF, which enables fast charging at the battery level. Thick electrode coatings in the cathode up to 150um (or more) on each side of the current collector can be achieved using this technology. The solvent used in the slurry is combined with a strong 3D carbon matrix to obtain a thick wet coating without cracking during the drying step. Thick cathodes and high-capacity anodes enable a significant jump in energy density to 400Wh / kg or more.
[0124] cathode
[0125] The cathode comprises one or more polymer binders (cathode polymer binders), one or more active materials and a conductive material. One or more polymer binders, one or more active materials and a conductive material are blended with a solvent to form a cathode mixture. The cathode mixture is then placed on a current collector (usually a metal) and dried to form a solid cathode active layer.
[0126] The cathode polymer binder (used in the cathode) includes a first cathode polymer binder comprising a polyamide. The polyamide has been described in detail above and will not be described again in detail for the sake of brevity.
[0127] The cathode polymer binder is present in an amount of 0.1 to 0.4 wt %, preferably 0.15 to 0.375 wt %, based on the weight of the cathode mixture (which includes the cathode polymer binder (the first cathode polymer binder and the second cathode polymer binder), the cathode active material, the cathode conductive material and the solvent). Based on the total weight of the cathode active layer, the cathode polymer binder is present in the cathode active layer in an amount of 0.2 to 0.5 wt %, preferably 0.25 to 0.45 wt %.
[0128] Cathode active material
[0129] The cathode active material may include lithium cobalt oxide (LCO, sometimes referred to as "lithium cobaltate" or "lithium cobaltite"). Examples of LCO formulations include LiCoO2; lithium nickel manganese cobalt oxide (NMC, a variant of which is LiNiMnCo); lithium manganese oxide (LMO, a variant of which is LiMn2O4, Li2MnO3, etc. or a combination thereof); lithium titanium oxide (LTO, a variant of which is Li4Ti5O 12 ); lithium iron phosphate oxide (LFP, one of its variants is LiFePO4), lithium nickel cobalt aluminum oxide (and its variant NCA) and other similar other materials. Other variants of the foregoing may be included.
[0130] In one embodiment, the cathode active material may include NMC, NCA, NCMA, or a combination thereof.
[0131] When NMC is used as the cathode active material, a nickel-rich NMC may be used. For example, a variant of NMC may be LiNi x Mn y Co (1-x-y) , wherein x is equal to or greater than about 0.7, 0.75, 0.80, 0.85 or more, y is equal to or greater than 0.1, 0.15, 0.2 or 0.25, and x+y is less than 1. For example, NMC811 can be used, wherein x is about 0.8 and y is about 0.1. Alternatively, the cathode active material may include an oxide of lithium nickel manganese cobalt (LiNi x Mn y Co z O2). Variants of this formula that can be used in the active material layer include NMC 111 (described in detail below), NMC532 (LiNi 0.5 Mn 0.3 Co 0.2 O2), NMC622(LiNi 0.6 Mn 0.2 Co 0.2 O2) or a combination thereof.
[0132] In one embodiment, NMC91 may be used as the cathode active material. NMC91 includes 91 mol % or more of nickel. An example of NMC91 is LiNi 0.91 Co 0.06 Mn 0.03 O2. Li[Ni 1–x–y Co x Al y ]O2(NCA) can also be used as a cathode active material. An example of NCA is NCA89.
[0133] In yet another embodiment, the cathode active material may be an NCMA material. An example of an NCMA is Li[Ni 0.89 Co 0.05 Mn 0.05 Al 0.01 ]O2, also known as NCMA89.
[0134] In one embodiment, the cathode active material may also include a nickel-rich combination of nickel, manganese and cobalt. Lithium-nickel-manganese-cobalt oxide (LiNiMnCoO2), referred to as NMC, has strong overall performance, excellent specific energy and the lowest self-heating rate of all mainstream cathode powders. Based on the total weight of the NMC blend, the NMC powder may contain 20 to 40wt% nickel, 20 to 40wt% manganese and 20 to 40wt% cobalt. Although the term "NMC powder" can refer to a variety of blends, it is desirable to use a blend containing 33wt% nickel, 33wt% manganese and 33wt% cobalt. This blend, sometimes referred to as 1-1-1 (NMC111), is suitable for applications (automobiles, energy storage) that use frequent cycles, due to the low cobalt content of the nickel-rich combination of nickel, manganese and cobalt (NMC), which leads to reduced material costs. The NMC powder may contain 20 to 40 wt% nickel, 20 to 40 wt% manganese, and 20 to 40 wt% cobalt, based on the total weight of the NMC blend. Although the term "NMC powder" can refer to a variety of blends, it is desirable to use a blend containing 33 wt% nickel, 33 wt% manganese, and 33 wt% cobalt. This blend, sometimes referred to as 1-1-1, is suitable for applications (automobiles, energy storage) that use frequent cycles due to the lower cobalt content, which results in reduced material costs. Lithium-nickel-manganese-cobalt oxide (LiNiMnCoO2) has strong overall performance, excellent specific energy, and the lowest self-heating rate of all mainstream cathode powders. Lithium-rich NCM materials manufactured by BASF (such as 424 and 523) can also be used as cathode active materials.
[0135] Generally speaking, adding increased active material loading to the cathode (measured as a function of the total weight of the cathode) results in increased levels of areal capacity and specific energy in the cathode.
[0136] As noted above, the cathode active material may be included or contained in a network of high aspect ratio conductive materials present in the cathode active layer. The cathode active material may be present in the mixture for forming the cathode in an amount of 90 to 99 wt%, preferably 96 to 98.5 wt%, based on the total weight of the cathode mixture (a mixture for making the cathode active layer, which contains a cathode binder material, a cathode active material, a cathode conductive material, and a solvent). The cathode active material is present in the cathode active layer (which does not contain a solvent) in an amount of 95 to 98.5 wt%, based on the total weight of the cathode active layer.
[0137] Fabrication of cathode active layer
[0138] The cathode active layer is disposed on the current collector. The cathode active layer is manufactured in a similar manner to the anode active layer. The cathode binder, cathode active material and cathode conductive material are mixed with a solvent to form a slurry. The slurry is disposed on the cathode current collector. The solvent is evaporated and the cathode current collector may be subjected to further finishing operations in a roller mill to produce a cathode, which may then be used in an energy storage device as described in detail below.
[0139] Cathode Overview
[0140] In one embodiment, the cathode includes an active layer, which includes a network of high aspect ratio carbon elements, which defines void spaces within the network; a plurality of electrode active material particles, which are arranged in the void spaces within the network; and a polymer additive, which is (i) selected from the polyamide family or (ii) at least one of a modified polyamide or a polyamide derivative.
[0141] The cathode includes a network of high aspect ratio carbon elements, which includes: a first set of carbon nanotubes, wherein the first set of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; and a second set of carbon nanotubes, wherein the second set of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and the second set of carbon nanotubes has one or more properties different from the first set of carbon nanotubes.
[0142] The first set of carbon nanotubes includes multi-walled nanotubes. The second set of carbon nanotubes includes single-walled nanotubes. In one embodiment, the first set of carbon nanotubes includes multi-walled carbon nanotubes; the second set of carbon nanotubes includes single-walled carbon nanotubes; and the ratio of the amount by weight of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:1.
[0143] In one embodiment, the network of high aspect ratio carbon elements includes a collection of multi-walled carbon nanotubes. Some of the multi-walled carbon nanotubes are branched, interdigitated, entangled, and / or share a common wall. The active layer includes 0.2 to 2 wt% of the multi-walled carbon nanotubes, or 0.25 to 1.5 wt% of the multi-walled carbon nanotubes.
[0144] In one embodiment, an energy storage device includes an electrolyte; an anode and a cathode, wherein multi-walled nanotubes (a first population of carbon nanotubes) of the cathode active layer swell more than single-walled carbon nanotubes (a second population of carbon nanotubes) when wetted with the electrolyte.
[0145] In one embodiment, the multi-walled carbon nanotubes of the cathode active layer comprise an average diameter between 6 nm and 10 nm, or between 6 nm and 15 nm; an average wall thickness between 6 nm and 7 nm; and an average length of about 16 microns. In one embodiment, the cathode active layer may comprise single-walled carbon nanotubes having an average diameter between 1 nm and 5 nm and an average length greater than or equal to about 5 microns up to about 200 microns. In one embodiment, the cathode active layer may comprise single-walled carbon nanotubes having an average diameter between 2 nm and 4 nm and an average length greater than or equal to about 6 microns up to about 8 microns. The single-walled carbon nanotubes comprise an average of 1 or 2 walls.
[0146] In one embodiment, the average thickness of the carbon nanotubes used in the cathode active layer undergoes an increase (increase in diameter) of less than 10% when wetted with an electrolyte. In one embodiment, the first average aspect ratio of the first set of carbon nanotubes is greater than the second average aspect ratio of the second set of carbon nanotubes. In another embodiment, the network of high aspect ratio carbon elements includes a plurality of multi-walled carbon nanotubes; and the length distribution of the plurality of multi-walled carbon nanotubes is biased toward a nominal length of the multi-walled carbon nanotubes, wherein the nominal length of the multi-walled carbon nanotubes is at least 15 microns.
[0147] In one embodiment, the network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes; and at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 8 microns, preferably greater than 12 microns.
[0148] In one embodiment, the first collection of carbon nanotubes has an average aspect ratio of at least 100, preferably between 200 and 1000. In one embodiment, the network of high aspect ratio carbon elements comprises a collection of multi-walled carbon nanotubes, the collection comprising a plurality of multi-walled carbon nanotubes; and the plurality of multi-walled carbon nanotubes have at least 5 walls, preferably at least 6 walls, and more preferably at least 7 walls.
[0149] In another embodiment, the high aspect ratio carbon element used in the cathode active layer includes at least one material selected from the group consisting of: carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes.
[0150] In one embodiment, the cathode active layer comprises a polymer binder comprising nylon (i.e., polyamide). In an exemplary embodiment, the polyamide is a water-soluble polyamide, an alcohol-soluble polyamide, or a combination thereof (i.e., soluble in a combination of water and alcohol). The cathode active layer does not include a polymer material that is insoluble in water or alcohol. In other words, the cathode active layer does not contain polyamide or any other non-water-soluble polymer binder.
[0151] The molecular weight of the polyamide is greater than 200 g / mol, preferably greater than 500,000 g / mol, preferably greater than 1,000,000 g / mol, and more preferably from 500,000 g / mol to 1,500,000 g / mol.
[0152] In one embodiment, the cathode active layer comprises at least 0.5 wt %, preferably 0.5 to 1.5 wt % of the polymer additive. The wt % is based on the total weight of the active layer.
[0153] In one embodiment, the average thickness of the cathode active layer is 20 to 100 micrometers, preferably 30 to 80 micrometers.
[0154] In one embodiment, the active material particles present in the active layer include at least one of the following: lithium iron phosphate, lithium metal oxide, lithium-sulfur, lithium-cobalt oxide, lithium-nickel-manganese-cobalt oxide, lithium-nickel-cobalt-aluminum oxide, lithium-nickel-cobalt-manganese-aluminum oxide, or a combination thereof.
[0155] In one embodiment, the cathode active material comprises particles of at least one electrode active material selected from the group consisting of LiCoO2, LiNiO2, LiMn2O4, LiCoPO4, LiFePO4, LiNiMhCoO2, and LiNi 1-x-y-z Co x M1 y M2 z O z (wherein M1 and M2 are each independently selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg and Mo, and x, y and z represent the atomic fractions of the corresponding constituent elements of the oxide and satisfy the relationship of 0≦x<0.5, 0≦y<0.5, 0≦z<0.5). The active layer contains at least 96 wt%, preferably 96.0 wt% to 98.5 wt% of active material particles.
[0156] In one embodiment, the cathode active layer comprises about 25% by weight of the dispersant.
[0157] In one embodiment, the cathode active layer includes a surface treatment agent on the surface of the high aspect ratio carbon element, which promotes adhesion between the high aspect ratio carbon element and the active material particles. In one embodiment, the surface treatment agent includes a material soluble in a solvent having a boiling point below 202°C, preferably below 185°C. In one embodiment, the surface treatment agent includes a surfactant layer; wherein the surfactant layer is bonded to the high aspect ratio carbon element and includes a plurality of surfactant elements, each surfactant element having a hydrophobic end and a hydrophilic end, wherein the hydrophobic end is disposed adjacent to a surface comprising one of the carbon elements, and the hydrophilic end is disposed away from the surface comprising one of the carbon elements.
[0158] In one embodiment, the surface treatment agent comprises a polymer additive (polyamide). In another embodiment, the polymer additive is a polymer binder. The polymer additive is at least partially disposed in at least one void space defined by the network of high aspect ratio carbon elements. The specific gravity of the polymer additive is greater than 1.135 g / cm 3 , preferably greater than 1.20 g / cm 3 The specific heat of the polymer additive is greater than 2.0 J / g°C at 23°C, preferably greater than 2.2 J / g°C at 23°C, and more preferably greater than 2.4 J / g°C at 23°C. The tensile strength of the polymer additive, as measured when the polymer additive is dry, is less than 70 MPa, preferably less than 50 MPa, preferably less than 25 MPa, preferably less than 10 MPa, preferably less than 7.5 MPa. The tensile strength of the polymer additive, as measured when the polymer additive is dry, is between 5 and 6 MPa.
[0159] The polymer additive has an elongation at yield greater than 5%, preferably greater than 10%, preferably greater than 20%, and more preferably greater than 30%, as measured when the polymer additive is dry.Tensile strength and elongation at yield are measured according to ASTM D638.
[0160] When measured using differential scanning calorimetry (DSC) at a temperature ramp rate of 10°C / minute, the polymer additive has a glass transition temperature of less than 0°C, preferably less than -10°C, preferably less than -25°C, preferably less than -30°C, preferably less than -45°C. The temperature of 5% weight reduction of the polymer additive is between 375°C and 400°C.
[0161] When the mixture of the polymer additive and ethyl cellosolve is cooled, the polymer additive exhibits gelation. The polymer additive is completely soluble in each of water, ethylene glycol, benzyl alcohol, acetic acid, N-methylpyrrolidone and isobutyl alcohol.
[0162] In one embodiment, an aqueous solution of the polymer additive and at least one of water and alcohol exhibits a viscosity of at least 60 Pa·s when the concentration of the polymer additive is about 50% by weight. In one embodiment, the mixture of the polymer additive and the water-soluble polymer forms a transparent mixture.
[0163] The active layer does not include polymeric materials that are insoluble in water or alcohol.
[0164] In one embodiment, an energy storage device (which may be a supercapacitor or a battery) includes: an anode; an electrolyte; and a cathode, the cathode including a cathode active layer, the cathode active layer including a network of high aspect ratio carbon elements, the network defining void spaces within the network; a plurality of electrode active material particles, the plurality of electrode active material particles being disposed in the void spaces within the network; and a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) modified polyamide or polyamide derivatives.
[0165] In another embodiment, the electrode includes an active layer, which includes a network of high-aspect ratio carbon elements, which defines void spaces within the network, wherein the network of high-aspect ratio carbon elements includes at least one material selected from the group consisting of: multi-walled carbon nanostructures, multi-walled carbon nanotubes, fragments of multi-walled carbon nanostructures, and broken multi-walled carbon nanotubes; a plurality of electrode active material particles, which are arranged in the void spaces within the network; and a polymer additive, which is a polyamide soluble in water or alcohol.
[0166] In another embodiment, an electrode includes an active layer, which includes a network of high-aspect ratio carbon elements, which defines void spaces within the network; a plurality of electrode active material particles, which are arranged in the void spaces within the network; and a polymer additive, which is a polyamide soluble in water or alcohol, wherein the network of high-aspect ratio carbon elements forms one or more highly conductive paths; the network of high-aspect ratio carbon elements includes multi-walled carbon nanotubes; the network of high-aspect ratio carbon elements provides mechanical support for at least a portion of the plurality of electrode active material particles; and the polymer additive provides support for at least a portion of the plurality of electrode active material particles.
[0167] Energy storage device
[0168] After assembling the electrode 100, an energy storage device may be assembled using the electrode 100. Assembly of the energy storage device may follow conventional steps for assembling electrodes with separators and placing them in a housing such as a can or bag, and may also include additional steps of electrolyte addition and sealing the housing.
[0169] One exemplary embodiment includes a lithium-ion battery energy storage device in the form of a pouch cell that combines a Ni-rich NMC active material in the cathode and a SiOx and graphite blend active material in the anode, wherein both the anode and cathode are made using a 3D carbon matrix process as described herein.
[0170] Figure 3A schematic diagram of an electrode arrangement of an example of a soft pack battery device is shown in . As shown, a cathode active layer 760 (e.g., an active layer according to various embodiments disclosed herein) is located on opposite sides of a current collector 710 (e.g., an aluminum foil current collector) to form a double-sided cathode disposed between two single-sided anodes. The single-sided anodes each have an anode layer 740 or 750 (e.g., an active layer including a carbon element network such as disclosed herein) disposed on a current collector 720 or 730 (e.g., a copper current collector). The electrodes are separated by a permeable separator material 780 wetted with an electrolyte (not shown). This arrangement can be accommodated in a soft pack battery of a type known in the art.
[0171] exist Figure 4 , a cross section of an energy storage device (ESD) 810 is shown. The energy storage device (ESD) 810 includes a housing 811. The housing 811 has two terminals 800 disposed on the exterior thereof. The terminals 800 provide internal electrical connections to a battery 812 contained within the housing 811 and external electrical connections to an external device such as a load or a charging device (not shown). The energy storage device disclosed herein may be a battery, a capacitor, a supercapacitor, etc.
[0172] The present disclosure may alternatively comprise, consist of, or consist essentially of any suitable components disclosed herein. Additionally or alternatively, the present disclosure may be formulated to be free of or substantially free of any component, material, ingredient, adjuvant, or species used in prior art compositions, or any component, material, ingredient, adjuvant, or species that is otherwise not necessary to achieve the functions and / or objectives of the present disclosure.
[0173] All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, if a term in the present application contradicts or conflicts with a term in the incorporated reference, the term from the present application takes precedence over the conflicting term from the incorporated reference.
[0174] Unless otherwise specified herein, all test standards are the most current standards in effect as of the filing date of this application or, if priority is claimed, the filing date of the earliest priority application in which such test standards appear.
[0175] Although the present invention has been described with reference to some embodiments, it will be appreciated by those skilled in the art that various changes may be made and elements of the present invention may be substituted with equivalents without departing from the scope of the present invention. In addition, many modifications may be made to adapt specific circumstances or materials to the teachings of the present invention without departing from the basic scope of the present invention. Therefore, it is intended that the present invention is not limited to the specific embodiments disclosed as the best mode contemplated for carrying out the present invention, but that the present invention will encompass all embodiments within the scope of the appended claims.
Claims
1. An anode, comprising: An active layer, the active layer comprising: a network of high aspect ratio carbon elements, said network defining void spaces within said network; a plurality of electrode active material particles disposed in the void spaces within the network, wherein the active material particles comprise silicon; and The polymer additive is (i) at least one selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative. 2 . The electrode according to claim 1 , wherein the silicon contained in the electrode active material particles is in the form of SiO. The electrode according to claim 1 , wherein the silicon contained in the electrode active material is micro silicon. 4 . The electrode according to claim 1 , wherein the silicon contained in the electrode active material is greater than fifty percent by weight of the active layer.
5. The electrode according to claim 1, wherein the silicon contained in the electrode active material is at least eighty percent by weight of the active layer.
6. The electrode according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a mesh of carbon nanotubes; and The network of carbon nanotubes maintains electrical connections between at least a subset of the carbon nanotubes contained in the network during expansion of the silicon.
7. The electrode according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a mesh of carbon nanotubes; and The network of carbon nanotubes maintains electrical connections between at least a subset of the carbon nanotubes contained in the network during charging and discharging of a battery in which the electrode is contained.
8. The electrode of claim 1, wherein the network of high aspect ratio carbon elements comprises: a first set of carbon nanotubes, wherein the first set of carbon nanotubes comprises a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; as well as A second set of carbon nanotubes, wherein: The second set of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second collection of carbon nanotubes has one or more properties that are different from the first collection of carbon nanotubes.
9. The electrode of claim 8, wherein the first collection of carbon nanotubes comprises multi-walled nanotubes.
10. The electrode of claim 8, wherein the second collection of carbon nanotubes comprises single-walled nanotubes.
11. A cathode comprising: An active layer, the active layer comprising: a network of high aspect ratio carbon elements, said network defining void spaces within said network; a plurality of electrode active material particles disposed in the void spaces within the network; and The polymer additive is (i) at least one selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative.
12. The electrode of claim 11, wherein the network of high aspect ratio carbon elements comprises: a first set of carbon nanotubes, wherein the first set of carbon nanotubes comprises a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; as well as A second set of carbon nanotubes, wherein: The second set of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second collection of carbon nanotubes has one or more properties that are different from the first collection of carbon nanotubes.
13. The electrode of claim 12, wherein the first collection of carbon nanotubes comprises multi-walled nanotubes.
14. The electrode of claim 12, wherein the second collection of carbon nanotubes comprises single-walled nanotubes.
15. The electrode according to claim 12, wherein: The first set of carbon nanotubes includes multi-walled carbon nanotubes; The second set of carbon nanotubes includes single-walled carbon nanotubes; and The ratio of the amount by weight of the first set of carbon nanotubes to the second set of carbon nanotubes is about 2:
1.
16. The electrode of claim 11, wherein the network of high aspect ratio carbon elements comprises a collection of multi-walled carbon nanotubes.
17. The electrode according to claim 16, wherein the active layer comprises 0.2 to 2% by weight of multi-walled carbon nanotubes, or 0.25 to 1.5% by weight of multi-walled carbon nanotubes. The electrode according to claim 16 , wherein the multi-walled carbon nanotubes are branched carbon nanotubes.
19. The electrode of claim 16, wherein the active layer comprises 0.25% to 1.5% by weight of multi-walled carbon nanotubes.
20. The electrode of claim 16, wherein the multi-walled carbon nanotubes are branched, interdigitated, entangled, and / or share a common wall.
21. An energy storage device, comprising: Electrolytes; and the electrode of claim 12, wherein the multi-walled carbon nanotubes contained in the first set of carbon nanotubes swell more than the single-walled carbon nanotubes contained in the second set of carbon nanotubes when wetted with the electrolyte.