Method for manufacturing LED mounting substrate with cured film

Through the coating and development technology of the photosensitive resin composition, a cured film is formed, which solves the problem of low production efficiency of LED mounting substrates, improves conductivity and optical performance, and enhances connection reliability.

CN118891741APending Publication Date: 2024-11-01TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380026931.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-20
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The production efficiency of existing LED mounting substrates is low, especially in terms of the bonding of conductive bumps and LED electrodes and the expansion barrier of liquid resin materials.

Method used

Using the LED mounting substrate manufacturing method with a cured film, the cured film between the bumps and the LEDs on the wiring electrode is formed by coating, exposure and development technology of the photosensitive resin composition to ensure the appropriate ratio of conductive particles and organic components. , the resin composition is optimized to improve the light shielding and reflectivity of the film using specific photopolymerization initiators and coloring pigments.

Benefits of technology

The production efficiency of the LED mounting substrate is improved, conductivity and optical performance are ensured, and the connection reliability of the bumps and LED electrodes are enhanced and the durability of the cured film is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891741A_ABST
    Figure CN118891741A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide: an LED mounting substrate which is coated with a patterned developed coating film (partition wall) that partitions an LED, and a peripheral portion of a bump and an electrode, and which is left on the LED mounting substrate; the purpose of the present invention is to provide a method for manufacturing an LED mounting substrate with a cured film, which has excellent production efficiency by selectively removing unwanted portions using a photosensitive method. The present invention can be realized by a method for manufacturing an LED mounting substrate with a cured film, the method being characterized in that: the method for manufacturing an LED mounting substrate with a cured film is a method for manufacturing an LED mounting substrate including a substrate having a wiring electrode, a bump formed on the wiring electrode, and a plurality of LED elements mounted on the bump mounted thereon; in a method for manufacturing an LED mounting substrate with a cured film in which specific processing steps are sequentially performed, in a step for removing an undesired portion of an exposed dry film by developing, the developed film remains at least around a bump and a wiring electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an LED mounting substrate with a cured film. Background Art

[0002] In recent years, with the development of information terminal devices such as smartphones and tablets, and the high-definition of flat-panel displays represented by televisions, the demand for higher performance of displays has further increased. Among them, micro-LED displays using tiny-sized LEDs have attracted attention as high-performance displays. This display is a display that uses micro-LEDs driven by an active matrix method as a light source to perform full-color display, and has excellent contrast and color reproducibility.

[0003] In the micro-LED display, it is necessary to configure a patterned cured film (partition wall) that separates the light source in a size corresponding to the micro-LED as the light source. As a method of forming a patterned cured film, photolithography using a pattern mask is well known (Patent Document 1). In addition, for these partition walls, in addition to the light shielding property to prevent the mixing of colors between adjacent micro-LEDs, it is also required to efficiently extract the reflection characteristics of the light from the micro-LED.

[0004] In addition, since the production of micro-LED displays requires a very large number of micro-LEDs, ranging from hundreds of thousands to tens of millions, an efficient installation method for the substrate is required. For example, it is known that after a conductive photoresist with conductive particles added is applied to the surface of a printed wiring board, exposure and development are performed to form a conductive bump on the electrode of the printed wiring board, and then the conductive bump is bonded to the LED electrode via a conductive adhesive (Patent Document 2). In addition, in order to install LEDs with finer pitches, the importance of a cured film (Patent Document 3) for the purpose of protecting the electrode and improving the light extraction efficiency has also increased.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-188037

[0008] Patent Document 2: Japanese Patent Application Publication No. 2018-82197

[0009] Patent Document 3: Japanese Patent Application Publication No. 2017-112295 Summary of the invention

[0010] Problems to be solved by the invention

[0011] As a method for mounting LEDs on a substrate, the technology described in Patent Document 2 requires an additional adhesive in order to bond the conductive bumps to the LED electrodes, thereby increasing the number of steps and causing poor production efficiency. In addition, the bottom fill forming technology described in Patent Document 3 has a problem that when a sealing film is formed using a liquid resin material on the electrode portion of the LED mounted on the substrate, a frame for blocking the expansion of the liquid resin material needs to be formed, causing poor production efficiency.

[0012] Therefore, the present invention provides a method for manufacturing an LED mounting substrate with a cured film with excellent production efficiency, which can cover the LED mounting substrate with a patterned developed coating (partitioning wall) that separates the LEDs, as well as the surrounding areas of the bumps and electrodes, and selectively remove unnecessary parts using a photosensitive method.

[0013] Means for solving problems

[0014] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by the following method for producing an LED mounting substrate with a cured film.

[0015] [1] A method for manufacturing an LED mounting substrate with a cured film, wherein the following processing steps (1) to (5) are sequentially performed on the LED mounting substrate, which includes a substrate having wiring electrodes, bumps formed on the wiring electrodes, and a plurality of LED elements mounted on the bumps.

[0016] (1) A step of applying a photosensitive resin composition to the LED mounting substrate to fill the gap between the LED element and the substrate having wiring electrodes and the space between adjacent LED elements with the coating film.

[0017] (2) Step of drying the coating film to obtain a dried film

[0018] (3) Step of exposing the dried film to light

[0019] (4) A step of removing unnecessary portions of the exposed dried film by development

[0020] (5) Process of converting the film from which unnecessary portions have been removed after development into a cured film

[0021] [2] The method for manufacturing an LED mounting substrate with a cured film according to [1] is characterized in that, in the processing step (4) described in [1], in which the unnecessary portion of the dried film after exposure is developed and removed, the developed film remains at least around the bumps and wiring electrodes.

[0022] [3] The method for producing a cured film-attached LED mounting substrate according to [1] or [2], wherein the bumps formed on the wiring electrodes contain (A) an organic component and (B) conductive particles.

[0023] [4] According to the method for manufacturing an LED mounting substrate with a cured film as described in any one of [1] to [3], the (A) organic component of the above-mentioned bump contains an acrylic copolymer having a carboxyl group and an epoxy resin, and the proportion of the above-mentioned (B) conductive particles in the total weight of the above-mentioned bump is 50 to 90 wt%.

[0024] [5] The method for producing an LED mounting substrate with a cured film according to any one of [1] to [4], wherein the bumps are obtained by exposing and developing a conductive paste containing (A) an organic component and (B) conductive particles to form a pattern.

[0025] [6] The method for producing an LED mounting substrate with a cured film according to any one of [1] to [5], wherein the photosensitive resin composition contains (C) a resin, (D) a photopolymerization initiator, (E) a photopolymerizable compound, (F) an organic solvent, and (G) a coloring pigment.

[0026] [7] The method for producing an LED mounting substrate with a cured film according to [6], wherein the (G) coloring pigment contains at least (G-1) a white pigment.

[0027] [8] The method for producing an LED mounting substrate with a cured film according to [6] or [7], wherein the resin (C) is a siloxane resin (C-1).

[0028] [9] An LED mounting substrate with a cured film, produced by the method described in any one of [1] to [8].

[0029]

[10] A device comprising the LED mounting substrate with a cured film according to [9].

[0030]

[11] An LED mounting substrate comprising a substrate having an electrode, a bump formed on the electrode and made of a composite material of an organic component and conductive particles, and a plurality of LED elements mounted on the bump, wherein:

[0031] At least a part of the periphery of the bump and the LED element is covered with a cured film of the photosensitive resin composition, and the cured film of the photosensitive resin composition is also present between adjacent LD elements.

[0032] Effects of the Invention

[0033] The present invention provides a method for producing an LED mounting substrate with a cured film with excellent production efficiency, which can cover a patterned developed coating film (partition wall) for separating LEDs and surrounding parts of bumps and wiring electrodes on the LED mounting substrate at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Top view of the LED mounting substrate

[0035] Figure 2 Cross-sectional view of the substrate for LED mounting

[0036] Figure 3 This is a cross-sectional view showing a state where a coating film of a photosensitive resin composition is formed on an LED mounting substrate.

[0037] Figure 4 This is a cross-sectional view showing a state where a dry film of a photosensitive resin composition is formed on an LED mounting substrate.

[0038] Figure 5 This is a cross-sectional view showing a state where a dry film of a photosensitive resin composition on an LED mounting substrate is exposed.

[0039] Figure 6 This is a cross-sectional view of a state where unnecessary portions of the photosensitive resin composition on the LED mounting substrate have been developed.

[0040] Figure 7 This is a cross-sectional view of a state where a coating film of a photosensitive resin composition on an LED mounting substrate is cured after development.

[0041] Figure 8 Schematic diagram showing an example of a bump formed on a wiring electrode of a substrate

[0042] Fig. 9 Schematic diagram showing an example of a method for manufacturing an LED mounting substrate DETAILED DESCRIPTION

[0043] The present invention is a method for manufacturing an LED mounting substrate with a cured film, which comprises the following steps in sequence: a step of applying a photosensitive resin composition to an LED mounting substrate including a substrate having wiring electrodes, bumps formed on the wiring electrodes, and carrying a plurality of LED elements mounted on the bumps, and filling the gap between the LED element and the substrate having wiring electrodes and the space between adjacent LED elements with the coating film; a step of drying the coating film to form a dry film; a step of exposing the dry film; a step of developing and removing unnecessary parts of the exposed dry film; and a step of forming the developed coating film into a cured film.

[0044] <LED mounting substrate>

[0045] The LED mounting substrate in the present invention refers to, for example, Figure 1 and Figure 2 A substrate as shown. Figure 1 This is a picture of the LED mounting substrate viewed from above. Figure 2 for Figure 1 Cross-sectional view at line AA'.

[0046] Wiring electrodes 2 are arranged on and inside the substrate 1, and a portion of the wiring electrodes connected to the LED electrodes 3 is partially exposed. A bump 4 formed of a conductive material is formed on the exposed wiring electrodes, and an LED element 5 is mounted via the bump. As the substrate, for example, a glass plate, a resin plate, a resin film, etc. can be cited. As the wiring electrodes, for example, metal electrodes can be cited. As the LED element, two LED electrodes can be provided on one side, or one LED electrode can be provided on each of the two sides.

[0047] <Step of Providing a Coating Film of Photosensitive Resin Composition>

[0048] As a process for forming a coating film of a photosensitive resin composition on an LED mounting substrate, for example, a process using methods such as micro-gravure coating, spin coating, dip coating, curtain coating, roller coating, spray coating, and slit coating can be cited. Among them, spin coating and slit coating are preferred from the viewpoint of improving the flatness of the film. Using these methods, the gap between the LED element and the substrate with wiring electrodes and the space between adjacent LED elements are filled with a coating film. Filling here refers to setting a coating film in the gap between the LED element and the substrate with wiring electrodes and the space between adjacent LED elements. The photosensitive resin composition is preferably a photosensitive coloring resin composition. The so-called photosensitive coloring resin composition refers to a photosensitive resin composition that is not colorless and transparent but colored. By using a photosensitive coloring resin composition, the efficiency of taking out the light from the LED element is improved, and the light-emitting characteristics of the LED mounting substrate are improved by suppressing stray light, etc.

[0049] Figure 3 A schematic diagram showing a state in which a coating film of a photosensitive resin composition is formed on an LED mounting substrate.

[0050] <Step of drying the coating film to form a dried film>

[0051] The step of drying the coating film to form a dried film may be, for example, a method using a heating device such as a hot plate, a vacuum dryer, a vacuum hot plate, an oven, etc. The drying temperature is preferably 10 to 110° C., and the drying time is preferably 30 seconds to 30 minutes. Figure 4A schematic diagram showing a state in which a dry film of a photosensitive resin composition is formed on an LED mounting substrate.

[0052] <Step of exposing the dried film to light>

[0053] Regarding the process of exposing the dried film, the exposure can be performed through a desired mask or without a mask. Examples of exposure machines include a stepper, a mirror projection mask exposure machine (MPA), a parallel light mask exposure machine (hereinafter, "PLA"), etc. The exposure intensity is generally 10 to 4000 J / m 2 As the exposure light source, for example, ultraviolet rays such as i-rays, g-rays, and h-rays, KrF (wavelength 248 nm) lasers, ArF (wavelength 193 nm) lasers, etc. can be cited. Figure 5 A schematic diagram showing the case where a dried film of a photosensitive resin composition is exposed through a mask.

[0054] <Step of removing unnecessary portions of the exposed dried film by development>

[0055] As a process for developing and removing the unnecessary part of the dry film after exposure, for example, a developing method such as spraying, dipping, and paddle can be cited. The time of immersion in the developer is preferably 5 seconds to 5 minutes. As a developer, for example, an alkaline developer containing an aqueous solution of an inorganic base such as hydroxide, carbonate, phosphate, silicate, borate, etc. of an alkali metal, amines such as 2-diethylaminoethanol, monoethanolamine, diethanolamine, tetramethylammonium hydroxide, quaternary ammonium salts such as choline, etc. can be cited. Preferably, after development, it is rinsed with water. It should be noted that, for the purpose of protecting the electrode, it is preferred that the developed film remain at least around the bump and the wiring electrode. As a method, a method can be cited in which the dry film is dissolved from the upper layer, and the developer is washed away by rinsing at a moment when the bottom of the substrate can be visually confirmed. The gap between the LED element and the substrate with the wiring electrode is very small, and the developer is not easy to penetrate, so the dissolution of the dry film is not easy to proceed compared with other parts. Therefore, the developed film can be left around the bump and the wiring electrode. Figure 6 A schematic diagram showing a coating film of a photosensitive resin composition formed on an LED mounting substrate after development. Figure 6 As shown in FIG. 1 , it is found that the developed film remains in the gap portion.

[0056] <Step of converting the developed coating film into a cured film>

[0057] As the process of making the developed coating film into a cured film, for example, a heat curing method by applying heat from a hot plate, an oven, etc., and a light curing method by irradiating light with an ultraviolet lamp, an LED lamp, etc. are mentioned. The heat curing temperature is preferably 60 to 230°C, and the heat curing time is preferably about 15 minutes to 2 hours. For light curing, the exposure intensity is preferably 10 to 4000 J / m 2 About (converted by wavelength 365nm exposure). As a method for curing the developed coating film, a thermal curing method is preferred from the viewpoint that the developed coating film can be cured efficiently regardless of its formation location. By making the developed coating film into a cured film, the cross-linking reaction of the resin proceeds, and the reliability of the cured film is improved. Figure 7 This is a cross-sectional view showing a state where a cured film of a photosensitive resin composition is formed on an LED mounting substrate.

[0058] <Bump>

[0059] The bumps in the present invention are formed on the wiring electrodes of the substrate. Figure 8 An example of a substrate on which a bump 4 is formed is shown. The bump in the present invention is preferably formed of a conductive material, and may also be a mixture with a metal such as solder, a resin, etc. The bump in the present invention is more preferably a bump formed of a composite material of (A) an organic component and (B) conductive particles. The bump formed of a composite material of (A) an organic component and (B) conductive particles has low rigidity, and therefore can improve the mountability of the LED chip.

[0060] As a method for forming a bump formed of a composite material of (A) an organic component and (B) conductive particles on a wiring electrode, there can be cited a pattern printing method such as screen printing or gravure printing of a photosensitive conductive paste, a laser etching method of removing unnecessary parts after rough pattern printing, a photolithography method of exposing and developing a photosensitive conductive paste, etc. Among them, a method of forming a pattern using a photosensitive conductive paste by an exposure and development process is preferred because it can form a fine pattern.

[0061] In the photolithography method, as the light source for exposure, an ultra-high pressure mercury lamp, a laser, or i-rays (365 nm) or h-rays (405 nm) of an LED are preferably used.

[0062] In the photolithography method, examples of the developer include aqueous solutions of tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine or 1,6-hexanediamine.

[0063] The shape of the pattern is not particularly limited, and examples of the planar shape include rectangular, circular, elliptical, triangular, polygonal, and combinations thereof. The shape of the pattern can be determined by the shape of the electrode on the LED side.

[0064] Bump thickness B H It is preferably 0.1 to 5.0 μm. Figure 8 In the case of a substrate with a bump formed thereon, the thickness of the bump is represented by symbol B. H By making the thickness of the bump B H The thickness B of the bump is 0.1 μm or more, so that the impact during LED mounting can be mitigated and the mounting performance can be improved. H More preferably, it is 1.0 μm or more, and even more preferably, it is 1.5 μm or more. Here, the so-called "mountability" refers to the state in which the two electrodes of the LED and the two electrodes on the LED mounting substrate side can be electrically connected respectively, which can be evaluated by applying voltage to a plurality of manufactured LED mounting substrates and counting the number of LED lightings. On the other hand, by making the thickness B of the bump H The thickness of the bump is 5.0 μm or less, thereby suppressing the expansion of the bump during mounting and suppressing short circuits with surrounding electrodes, thereby improving mounting properties. H More preferably, it is 3.5 μm or less. The thickness of the bump can be measured by non-contact measurement using a laser microscope.

[0065] (A) Organic ingredients

[0066] (A) The organic component may include a substance having acrylic copolymers, epoxy resins, silicone resins, polyimide resins, phenolic resins, etc. as main components, preferably containing acrylic copolymers and epoxy resins having carboxyl groups. By including acrylic copolymers and epoxy resins having carboxyl groups in the organic component, the carboxyl groups and epoxy groups react with the organic components in the bump and the insulating layer to undergo a thermosetting reaction, thereby improving the adhesion between the LED electrode and the bump after thermal compression bonding, and further improving the connection reliability.

[0067] As the carboxyl group-containing acrylic copolymer, a copolymer of an acrylic monofunctional monomer and an unsaturated acid or an anhydride thereof is preferred.

[0068] Examples of the acrylic monofunctional monomer include methyl acrylate, ethyl acrylate, 2-ethylhexyl acrylate, n-butyl acrylate, isobutyl acrylate, isopropyl acrylate, glycidyl acrylate, butoxytriethylene glycol acrylate, dicyclopentyl acrylate, dicyclopentenyl acrylate, 2-hydroxyethyl acrylate, isobornyl acrylate, 2-hydroxypropyl acrylate, isodecyl acrylate, isooctyl acrylate, lauryl acrylate, 2-methoxyethyl acrylate, methoxyethylene glycol acrylate, methoxydiglycol acrylate, octafluoropentyl acrylate, phenoxyethyl acrylate, stearyl acrylate, trifluoroethyl acrylate, aminoethyl acrylate, phenyl acrylate, phenoxyethyl acrylate, 1-naphthyl acrylate, 2-methoxyethyl acrylate, Naphthyl ester, thiophenol acrylate, benzyl mercaptan acrylate, acrylamide, N-methoxymethyl acrylamide, N-ethoxymethyl acrylamide, N-n-butoxymethyl acrylamide, N-isobutoxymethyl acrylamide, methacrylic acid phenol, methacrylamide phenol, γ-acryloxypropyl trimethoxysilane, N-(2-hydroxyphenyl) acrylamide, N-(3-hydroxyphenyl) acrylamide, N-(4-hydroxyphenyl) acrylamide, o-hydroxyphenyl acrylate, m-hydroxyphenyl acrylate, p-hydroxyphenyl acrylate, o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, 2-(2-hydroxyphenyl) ethyl acrylate, 2-(3-hydroxyphenyl) ethyl acrylate, 2-(4-hydroxyphenyl) ethyl acrylate, etc. Two or more of them can be used. Among them, ethyl acrylate, 2-hydroxyethyl acrylate, and isobornyl acrylate are preferred.

[0069] As unsaturated acid or its anhydride, for example, acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinyl acetate, their anhydrides, etc. can be mentioned. Two or more of them can be used. The acid value of the acrylic copolymer containing a carboxyl group can be adjusted by the copolymerization ratio of the unsaturated acid.

[0070] Examples of epoxy resins include bisphenol A type, cresol novolac type, phenol novolac type, bisphenol A novolac type, dicyclopentadiene type, naphthalene type, etc., and preferably, the one having a softening point of 30° C. or higher and 100° C. or lower is preferred. If the softening point is 30° C. or higher, the occurrence of short circuit failure with nearby bumps caused by excessive flow during heat compression bonding can be suppressed, and if it is 100° C. or lower, low-temperature component mounting can be performed. More specifically, EPICRON N-660, EPICRON N-670, EPICRON N-680, EPICRON N-770, EPICRON N-775, EPICRON 840, EPICRON N-865, EPICRON N-890, EPICRON HP-7200L, EPICRON HP-7200, EPICRON HP-7200H, EPICRON HP-4700 manufactured by DIC Corporation, KAYARAD NC-3000, NC-3000H manufactured by Nippon Kayaku Co., Ltd., etc. Two or more of these may be used.

[0071] (B) Conductive particles

[0072] As (B) conductive particles, for example, particles of silver, gold, copper, platinum, lead, tin, nickel, aluminum, tungsten, molybdenum, chromium, titanium, indium, magnesium, cobalt, zinc, potassium, lithium, iron, mercury, beryllium, cadmium, rhodium, ruthenium, iridium, their alloys, and carbon black can be cited. Two or more of them can be contained. Among them, from the viewpoint of conductivity, particles of metals selected from silver, gold and copper are preferably selected, and silver particles are more preferably considered from the viewpoint of cost and stability. In addition, (B) conductive particles can be substances obtained by coating the surface of resins, inorganic oxides, etc. The conductive particles obtained by coating the surface of resin particles with metals are preferably metal particles because they have rebound caused by resin particles during transfer.

[0073] The aspect ratio of the conductive particles (B) is preferably 1.1 to 2.0, which is a value obtained by dividing the major axis length by the minor axis length. The aspect ratio of the conductive particles (B) can be calculated by observing the conductive particles (B) with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) at a magnification of 15,000 times, measuring the major axis length and the minor axis length of each of 100 primary particles of the conductive particles selected at random, and calculating the average value of the two.

[0074] The average particle size of the conductive particles (B) is preferably 0.05 to 1.0 μm. By having an average particle size of 0.05 μm or more, the number of conductive paths in the bump increases, and the electrical connection reliability can be further improved. On the other hand, by having an average particle size of 1.0 μm or less, the surface smoothness, pattern accuracy, and dimensional accuracy of the resulting bump can be improved. Here, the average particle size of the conductive particles (B) can be measured using a laser irradiation type particle size distribution meter. The value of D50 of the particle size distribution obtained by the measurement is set to the average particle size (D50) of the conductive particles.

[0075] The proportion of (B) conductive particles in the total weight of the bump formed by the composite material of (A) organic component and (B) conductive particles is preferably 50 to 90wt%. If the proportion of (B) conductive particles is 50wt% or more, the number of conductive paths formed in the bump increases, and the electrical connection reliability can be further improved. The proportion of (B) conductive particles is more preferably 60wt% or more. In addition, if the proportion of (B) conductive particles is 90wt% or less, the rigidity of the bump becomes lower, the capture property is improved, and the position accuracy can be high, which can further improve the mounting performance. In addition, by increasing the content of the organic component, the adhesion between the bump and the electrode of the LED is improved, thereby further improving the connection reliability. The proportion of (B) conductive particles is more preferably 80wt% or less. Regarding the proportion of (B) conductive particles in the total weight of the bump, the bump on the substrate can be scraped off and calculated by thermogravimetric analysis from the weight of the residual component after the organic component is burned off.

[0076] <Photosensitive resin composition>

[0077] The photosensitive resin composition of the present invention is a material whose solubility in a developer changes due to the action of light. As the photosensitive resin composition of the present invention, from the viewpoint of improving the reflectivity and light-shielding properties of the cured film, it is preferred to contain (G) a coloring pigment. The photosensitive resin composition containing the (G) coloring pigment is set as a photosensitive coloring resin composition. In addition, as the photosensitive coloring resin composition of the present invention, it is preferred to contain (C) a resin, (D) a photopolymerization initiator, (E) a photopolymerization compound, and (F) an organic solvent in addition to the (G) coloring pigment. From the viewpoint of filling the gap between the LED element and the substrate having wiring electrodes and the space between adjacent LED elements without defects such as bubbles, the viscosity of the photosensitive coloring resin composition of the present invention at 25°C is preferably 30 mPa·s or less, and more preferably 10 mPa·s. By filling the gap between the LED element and the substrate having wiring electrodes and the space between adjacent LED elements without defects, the reliability of the LED element can be improved, so it is preferred. On the other hand, from the viewpoint of suppressing fluidity and improving the uniformity of the coating film thickness, it is preferably 1 mPa·s or more, more preferably 2 mPa·s or more. The viscosity is a value measured at 100 rpm using a cone-plate viscometer set at 25.0±0.2°C.

[0078] (C) Resin

[0079] Examples of the resin (C) include siloxane, polyimide, a polyimide precursor, polybenzoic acid, Azoles, polybenzo The present invention can be used in combination with (C-1) siloxane resins, such as oxazole precursors, (meth) acrylic polymers, etc. Here, the so-called (meth) acrylic polymers refer to polymers of methacrylate and / or acrylate. Two or more of these can be contained. Among them, (C-1) siloxane resins are preferred from the perspective of transparency, heat resistance and light resistance.

[0080] The siloxane resin (C-1) is a hydrolysis / dehydration condensate of an organic silane and in the present invention comprises at least a repeating unit represented by the formula (1) and / or a repeating unit represented by the formula (2).

[0081]

[0082] In formula (1) and formula (2), R 2 represents a linear alkylene group having 1 to 6 carbon atoms, R 1 represents a hydrogen atom or a methyl group, R 3 It represents an alkyl group having 1 to 20 carbon atoms. * represents a bonding site.

[0083] By including these repeating units, the side chains of the siloxane resin react with free radicals generated by the cleavage of the photopolymerization initiator (D) during exposure. As a result, the contrast of the curing degree between the exposed part and the unexposed part is easily formed, thereby improving the resolution and suppressing the development residue.

[0084] (C-1) The siloxane resin is characterized by containing a total of 10 to 50 mol% of the repeating unit represented by formula (1) and the repeating unit represented by formula (2) in all the repeating units of the siloxane resin. By making the total content of the repeating unit represented by formula (1) and formula (2) 10 mol% or more, a contrast between the curing degrees of the exposed part and the unexposed part is formed, and the resolution can be improved. On the other hand, by containing 50 mol% or less of these repeating units, excessive curing of the exposed part can be suppressed, and the resolution can be further improved.

[0085] The content ratio of the organosilane unit including the repeating unit represented by the formula (1) and the repeating unit represented by the formula (2) can be determined by 29 Si-NMR measurement was performed by calculating the ratio of the integrated value of Si derived from the organosilane unit having the repeating unit represented by the formula (1) and the repeating unit represented by the formula (2) to the integrated value of the entire Si derived from the organosilane.

[0086] Furthermore, the siloxane resin preferably contains a repeating unit represented by formula (3) and / or a repeating unit represented by formula (4).

[0087]

[0088] In formula (3) and formula (4), R 4 R represents a monovalent organic group having 1 to 20 carbon atoms and having a carboxyl group and / or a carboxylic anhydride group. 5 It represents an alkyl group having 1 to 20 carbon atoms. * represents a bonding site.

[0089] By including the repeating unit represented by the formula (3) and / or the repeating unit represented by the formula (4), excellent developing solubility can be obtained, and the resolution can be improved.

[0090] In addition, the repeating unit represented by formula (3) and the repeating unit represented by formula (4) preferably contain 5 to 20 mol% of the total repeating amount of the siloxane resin (A). By containing 5 mol% or more of these repeating units, the development residue can be further suppressed. On the other hand, by containing 20 mol% or less of these repeating units, the resolution can be further improved.

[0091] The content ratio of the organosilane unit including the repeating unit represented by the formula (3) and the repeating unit represented by the formula (4) can be determined by 29Si-NMR measurement was performed by calculating the ratio of the integrated value of Si derived from the organosilane unit having the repeating unit represented by the formula (3) and the repeating unit represented by the formula (4) to the integrated value of the entire Si derived from the organosilane.

[0092] The siloxane resin (C-1) may contain other repeating units. As other repeating units, repeating units having non-aromatic functional groups are preferred, and the presence of such repeating units can improve light resistance.

[0093] The repeating units represented by formulae (1) to (4) are derived from the organosilane compounds represented by formulae (5) to (8), respectively.

[0094] That is, the repeating unit represented by the above formula (1) and / or the repeating unit represented by the formula (2) is derived from the organosilane compound represented by the formula (5) and / or the organosilane compound represented by the formula (6).

[0095] The repeating unit represented by the formula (3) and / or the repeating unit represented by the formula (4) is derived from the organosilane compound represented by the formula (7) and / or the organosilane compound represented by the formula (8).

[0096] The (C-1) polysiloxane resin having repeating units represented by formulae (1) to (4) can be obtained by hydrolyzing and polycondensing the corresponding organosilane compounds represented by formulae (5) to (8). Other organosilane compounds may be further used.

[0097]

[0098] In the above formula (5) and formula (6), R 1 , R 2 and R 3 Each represents the same as R in formula (1) and formula (2) 1 , R 2 and R 3 The same group. a Each of them may be the same or different and represents a monovalent organic group having 1 to 20 carbon atoms, and is preferably an alkyl group having 1 to 6 carbon atoms.

[0099] In the above formulas (7) and (8), R 4 and R 5 Each represents the same as R in formula (3) and formula (4) 4 and R 5 The same group. a In the above formula (5) and formula (6), R a Same group.

[0100] Examples of the organosilane compound represented by formula (5) include γ-acryloylpropyltrimethoxysilane, γ-acryloylpropyltriethoxysilane, γ-methacryloylpropyltrimethoxysilane, and γ-methacryloylpropyltriethoxysilane, and two or more thereof may be used.

[0101] Examples of the organosilane compound represented by formula (6) include γ-acryloylpropylmethyldimethoxysilane, γ-acryloylpropylmethyldiethoxysilane, γ-methacryloylpropylmethyldimethoxysilane, and γ-methacryloylpropylmethyldiethoxysilane. Two or more of these may be used.

[0102] Examples of the organosilane compound having a structure represented by formula (7) include 3-trimethoxysilylpropionic acid, 3-triethoxysilylpropionic acid, 4-trimethoxysilylbutyric acid, 4-triethoxysilylbutyric acid, 5-trimethoxysilylvaleric acid, 5-triethoxysilylvaleric acid, 3-trimethoxysilylpropylsuccinic anhydride, 3-triethoxysilylpropylsuccinic anhydride, 3-trimethoxysilylpropylcyclohexyldicarboxylic anhydride, 3-triethoxysilylpropylcyclohexyldicarboxylic anhydride, 3-trimethoxysilylpropylphthalic anhydride, and 3-triethoxysilylpropylphthalic anhydride. Two or more of these may be used.

[0103] Examples of the organosilane compound having a structure represented by formula (8) include 3-dimethylmethoxysilylpropionic acid, 3-dimethylethoxysilylpropionic acid, 4-dimethylmethoxysilylbutyric acid, 4-dimethylethoxysilylbutyric acid, 5-dimethylmethoxysilylvaleric acid, 5-dimethylethoxysilylvaleric acid, 3-dimethylmethoxysilylpropylsuccinic anhydride, 3-dimethylethoxysilylpropylsuccinic anhydride, 3-dimethylmethoxysilylpropylcyclohexyldicarboxylic anhydride, and 3-dimethylethoxysilylpropylcyclohexyldicarboxylic anhydride. Two or more of these may be used.

[0104] Examples of other organosilane compounds include organosilane compounds such as tetramethoxysilane, tetraethoxysilane, and silicate 51 (tetraethoxysilane oligomer). Two or more of these may be used.

[0105] From the viewpoint of coating properties, the weight average molecular weight (Mw) of the siloxane resin (C-1) is preferably 1,000 or more, and more preferably 2,000 or more. On the other hand, from the viewpoint of developability, the Mw of the siloxane resin (A) is preferably 50,000 or less, and more preferably 20,000 or less. Here, the Mw of the siloxane resin in the present invention refers to a polystyrene conversion value measured by gel permeation chromatography (GPC).

[0106] In the photosensitive color resin composition, the content of the (C) resin can be arbitrarily set according to the desired film thickness and application, but is generally 10 to 50% by weight in the solid content of the photosensitive color resin composition. In addition, the content of the (C) resin is preferably 10% by weight or more, more preferably 20% by weight or more in the solid content of the photosensitive color resin composition. On the other hand, the content of the (C) resin is preferably 50% by weight or less in the solid content of the photosensitive color resin composition.

[0107] The siloxane resin (C-1) can be obtained by hydrolyzing the above-mentioned organosilane compound and then subjecting the hydrolyzate to a dehydration condensation reaction in the presence of a solvent or in the absence of a solvent.

[0108] Various conditions in the hydrolysis can be set according to physical properties suitable for the intended use in consideration of the reaction scale, the size and shape of the reaction container, etc. Examples of the various conditions include acid concentration, reaction temperature, reaction time, and the like.

[0109] In the hydrolysis reaction, an acid catalyst such as hydrochloric acid, acetic acid, formic acid, nitric acid, oxalic acid, hydrochloric acid, sulfuric acid, phosphoric acid, polyphosphoric acid, polycarboxylic acid, anhydrides thereof, ion exchange resins, etc. can be used. Among them, an acidic aqueous solution containing formic acid, acetic acid and / or phosphoric acid is preferred.

[0110] In the case of using an acid catalyst for the hydrolysis reaction, from the viewpoint of making the hydrolysis proceed more rapidly, the amount of the acid catalyst added is preferably 0.05 parts by weight or more, more preferably 0.1 parts by weight or more, relative to 100 parts by weight of the total organosilane compounds used for the hydrolysis reaction. On the other hand, from the viewpoint of appropriately adjusting the progress of the hydrolysis reaction, the amount of the acid catalyst added is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, relative to 100 parts by weight of the total organosilane compounds. Here, the so-called total organosilane compound amount refers to the amount of the total organosilane compound, its hydrolyzate and its condensate, and the same applies below.

[0111] The hydrolysis reaction can be carried out in an organic solvent. The organic solvent can be appropriately selected in consideration of the stability, wettability, volatility, etc. of the photosensitive colored resin composition. Examples of the organic solvent include alcohols such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, tert-butanol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxy-1-butanol, and diacetone alcohol; glycols such as ethylene glycol and propylene glycol; ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol mono-tert-butyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, and diethyl ether; and ethers such as methyl ethyl ketone, acetyl Ketones such as acetone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, and 2-heptanone; amides such as dimethylformamide and dimethylacetamide; acetates such as ethyl acetate, propyl acetate, butyl acetate, isobutyl acetate, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, methyl lactate, ethyl lactate, and butyl lactate; aromatic or aliphatic hydrocarbons such as toluene, xylene, hexane, and cyclohexane; γ-butyrolactone, N-methyl-2-pyrrolidone, and dimethyl sulfoxide. Two or more of these may be used.

[0112] Among them, diacetone alcohol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol mono-tert-butyl ether, γ-butyrolactone, etc. are preferably used from the viewpoint of crack resistance of the cured film.

[0113] When an organic solvent is generated by the hydrolysis reaction, the hydrolysis can be performed without a solvent. It is also preferred to further add an organic solvent after the hydrolysis reaction to adjust the concentration to an appropriate concentration as a photosensitive coloring composition. In addition, after the hydrolysis, the total amount or a part of the generated alcohol etc. can be distilled off and removed by heating and / or reducing pressure, and then a suitable organic solvent can be added.

[0114] When an organic solvent is used in the hydrolysis reaction, the amount of the organic solvent added is preferably 50 parts by weight or more, more preferably 80 parts by weight or more, based on 100 parts by weight of the total organosilane compound, from the viewpoint of suppressing the formation of gel. On the other hand, from the viewpoint of causing the hydrolysis to proceed more rapidly, the amount of the organic solvent added is preferably 500 parts by weight or less, more preferably 200 parts by weight or less, based on 100 parts by weight of the total organosilane compound.

[0115] In addition, as water used for the hydrolysis reaction, ion-exchanged water is preferred. The amount of water can be arbitrarily set, but is preferably 1.0 to 4.0 mol per 1 mol of the total organosilane compound.

[0116] As a method for the dehydration condensation reaction, for example, a method of directly heating a silanol compound solution obtained by the hydrolysis reaction of an organic silane compound can be cited. The heating temperature is preferably above 50° C. and below the boiling point of the solvent, and the heating time is preferably 1 to 100 hours. In addition, in order to increase the degree of polymerization of the siloxane resin, reheating or addition of an alkali catalyst can be performed. In addition, according to the purpose, after hydrolysis, an appropriate amount of generated alcohol can be distilled off and removed under heating and / or reduced pressure, and then a suitable solvent can be added.

[0117] From the perspective of storage stability of the photosensitive colored resin composition, it is preferred that the above-mentioned catalyst is not contained in the siloxane resin solution after hydrolysis and dehydration condensation, and the catalyst can be removed as needed. As a catalyst removal method, from the perspective of ease of operation and removability, water washing, treatment with ion exchange resin, etc. are preferred. The so-called water washing is a method in which the siloxane resin solution is diluted with an appropriate hydrophobic solvent, washed with water several times, and the resulting organic layer is concentrated using an evaporator or the like. The so-called treatment with ion exchange resin is a method in which the siloxane resin solution is contacted with an appropriate ion exchange resin.

[0118] (D) Photopolymerization initiator

[0119] (D) The photopolymerization initiator may be any substance as long as it is decomposed and / or reacted by light (including ultraviolet rays and electron beams) to generate free radicals. Examples thereof include α-aminoalkylphenone compounds such as 2-methyl-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholino-4-yl-phenyl)-butane-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1; 2,4,6-trimethylbenzoylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)-phosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)-phosphine oxide. Acylphosphine oxide compounds such as phosphine oxide; 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl) oxime, 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyl oxime)], 1-phenyl-1,2-butanedione-2-(O-methoxycarbonyl) oxime, 1,3-diphenylpropanetrione-2-(O-ethoxycarbonyl) oxime, ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime) and other oxime ester compounds; benzyl ketal compounds such as benzyl dimethyl ketal; 2- α-Hydroxy ketone compounds such as hydroxy-2-methyl-1-phenylpropane-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl-phenylketone, etc.; benzophenone, 4,4-bis(dimethylamino)benzophenone, 4,4-bis(diethylamino)benzophenone, O-benzoylbenzoic acid methyl ester, 4-phenylbenzophenone, 4,4-dichlorobenzophenone, hydroxybenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, alkane Benzophenone compounds such as benzophenone, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone; acetophenone compounds such as 2,2-diethoxyacetophenone, 2,3-diethoxyacetophenone, 4-tert-butyldichloroacetophenone, benzylideneacetophenone, 4-azidobenzylideneacetophenone; aromatic ketoester compounds such as methyl 2-phenyl-2-oxyacetate; benzoate compounds such as ethyl 4-dimethylaminobenzoate, (2-ethyl)hexyl 4-dimethylaminobenzoate, ethyl 4-diethylaminobenzoate, methyl 2-benzoylbenzoate, etc. Two or more of these may be contained.

[0120] In order to suppress coloration caused by the (D) photopolymerization initiator, the photosensitive colored resin composition preferably uses an acylphosphine oxide-based photopolymerization initiator such as 2,4,6-trimethylbenzoylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)-phosphine oxide.

[0121] From the viewpoint of efficiently performing radical curing, the content of the (D) photopolymerization initiator in the photosensitive colored resin composition is preferably 0.01% by weight or more, more preferably 1% by weight or more in the solid content. On the other hand, from the viewpoint of suppressing the elution of the residual (D) photopolymerization initiator, the content of the (D) photopolymerization initiator is preferably 20% by weight or less, more preferably 10% by weight or less in the solid content.

[0122] (E) Photopolymerizable compound

[0123] The so-called (E) photopolymerizable compound refers to a compound having two or more ethylenically unsaturated double bonds in the molecule. If the ease of free radical polymerization is considered, the (E) photopolymerizable compound preferably has a (meth)acryloyl group. In addition, from the viewpoint of further improving the sensitivity in pattern processing, the double bond equivalent of the (E) photopolymerizable compound is preferably 400 g / mol or less. On the other hand, from the viewpoint of further improving the resolution in pattern processing, the double bond equivalent of the (E) photopolymerizable compound is preferably 80 g / mol or more.

[0124] Examples of the photopolymerizable compound (E) include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,3-butanediol diacrylate, 1,3-butanediol dimethacrylate, neopentyl glycol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, Dimethylol-tricyclodecane diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, tripentaerythritol heptaacrylate, tripentaerythritol octaacrylate, four-pentaerythritol nonaacrylate, four-pentaerythritol decaacrylate, pentaerythritol undecaacrylate, pentaerythritol dodecaacrylate, tripentaerythritol heptamethacrylate, tripentaerythritol octamethacrylate, four-pentaerythritol nonamethacrylate, four-pentaerythritol decamethacrylate, pentaerythritol undecamethacrylate, pentaerythritol dodecamethacrylate, and dimethylol-tricyclodecane diacrylate. Two or more of these may be contained.

[0125] From the viewpoint of efficiently performing radical curing, the content of the (E) photopolymerizable compound in the photosensitive color resin composition is preferably 1% by weight or more in the solid content of the photosensitive color resin composition. On the other hand, from the viewpoint of suppressing excessive reaction of free radicals and further improving resolution, the content of the (E) photopolymerizable compound is preferably 40% by weight or less in the solid content.

[0126] (F) Organic solvents

[0127] The photosensitive color resin composition of the present invention preferably contains (F) an organic solvent.

[0128] As the organic solvent, it is preferred to combine an organic solvent having a boiling point of 150°C to 250°C at atmospheric pressure with an organic solvent having a boiling point of less than 150°C. By containing an organic solvent having a boiling point of 150°C to 250°C, the organic solvent volatilizes appropriately during coating and the coating film is dried, thereby suppressing uneven coating and improving the uniformity of film thickness. Furthermore, by containing an organic solvent having a boiling point of less than 150°C at atmospheric pressure, it is possible to suppress the residual organic solvent in the cured film of the present invention described later. From the viewpoint of suppressing the residual organic solvent in the cured film and improving the chemical resistance and adhesion for a long time, it is preferred to contain an organic solvent having a boiling point of less than 150°C at atmospheric pressure, which accounts for more than 50% by weight of the total organic solvent.

[0129] As the organic solvent having a boiling point of less than 150° C. under atmospheric pressure, for example, ethanol, isopropanol, 1-propanol, 1-butanol, 2-butanol, isopentanol, ethylene glycol monomethyl ether, ethylene glycol dimethyl ether, ethylene glycol monoethyl ether, methoxymethyl acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monopropyl ether, ethylene glycol monomethyl ether acetate, 1-methoxypropyl-2-acetate, acetol, acetylacetone, methyl isobutyl ketone, methyl ethyl ketone, methyl propyl ketone, methyl lactate, toluene, cyclopentanone, cyclohexane, n-heptane, benzene, methyl acetate, ethyl acetate, propyl acetate, isobutyl acetate, butyl acetate, isopentyl acetate, amyl acetate, 3-hydroxy-3-methyl-2-butanone, 4-hydroxy-3-methyl-2-butanone, and 5-hydroxy-2-pentanone can be used. Two or more of these can be used.

[0130] As the organic solvent having a boiling point of 150° C. or more and 250° C. or less under atmospheric pressure, for example, ethylene glycol diethyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol mono-tert-butyl ether, propylene glycol mono-n-butyl ether, propylene glycol mono-tert-butyl ether, 2-ethoxyethyl acetate, 3-methoxy-1-butanol, 3-methoxy-3-methylbutanol, 3-methoxy-3-methylbutyl acetate, 3-methoxybutyl acetate, 3-ethoxyethyl propionate, propylene glycol monomethyl ether propionate, dipropylene glycol methyl ether, diisobutyl ketone, diacetone alcohol, ethyl lactate, butyl lactate, dimethylformamide, dimethylacetamide, γ-butyrolactone, γ-valerolactone, δ-valerolactone, propylene carbonate, N-methylpyrrolidone, cyclohexanone, cycloheptanone, diethylene glycol monobutyl ether, ethylene glycol dibutyl ether. Two or more of these can be used.

[0131] The content of the organic solvent can be arbitrarily set according to the coating method, etc. For example, when the film is formed by spin coating, the content is generally 50% by weight or more and 95% by weight or less in the photosensitive coloring resin composition.

[0132] (G) Coloring Pigments

[0133] The photosensitive colored resin composition of the present invention preferably contains (G) coloring pigment. By containing (G) coloring pigment, the light-shielding property of the cured film can be improved. In addition, as a coloring pigment, it is further preferred to contain at least (G-1) white pigment. By including (G-1) white pigment, the reflectivity of the cured film can be improved. As (G-1) white pigment, for example, titanium dioxide, magnesium oxide, barium sulfate, zirconium oxide, zinc oxide, white lead, etc. can be mentioned. It can contain two or more of them. Among them, it is preferred to contain at least one of titanium dioxide, zirconium oxide, zinc oxide, barium sulfate and their composite compounds, and titanium dioxide with high reflectivity and easy industrial use is more preferred.

[0134] The crystal structure of titanium dioxide is classified into anatase type, rutile type, and brookite type. Among them, rutile type titanium dioxide is preferred because of its low photocatalytic activity.

[0135] The (G-1) white pigment may be subjected to a surface treatment, preferably a surface treatment with Al, Si and / or Zr, which can improve the dispersibility of the (G-1) white pigment in the photosensitive color resin composition and further improve the light resistance and heat resistance of the cured film.

[0136] From the viewpoint of further improving the reflectivity, the average primary particle size of the white pigment (G-1) is preferably 170 to 310 nm. The average primary particle size of the white pigment (G-1) here refers to the median particle size calculated from the particle size distribution measured by laser diffraction.

[0137] Examples of titanium dioxide pigments preferably used as the white pigment (G-1) include R960; manufactured by Dupont Co., Ltd. (rutile type, SiO2 / Al2O3 treated, average primary particle size 210 nm), CR-97; manufactured by Ishihara Sangyo Co., Ltd. (rutile type, Al2O3 / ZrO2 treated, average primary particle size 250 nm), JR-301; manufactured by Teika Co., Ltd. (rutile type, Al2O3 / ZrO2 treated, average primary particle size 250 nm), and 3 treatment, average primary particle size 300nm), JR-405; Teika (co., Ltd.) (rutile type, Al2O3 treatment, average primary particle size 210nm), JR-600A; Teika (co., Ltd.) (rutile type, Al2O3 treatment, average primary particle size 250nm), JR-603; Teika (co., Ltd.) (rutile type, Al2O3 / ZrO2 treatment, average primary particle size 280nm), etc. Two or more of them may be contained.

[0138] From the viewpoint of further improving the reflectivity, the content of the white pigment (G-1) is preferably 10% by weight or more, more preferably 20% by weight or more, in the solid content of the photosensitive color resin composition. On the other hand, from the viewpoint of suppressing development residues and forming a pattern with higher resolution, the content of the white pigment (G-1) is preferably 80% by weight or less, more preferably 60% by weight or less, in the solid content.

[0139] The photosensitive coloring resin composition may contain a pigment dispersant together with the (G-1) white pigment, so that the dispersibility of the (G-1) white pigment in the photosensitive coloring resin composition can be improved. The pigment dispersant is appropriately selected according to the type and surface state of the white pigment used. The pigment dispersant preferably contains an acidic group and / or a basic group. Examples of commercially available pigment dispersants include "Disperbyk" (registered trademark) 106, "Disperbyk" 108, "Disperbyk" 110, "Disperbyk" 180, "Disperbyk" 190, "Disperbyk" 2001, "Disperbyk" 2155, "Disperbyk" 140, "Disperbyk" 145 (above, trade names, manufactured by Bicchem (KK)), etc. Two or more of them may be contained.

[0140] In addition, the photosensitive colored resin composition of the present invention may contain (H) black pigment as needed. By containing (H) black pigment, the light-shielding property of the cured film can be improved. As (H) black pigment, for example, black organic pigment, mixed color organic pigment, black inorganic pigment, etc. can be mentioned. As black organic pigment, for example, carbon black, perylene black, aniline black, benzofuranone pigment, etc. can be mentioned. They can be coated with resin. As mixed color organic pigment, for example, a substance that is pseudo-blackened by mixing two or more pigments of red, blue, green, purple, yellow, magenta and / or cyan can be mentioned. Among them, from the viewpoint of having both moderately high OD value and pattern processability, a mixed pigment of red pigment and blue pigment is preferred. The weight ratio of red pigment to blue pigment is preferably 20 / 80 to 80 / 20, and more preferably 30 / 70 to 70 / 30. If the specific examples of representative pigments are represented by pigment index (CI) numbers, the following substances can be mentioned. As red pigment, for example, Pigment Red (hereinafter abbreviated as PR) 9, PR48, PR97, PR122, PR123, PR144, PR149, PR166, PR168, PR177, PR179, PR180, PR192, PR209, PR215, PR216, PR217, PR220, PR223, PR224, PR226, PR227, PR228, PR240, PR254, etc. can be mentioned. Two or more of them can be contained. As blue pigment, for example, Pigment Blue (hereinafter abbreviated as PB) 15, PB15:3, PB15:4, PB15:6, PB22, PB60, PB64, etc. can be mentioned. Two or more of them can be contained. Examples of black inorganic pigments include graphite, fine particles of metals such as titanium, copper, iron, manganese, cobalt, chromium, nickel, zinc, calcium, silver, gold, platinum, and palladium, metal oxides, metal composite oxides, metal sulfides, metal nitrides, metal oxynitrides, and metal carbides, etc. Two or more of these may be contained.

[0141] Among the above black pigments, from the perspective of having high light-shielding properties, it is further preferred to include at least one of titanium nitride, zirconium nitride, carbon black, and a mixed pigment of a red pigment and a blue pigment. From the perspective of adjusting the reflectivity and OD to suppress the color mixing of light in adjacent pixels, the content of the black pigment is preferably 0.2% by weight or more, more preferably 0.5% by weight or more. On the other hand, from the perspective of adjusting the reflectivity and OD, the content of the black pigment is preferably 5% by weight or less, more preferably 3% by weight or less.

[0142] The photosensitive colored resin composition of the present invention may contain (I) an organic metal compound as needed. The (I) organic metal compound has a function of improving light-shielding properties by decomposing / aggregating to form a black pigment in the exposure step and / or heating step when forming a pattern of a cured film.

[0143] As (I) the organometallic compound, it is more preferable to contain at least one metal selected from silver, gold, platinum and palladium from the viewpoint of having high light-shielding property. As the metal compound selected from silver, gold, platinum and palladium, for example, organometallic compounds containing silver such as silver neodecanoate, silver octoate and silver salicylate; organometallic compounds containing gold such as chloro(triphenylphosphine)gold and tetrachloroauric acid tetrahydrate; organometallic compounds containing platinum such as bis(acetylacetonate)platinum, dichlorobis(triphenylphosphine)platinum and dichlorobis(benzonitrile)platinum; organometallic compounds containing palladium such as bis(acetylacetonate)palladium, dichlorobis(triphenylphosphine)palladium, dichlorobis(benzonitrile)palladium, tetrakis(triphenylphosphine)palladium and dibenzylideneacetonepalladium, etc. Two or more of them may be contained. Among them, from the viewpoint of further improving the light-shielding property, bis(acetylacetonate)palladium, dichlorobis(triphenylphosphine)palladium, dichlorobis(benzonitrile)palladium and tetrakis(triphenylphosphine)palladium are more preferable.

[0144] (I) The content of the organic metal compound in the solid content of the photosensitive colored resin composition is preferably 0.2 to 5% by weight. By making the content of the organic metal compound 0.2% by weight or more, the OD value can be further improved. The content of the organic metal compound is more preferably 1.5% by weight or more. On the other hand, by making the content of the organic metal compound 5% by weight or less, the reflectivity can be further improved.

[0145] Moreover, the photosensitive color resin composition of this invention can further contain a crosslinking agent, an ultraviolet absorber, a polymerization inhibitor, a surfactant, etc. as needed.

[0146] By containing a crosslinking agent in the photosensitive colored resin composition, the crosslinking of the siloxane resin is promoted during heat curing, and the crosslinking degree of the cured film becomes high. Therefore, the reduction of the pattern resolution caused by the melting of the fine pattern during heat curing is suppressed. As a curing agent, for example, organic substances containing nitrogen, silicone resin curing agents, isocyanate compounds and polymers thereof, methylolated melamine derivatives, methylolated urea derivatives, various metal alcoholates, various metal chelates, thermal acid-generating materials, photoacid-generating materials, etc. can be cited. Two or more of them can be contained. Among them, from the viewpoints of the stability of the curing agent, the processability of the coating film, etc., methylolated melamine derivatives, methylolated urea derivatives, and photoacid-generating materials are preferably used.

[0147] The photosensitive colored resin composition contains an ultraviolet absorber, so that the light resistance of the cured film can be improved and the resolution can be further improved. As the ultraviolet absorber, from the viewpoint of further suppressing the color change caused by heating, it is preferable to use a benzotriazole compound such as 2-(2H-benzotriazol-2-yl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-tert-amylphenol, 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole; a benzophenone compound such as 2-hydroxy-4-methoxybenzophenone; and a triazine compound such as 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol. Two or more of these may be contained.

[0148] The photosensitive color resin composition contains a polymerization inhibitor, whereby the resolution can be improved. Examples of the polymerization inhibitor include di-tert-butylhydroxytoluene, butylhydroxyanisole, hydroquinone, 4-methoxyphenol, 1,4-benzoquinone, and tert-butylcatechol. In addition, examples of commercially available polymerization inhibitors include "IRGANOX" (registered trademark) 1010, "IRGANOX" 1035, "IRGANOX" 1076, "IRGANOX" 1098, "IRGANOX" 1135, "IRGANOX" 1330, "IRGANOX" 1726, "IRGANOX" 1425, "IRGANOX" 1520, "IRGANOX" 245, "IRGANOX" 259, "IRGANOX" 3114, "IRGANOX" 565, and "IRGANOX" 295 (these are trade names, manufactured by BASF Japan Co., Ltd.). Two or more of these may be contained.

[0149] When the photosensitive colored resin composition contains a surfactant, the fluidity during coating can be improved. Examples of the surfactant include "Microflex" (registered trademark) F142D, "Microflex" F172, "Microflex" F173, and "Microflex" "ク" F183, "メガファック" F445, "メガファック" F470, "メガファック" F475, "メガファック" F477 (above, trade name, D IC (manufactured by Co., Ltd.); silicone surfactants such as BYK (registered trademark)-333, BYK-301, BYK-331, BYK-345, BYK-307 (above, trade names, manufactured by Bicchemie Japan Co., Ltd.); polyoxyalkylene surfactants; poly(meth)acrylate surfactants, etc. Two or more of these may be contained.

[0150] The solid content concentration of the photosensitive color resin composition of the present invention can be arbitrarily set according to the coating method, etc. For example, when the film is formed by spin coating as described later, the solid content concentration is generally 5% by weight or more and 50% by weight or less. The so-called solid content here refers to all components except volatile components such as solvents among the components contained in the photosensitive color resin composition. The amount of the solid content can be obtained by measuring the residual component obtained by heating the photosensitive color resin composition at 250°C for 30 minutes to evaporate the volatile components.

[0151] Next, the method for producing the photosensitive colored resin composition of the present invention is described below. The photosensitive colored resin composition of the present invention can be obtained by mixing the above-mentioned (C) to (G) components and other components as required. More specifically, for example, it is preferred that (C) resin, (D) photopolymerization initiator, (E) photopolymerizable compound, (F) organic solvent, (G) coloring pigment and other components as required are stirred and dissolved, and filtered.

[0152] Next, the LED mounting substrate with a cured film of the present invention is described. The LED mounting substrate with a cured film of the present invention is composed of a substance obtained by forming a cured film composed of a cured product of the photosensitive resin composition of the present invention on the above-mentioned LED mounting substrate. The film thickness of the cured film is preferably 0.5 to 25 μm. By making the film thickness of the cured film greater than 0.5 μm, a cured film can be fully formed in the gap between the LED element and the substrate having wiring electrodes, so that the reliability of the LED element is improved, which is therefore preferred. In addition, by making the film thickness of the cured film less than 25 μm, the film uniformity of the cured film can be improved, which is therefore preferred.

[0153] Next, the component with an LED mounting substrate with a cured film in the present invention is described. The component with an LED mounting substrate with a cured film in the present invention can be manufactured by installing an IC driver for driving on the LED mounting substrate, etc. After the LED mounting substrate forms a bump formed of a composite material of an organic component and conductive particles formed on the electrode on a substrate having an electrode, a plurality of LED elements are mounted on the bump, at least a portion of the surrounding portion of the bump and the LED element is covered with a cured film of the photosensitive resin composition of the present invention, and a cured film of the photosensitive resin composition is also provided between adjacent LD elements. The cured film covering a portion of the surrounding portion of the bump and the LED element and the cured film located between adjacent LD elements preferably have the same composition. The cured film covering a portion of the surrounding portion of the bump and the LED element and the cured film located between adjacent LD elements can be formed together by using materials of the same composition, which can improve productivity.

[0154] Example

[0155] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. The compounds used in the Synthesis Examples and Examples for which abbreviations are used are shown below.

[0156] PGMEA: Propylene glycol monomethyl ether acetate

[0157] DAA: diacetone alcohol.

[0158] The solid content concentration of the polysiloxane solution and the acrylic resin solution in Synthesis Examples 1 and 2 was determined by the following method. 1.5 g of the polysiloxane solution or the acrylic resin solution was weighed in an aluminum cup and heated at 250° C. for 30 minutes using a hot plate to evaporate the liquid component. The weight of the solid content remaining in the aluminum cup after heating was weighed, and the solid content concentration of the polysiloxane solution or the acrylic resin solution was determined from the ratio to the weight before heating.

[0159] The weight average molecular weight of the polysiloxane and acrylic resin in Synthesis Examples 1 and 2 was determined by the following method: A GPC analysis was performed using a GPC analyzer (HLC-8220; manufactured by Tosoh Corporation) and tetrahydrofuran as a mobile phase in accordance with "JIS K7252-3 (established on March 20, 2008)" to measure the weight average molecular weight in terms of polystyrene.

[0160] The content ratio of each organosilane unit in the polysiloxane in Synthesis Example 1 was determined by the following method. The polysiloxane solution was injected into a "Teflon" (registered trademark) NMR sample tube having a diameter of 10 mm. 29In Si-NMR measurement, the content ratio of each organosilane unit was calculated from the ratio of the integrated value of Si derived from a specific organosilane unit to the integrated value of Si derived from the entire organosilane. 29 Si-NMR measurement conditions.

[0161] Apparatus: Nuclear magnetic resonance apparatus (JNM-GX270; manufactured by JEOL Ltd.)

[0162] Determination method: Gated decoupling method

[0163] Determined core frequency: 53.6693MHz( 29 Si core)

[0164] Spectral width: 20000Hz

[0165] Pulse width: 12μs (45° pulse)

[0166] Pulse repetition time: 30.0 seconds

[0167] Solvent: Acetone-d6

[0168] Reference substance: Tetramethylsilane

[0169] Measurement temperature: 23°C

[0170] Sample rotation speed: 0.0Hz.

[0171] Synthesis Example 1 Siloxane resin (c-1) solution

[0172] In a 500 ml three-necked flask, 59.15 g (0.400 mol) of propyltrimethoxysilane, 41.32 g (0.175 mol) of 3-trimethoxysilylpropylsuccinic anhydride, 36.60 g (0.175 mol) of 3-methacryloxypropylmethyldimethoxysilane, 11.09 g (0.05 mol) of 3-(3,4-epoxycyclohexyl)propyltrimethoxysilane, 24.52 g (0.200 mol) of methyltrimethoxysilane, 0.561 g of BHT, and 122.34 g of PGMEA were added, and an aqueous solution of phosphoric acid obtained by dissolving 1.727 g (1.0 wt % relative to the charged monomers) of phosphoric acid in 48.60 g of water was added over 30 minutes while stirring at room temperature.

[0173] Then, after the flask was immersed in an oil bath at 70°C and stirred for 90 minutes, the oil bath was heated to 115°C over 30 minutes. One hour after the start of heating, the solution temperature (internal temperature) reached 100°C, and heating and stirring were started there for 1 hour and 30 minutes (internal temperature was 100-110°C), and a siloxane resin solution was obtained. It should be noted that during the heating and heating and stirring, a mixed gas of 95% by volume of nitrogen and 5% by volume of oxygen was circulated at 0.05 liters / minute. A total of 110.70 g of methanol and water as by-products in the reaction were distilled out. PGMEA was added to the obtained siloxane resin solution in a manner such that the solid content concentration became 40% by weight, and a siloxane resin (c-1) solution was obtained. It should be noted that the weight average molecular weight of the obtained siloxane resin (c-1) was 3,700 (polystyrene conversion).

[0174] In addition, according to 29 As a result of Si-NMR measurement, the molar ratios of repeating units derived from propyltrimethoxysilane, 3-trimethoxysilylpropylsuccinic anhydride, 3-methacryloxypropylmethyldimethoxysilane, 3-(3,4-epoxycyclohexyl)propyltrimethoxysilane, and methyltrimethoxysilane in the siloxane resin (c-1) were 40 mol%, 17.5 mol%, 17.5 mol%, 5 mol%, and 20 mol%, respectively.

[0175] Synthesis Example 2 Acrylic Resin (d-1) Solution

[0176] In a 500 ml three-necked flask, 3 g of 2,2'-azobis(isobutyronitrile) and 50 g of PGMEA were added. Then, 30 g of methacrylic acid, 35 g of benzyl methacrylate, and tricyclo[5.2.1.0 2,6 ] 35g of decane-8-yl methacrylate was stirred at room temperature for a while, and after nitrogen substitution in the flask, heated and stirred at 70°C for 5 hours to obtain an acrylic resin solution. PGMEA was added to the obtained acrylic resin solution in a manner such that the solid content concentration became 40% by weight to obtain an acrylic resin (d-1) solution. The weight average molecular weight of the acrylic resin (d-1) was 10,000 (polystyrene conversion).

[0177] Synthesis Example 3: Carboxyl-containing acrylic copolymer having unsaturated double bonds (J)

[0178] 150 g of diethylene glycol monobutyl ether (hereinafter, "DGME") was added to a reaction container in a nitrogen atmosphere, and the temperature was raised to 80°C using an oil bath. A mixture consisting of 20 g of ethyl acrylate (hereinafter, "EA"), 40 g of 2-ethylhexyl methacrylate (hereinafter, "2-EHMA"), 20 g of n-butyl acrylate (hereinafter, "BA"), 15 g of N-hydroxymethyl acrylamide (hereinafter, "MAA"), 0.8 g of 2,2'-azobisisobutyronitrile and 10 g of DGME was added dropwise over 1 hour. After the addition was completed, the mixture was further heated at 80°C for 6 hours to carry out a polymerization reaction. Then, 1 g of hydroquinone monomethyl ether was added to stop the polymerization reaction. Next, a mixture consisting of 5 g of glycidyl methacrylate (hereinafter, "GMA"), 1 g of triethylbenzylammonium chloride and 10 g of DGME was added dropwise over 0.5 hours. After the addition was completed, the mixture was further heated for 2 hours to carry out an addition reaction. The obtained reaction solution was purified with methanol to remove unreacted impurities, and then vacuum dried for 24 hours to obtain an acrylic copolymer (J) having an unsaturated double bond and containing a carboxyl group, with a copolymerization ratio (based on mass): EA / 2-EHMA / BA / GMA / AA=20 / 40 / 20 / 5 / 15.

[0179] Preparation Example 1 Photosensitive resin composition (P-1)

[0180] 5.00 g of a siloxane resin (c-1) solution as the (C) resin was mixed with 5.00 g of a titanium dioxide pigment (R-960; manufactured by BASF Japan Co., Ltd.) as the (G-1) white pigment, and the mixture was dispersed using a mill-type disperser filled with zirconia beads to obtain a pigment dispersion (MW-1).

[0181] Next, 6.400 g of the pigment dispersion (MW-1), 3.425 g of the siloxane resin (c-1) solution, ethyl ketone as a photopolymerization initiator (D), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime) ("Ilgacura" (registered trademark) OXE-02 (trade name) manufactured by BASF Japan Co., Ltd. (hereinafter referred to as " OXE-02”)) 0.120 g, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (“ILGAQUA” (registered trademark)-819 (trade name), manufactured by BASF Japan Co., Ltd.) 0.240 g, (E) pentaerythritol acrylate (“LITE ACRYLATE” (registered trademark) PE-4A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.) ), 3.20 g of a 50 wt% PGMEA diluted solution, 0.160 g of 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate ("Cello Cycloside" (registered trademark)-2021P (trade name), manufactured by Daicel Co., Ltd.), 0.160 g of ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] ("Ilganox" (registered trademark) 0.024 g of DAA-1010 (trade name, manufactured by BASF Japan Co., Ltd.) and 0.060 g of a 10 wt% diluted solution of PGMEA (equivalent to a concentration of 300 ppm) of an acrylic surfactant (trade name "BYK"-352, manufactured by Bic Chemi Japan Co., Ltd.) were dissolved in a mixed solvent of 1.200 g of DAA and 5.171 g of PGMEA, and stirred. Then, the mixture was filtered with a 5.0 μm filter to obtain a photosensitive color resin composition (P-1).

[0182] Preparation Example 2 Photosensitive resin composition (P-2)

[0183] 5.00 g of a solution of a siloxane resin (c-1) as the (C) resin was mixed with 5.00 g of titanium nitride (produced by Wako Pure Chemical Industries, Ltd.; particle size: 50 nm, titanium content: 74.3 wt %, nitrogen content: 20.3 wt %, oxygen content: 2.94 wt %) as the (H) black pigment, and the mixture was dispersed using a mill-type disperser filled with zirconia beads to obtain a pigment dispersion (MW-2).

[0184] A photosensitive color resin composition (P-2) was obtained in the same manner as in Preparation Example 1 except that the amount of the siloxane resin (c-1) solution added was changed to 3.383 g, the PGMEA in the mixed solvent was changed to 5.189, and 0.24 g of the pigment dispersion (MW-2) was additionally added.

[0185] Preparation Example 3 Photosensitive Colored Resin Composition (P-3)

[0186] As the (I) organometallic compound, 2.00 g of bis(acetylacetonate)palladium was dissolved in 8.00 g of DAA to obtain an organometallic compound solution (OM-1).

[0187] A photosensitive colored resin composition (P-3) was obtained in the same manner as in Preparation Example 1 except that the amount of the siloxane resin (c-1) solution added was changed to 3.065 g, PGMEA in the mixed solvent was changed to 5.3870 g, DAA was changed to 0.624 g, and 0.720 g of the organometallic compound solution (OM-1) was added.

[0188] Preparation Example 4 Photosensitive Colored Resin Composition (P-4)

[0189] A photosensitive resin composition (P-4) was obtained in the same manner as in Preparation Example 1 except that the acrylic resin (d-1) solution was used instead of the siloxane resin (c-1) solution.

[0190] Preparation Example 5 Photosensitive Colored Resin Composition (P-5)

[0191] The amount of the pigment dispersion (MW-1) was changed to 7.520 g, and the amount of ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetoxime) ("Ilugacur" (registered trademark) OXE-02 (trade name) manufactured by BASF Japan Co., Ltd. (hereinafter "OXE-02")) was changed to 0.14 1 g, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide ("ILGAQUA" (registered trademark)-819 (trade name), manufactured by BASF Japan Co., Ltd.) 0.282 g, 50 wt% PG of pentaerythritol acrylate ("LITE ACCRYLATE" (registered trademark) PE-4A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.) 3.78 g of MEA diluted solution, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate ("Cellocid" (registered trademark)-2021P (trade name), manufactured by Daicel Co., Ltd.) 0.188 g, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] ("Ilganox" (registered trademark)-1010 (trade name), manufactured by BASF Japan Co., Ltd.) 0.028 g, DAA 1.060 g and PGMEA 2.934 g, except that the addition amount of the siloxane resin (c-1) solution was changed to 4.027 g, the same procedure as in Preparation Example 1 was carried out to obtain a photosensitive color resin composition (P-5).

[0192] Preparation Example 6 Photosensitive Colored Resin Composition (P-6)

[0193] The amount of the pigment dispersion (MW-1) was changed to 8.800 g, and the amount of ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetoxime) ("Ilgacura" (registered trademark) OXE-02 (trade name) manufactured by BASF Japan Co., Ltd. (hereinafter "OXE-02")) was changed to 0.16 5 g, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide ("ILGAQUA" (registered trademark)-819 (trade name), manufactured by BASF Japan Co., Ltd.) 0.330 g, 50 wt% PG of pentaerythritol acrylate ("LITE ACCRYLATE" (registered trademark) PE-4A (trade name), manufactured by Kyoeisha Chemical Co., Ltd.) 4.400 g of MEA diluted solution, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate ("Cellocid" (registered trademark)-2021P (trade name), manufactured by Daicel Co., Ltd.) 0.220 g, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] ("Ilganox" (registered trademark)-1010 (trade name), manufactured by BASF Japan Co., Ltd.) 0.033 g, DAA 0.900 g and PGMEA 0.377 g, except that the addition amount of the siloxane resin (c-1) solution was changed to 4.715 g, the same procedure as in Preparation Example 1 was carried out to obtain a photosensitive color resin composition (P-6).

[0194] Preparation Example 7 Photosensitive Colored Resin Composition (P-7)

[0195] A photosensitive color resin composition (P-7) was obtained in the same manner as in Preparation Example 1 except that the pigment dispersion (MW-1) was not added and the addition amount of PGMEA was changed to 0.371 g and the addition amount of the siloxane resin (c-1) solution was changed to 14.625 g.

[0196] Table 1 shows the compositions of Preparation Examples 1 to 7 in summary.

[0197] [Table 1]

[0198]

[0199] Preparation Example 8 Conductive Paste

[0200] In a 100 ml clean bottle, 15.00 g of an acrylic copolymer (J) containing carboxyl groups and having unsaturated double bonds, 0.66 g of (“IRGACURE (registered trademark)” OXE04 (trade name), manufactured by BASF Japan Ltd.) as a photoinitiator, 1.5 g of (“Light Acrylate (registered trademark)” BP-4EA (trade name), manufactured by Kyoeisha Chemical Co., Ltd.) as a compound having unsaturated double bonds, 3.82 g of (“EPICLON (registered trademark)” 840 (trade name), manufactured by DIC Corporation) as an epoxy resin, 2.17 g of H-4 ((trade name), manufactured by Meiwafosis Co., Ltd.) as a novolak phenolic resin, and 5.78 g of DGME were mixed using a rotation-revolution vacuum mixer “Awatori Rentaro (registered trademark)” ARE-310 (manufactured by Shinki Co., Ltd.) to obtain 28.94 g of a resin solution.

[0201] The obtained 28.94 g of the resin solution was mixed with 54.02 g of Ag particles having a particle size (D50) of 0.5 μm and an aspect ratio of 1.1, and kneaded using a three-roll mill (EXAKT M-50; manufactured by EXAKT) to obtain 82.96 g of a conductive paste.

[0202] <Bump-Forming Substrate (K-1)>

[0203] The obtained conductive paste was coated on a glass substrate having electrodes with a substrate thickness of 0.7 mm and heated in a drying oven at 100 °C for 5 minutes.

[0204] Using a direct drawing exposure apparatus (MX-1201; manufactured by Dainippon Kagaku Kenkyusho Co., Ltd.), considering the line thickening amount in the exposure part, at an exposure amount of 300 mJ / cm 2 (converted to a wavelength of 375 nm), 200 bumps with a film thickness of 5 μm and a size of φ10 μm were exposed in such a way that the distance between adjacent bumps was 10 μm.

[0205] After exposure, development was carried out by spraying a 0.1 wt% aqueous Na2CO3 solution for 20 seconds and rinsing with ultrapure water to produce a bump-forming substrate (K-1).

[0206] <Bump-Forming Substrate (K-2)>

[0207] Indium plating was performed on a circuit substrate with electrodes having a substrate thickness of 0.7 mm to obtain a bump-forming substrate (K-2) having indium bumps with a thickness of 0.5 μm formed on the substrate electrodes.

[0208] <Bump-Forming Substrate (K-3)>

[0209] A bump-formed substrate (K-3) was produced by the same method as that of the bump-formed substrate (K-1), except that the film thickness of the bumps was changed to 2.5 μm.

[0210] <Bump formation substrate (K-4)>

[0211] A bump-formed substrate (K-4) was produced by the same method as that of the bump-formed substrate (K-1), except that the film thickness of the bumps was changed to 1.0 μm.

[0212] <LED mounting substrate (L-1)>

[0213] like Fig. 9 As shown in (a), a release layer 12 with a thickness of 5 μm and containing polyimide as the main component is prepared on a transparent substrate 11, and an LED transfer substrate 14 is prepared in which the surface of the LED light-emitting portion 13 in the LED element 5 that does not have the LED electrode 4 is retained by the adhesiveness of the release layer 12.

[0214] Next, if Fig. 9 As shown in (b), the bump formation substrate 15 is subjected to 200 mJ / cm 2 The LED element 5 is irradiated with a 266 nm laser beam 16 from the transparent substrate 11 side of the LED transfer substrate 14 to transfer the LED chip 14 to the LED mounting substrate. Fig. 9 As shown in (c), heat pressing is performed using a separator laminator at 1 MPa, 120°C, and 60 seconds. Fig. 9 The LED mounting substrate (L-1) 17 was manufactured as shown in (d). In addition, the cross-sectional shape of the LED was observed using a focused ion beam device (FIB) and a scanning electron microscope (SEM) for the manufactured LED mounting substrate (L-1), and the distance S between the bottom surface of the LED and the substrate having the wiring electrodes was measured. H .exist Fig. 9 In the case of a substrate formed by mounting LEDs as shown in FIG. 1 , the distance between the bottom surface of the LED and the substrate having wiring electrodes is represented by the symbol S H The distance S between the bottom surface of the LED and the substrate having the wiring electrodes in the LED mounting substrate (L-1) is shown. H , is 6.5μm.

[0215] <LED mounting substrate (L-2)>

[0216] By the same method as the LED mounting substrate (L-1), the bump forming substrate (K-1) is replaced with the bump forming substrate (K-2), and the LED mounting substrate (L-2) is manufactured. Regarding the manufactured LED mounting substrate (L-2), the distance S between the bottom surface of the LED and the substrate having the wiring electrodes isH 0.5μm.

[0217] <LED mounting substrate (L-3)>

[0218] By the same method as the LED mounting substrate (L-1), the bump forming substrate (K-1) is replaced with the bump forming substrate (K-3), and the LED mounting substrate (L-3) is manufactured. Regarding the manufactured LED mounting substrate (L-3), the distance S between the bottom surface of the LED and the substrate having the wiring electrodes is H is 2.5μm.

[0219] <LED mounting substrate (L-4)>

[0220] By the same method as the LED mounting substrate (L-1), the bump forming substrate (K-1) is replaced with the bump forming substrate (K-4), and the LED mounting substrate (L-4) is manufactured. Regarding the manufactured LED mounting substrate (L-4), the distance S between the bottom surface of the LED and the substrate having the wiring electrodes is H is 1.0μm.

[0221] The evaluation methods in each of Examples and Comparative Examples are shown below.

[0222] <Evaluation of installability>

[0223] Regarding the LED mounting substrates used in the examples and comparative examples, voltage was applied to 100 mounted LEDs, the number of LEDs that lit up was counted, and the number was used as the mountability evaluation result.

[0224] <Connection reliability evaluation (continuous lighting test)>

[0225] A voltage was applied to the LED mounting substrates with cured films obtained in the examples and comparative examples to count the number of LEDs that lit up. The lighting state was then continued for 3 hours, and the LED lighting rate was calculated using the following formula to evaluate the connection reliability.

[0226] Connection reliability evaluation=number of LED lighting after the test / number of LED lighting before the test×100.

[0227] <Reflectivity>

[0228] The photosensitive colored resin composition used in each example and comparative example was processed in the same manner except that the film thickness was changed among the conditions processed in each example and comparative example, and a 10 μm cured film was prepared on a flat glass substrate. The obtained cured film was used as a model of the cured film of the substrate with a cured film formed on the LED mounting substrate formed in each example and comparative example, and the reflectance at a wavelength of 550 nm was measured from the cured film side in SCI mode using a spectrophotometer (trade name CM-2600d, manufactured by Conika Minolta Co., Ltd.).

[0229] <Absorbance (OD value)>

[0230] The photosensitive resin composition used in each example and comparative example was processed in the same manner except that the film thickness was changed among the conditions processed in each example and comparative example, and a 10 μm cured film was produced on a flat glass substrate. The obtained cured film was used as a model of the cured film of the substrate with a cured film formed on the substrate having a concavo-convex structure formed in each example and comparative example, and the intensity of the incident light and the transmitted light was measured from above using a densitometer (U-4100 manufactured by Hitachi HiTech Science) and the absorbance (OD value) was calculated by the following formula (III).

[0231] OD value = log10 (I0 / I) formula (III)

[0232] I0: incident light intensity

[0233] I: Transmitted light intensity.

[0234] (Example 1)

[0235] The photosensitive colored resin composition of Example 1 was spin-coated (trade name 1H-360S, manufactured by Mikasa Co., Ltd.) on the LED mounting substrate (L-1), and a coating film was formed using a hot plate (trade name SCW-636, manufactured by Dainippon Screen Manufacturing Co., Ltd.). Then, it was dried at a temperature of 100°C for 2 minutes to form a dry film. As an exposure machine for the process of exposing the substrate with the dry film, a parallel light mask exposure machine (trade name PLA-501F, manufactured by Canon Co., Ltd.) was used, and an exposure machine using an ultra-high pressure mercury lamp as a light source was used. Regarding the mask pattern, a mask pattern designed so that the gap between the mounted LED element and the developed coating film is 5μm was used. The platform was moved to a specified position using an alignment camera, and an exposure amount of 200mJ / cm 2(i-ray) was exposed at a gap of 100 μm. Then, an automatic developing device ("AD-2000 (trade name)" manufactured by Takizawa Industry Co., Ltd.) was used to perform shower development for 100 seconds using a 0.045 wt% potassium hydroxide aqueous solution, followed by rinsing with water for 30 seconds. Then, an oven (trade name IHPS-222, manufactured by Espec Co., Ltd.) was used to heat at a temperature of 170°C in air for 30 minutes to produce an LED mounting substrate with a cured film having a film thickness of 10 μm on the LED mounting substrate.

[0236] (Example 2)

[0237] The processing was carried out in the same manner as in Example 1 except that the LED mounting substrate (L-2) was used instead of the LED mounting substrate (L-1).

[0238] (Example 3)

[0239] Processing was carried out in the same manner as in Example 1 except that P-2 was used as the photosensitive resin composition and the exposure amount before development was 80 mJ.

[0240] (Example 4)

[0241] Processing was carried out in the same manner as in Example 1 except that P-3 was used as the photosensitive resin composition and the exposure amount before development was 100 mJ.

[0242] (Example 5)

[0243] Processing was carried out in the same manner as in Example 1 except that P-4 was used as the photosensitive resin composition and the exposure amount before development was 40 mJ.

[0244] (Example 6)

[0245] Processing was carried out in the same manner as in Example 1 except that P-5 was used as the photosensitive resin composition.

[0246] (Example 7)

[0247] Processing was carried out in the same manner as in Example 1 except that P-6 was used as the photosensitive resin composition.

[0248] (Example 8)

[0249] Processing was carried out in the same manner as in Example 1 except that P-7 was used as the photosensitive resin composition.

[0250] (Example 9)

[0251] The processing was carried out in the same manner as in Example 1 except that the LED mounting substrate (L-3) was used instead of the LED mounting substrate (L-1).

[0252] (Example 10)

[0253] The processing was carried out in the same manner as in Example 1 except that the LED mounting substrate (L-3) was used instead of the LED mounting substrate (L-1).

[0254] (Comparative Example 1)

[0255] The LED mounting substrate (L-1) was processed in the same manner as in Example 1 except that the photosensitive coloring resin composition P-1 was not applied.

[0256] [Table 2]

[0257]

[0258] Explanation of symbols

[0259] 1: Substrate

[0260] 2: Wiring electrode

[0261] 3: LED electrode

[0262] 4: Bump

[0263] 5: LED components

[0264] 6: Coating film of photosensitive coloring resin composition

[0265] 7: Dry film of photosensitive coloring resin composition

[0266] 8: Coating film of photosensitive colored resin composition after exposure

[0267] 9: Coating film after development of photosensitive resin composition

[0268] 10: Cured film of photosensitive resin composition

[0269] 11: Transparent substrate

[0270] 12: Release layer

[0271] 13: LED light emitting part

[0272] 14: LED transfer substrate

[0273] 15: LED mounting substrate

[0274] 16: Laser

[0275] 17: LED mounting substrate.

Claims

1. A method for manufacturing an LED mounting substrate with a cured film, wherein: The following processing steps (1) to (5) are sequentially performed on an LED mounting substrate including a substrate having wiring electrodes, bumps formed on the wiring electrodes, and a plurality of LED elements mounted on the bumps. (1) a step of applying a photosensitive resin composition to the LED mounting substrate to fill the gap between the LED element and the substrate having wiring electrodes and the space between adjacent LED elements with the coating film, (2) a step of drying the coating film to obtain a dried film, (3) a step of exposing the dried film to light, (4) a step of removing unnecessary portions of the exposed dried film by development, (5) A step of converting the film from which unnecessary portions have been removed after development into a cured film.

2. The method for manufacturing an LED mounting substrate with a cured film according to claim 1, wherein: In the step (4) of removing unnecessary portions of the exposed dried film by development, the developed film is left at least around the bumps and wiring electrodes. 3 . The method for producing a LED mounting substrate with a cured film according to claim 1 , wherein the bumps formed on the wiring electrodes contain (A) an organic component and (B) conductive particles.

4. The method for manufacturing an LED mounting substrate with a cured film according to claim 1 or 2, wherein the (A) organic component of the bump comprises an acrylic copolymer having a carboxyl group and an epoxy resin, and the proportion of the (B) conductive particles in the total weight of the bump is 50 to 90 wt%.

5. The method for producing an LED mounting substrate with a cured film according to claim 1 or 2, wherein the bumps are obtained by exposing and developing a conductive paste containing (A) an organic component and (B) conductive particles to form a pattern. 6 . The method for producing an LED mounting substrate with a cured film according to claim 1 , wherein the photosensitive resin composition contains (C) a resin, (D) a photopolymerization initiator, (E) a photopolymerizable compound, (F) an organic solvent, and (G) a coloring pigment.

7. The method for manufacturing an LED mounting substrate with a cured film according to claim 6, wherein: The (G) coloring pigment includes at least (G-1) a white pigment.

8. The method for manufacturing an LED mounting substrate with a cured film according to claim 6, wherein: The (C) resin is (C-1) a siloxane resin.

9. An LED mounting substrate with a cured film, produced by the method according to claim 6. 10 . A device comprising the LED mounting substrate with a cured film according to claim 9 .

11. An LED mounting substrate comprising a substrate having an electrode, a bump formed of a composite material of an organic component and conductive particles formed on the electrode, and a plurality of LED elements mounted on the bump, characterized in that: At least a part of the periphery of the bump and the LED element is covered with a cured film of the photosensitive coloring resin composition, and the cured film of the photosensitive resin composition is also present between adjacent LD elements.

Citation Information

Patent Citations

  • Therapeutic selenium compositions and the use thereof

    EP0000670A1

  • 1-Methylisoguanosin, processes and intermediates for its preparation, its pharmaceutical compositions and their preparation

    EP0000770A2

  • Water vapour absorbent and permeant flat rubber product and a method for its manufacture

    EP0000775A1

  • Light-emitting device and method of manufacturing the same

    JP2017112295A

  • Light-emitting device

    JP2018082197A