Drug-loadable sodium alginate microspheres and preparation method thereof
Microspheres were prepared by physical cross-linking of sodium alginate and carboxymethyl chitosan, combined with cellulose butyrate acetate and n-butyl acetate, which solved the shortage of drug-loading microspheres in tumor interventional treatment. The problem of this problem is to realize high-efficiency drug loading and simplify the production process, and reduce the sudden release of the drug release rate.
Patent Information
- Application Number
- CN202411011547.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-05
AI Technical Summary
Existing drug-loading microspheres are difficult to quickly load drugs in tumor interventional treatment and have insufficient mechanical properties. The preparation method is complex and difficult to produce on a large scale. The drug release rate is slow and the storage conditions are harsh, which affects the treatment effect and production efficiency.
The physical cross-linking effect of sodium alginate and carboxymethyl chitosan was used to prepare microspheres, combined with cellulose butyrate acetate, n-butyl acetate and acetic acid as oily solvents and pH regulators, and a homogenized gel microspheres were formed by stirring reaction. The ball avoids the use of chemical crosslinking agents and improves the drug-carrying performance and compression performance.
Achieve rapid drug loading (5min drug loading rate can reach 70%), improve sphere-forming performance and compression performance, the material can be degraded in the body, avoid crosslinking agent residue problems, simplify the production process, and reduce the drug release rate a sudden analysis.
Smart Images

Figure CN118892458A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedicine technology, in particular to the field of IPCA61L24, and more specifically to a drug-carrying sodium alginate microsphere and a preparation method thereof. Background Art
[0002] In recent years, with the development of minimally invasive interventional technology, tumor interventional therapy has penetrated into the field of tumor treatment and has become one of the important methods of cancer treatment, especially in the treatment of blood-rich tumors such as liver cancer, kidney cancer and uterine fibroids. At present, the embolic microspheres that are widely used for interventional embolization therapy mainly include: polylactic acid microspheres, sodium alginate microspheres, chitosan microspheres, gelatin sponge microspheres, polyvinyl alcohol microspheres, etc. The drug-loaded embolic microspheres can not only block the blood supply of tumors, but also continuously release anticancer drugs to the tumor target area at the tumor site, achieving a "two-pronged" treatment effect. In addition, at the same dosage, the increase in the drug loading of the drug-loaded embolic microspheres can greatly reduce the amount of excipients and reduce the side effects of the excipients and their degradation products. How to achieve rapid drug loading while improving the mechanical properties of microspheres and having safety is an urgent problem to be solved in the industry.
[0003] CN106821993A introduces a type of gel polymer cross-linked by groups containing disulfide bonds, in which the groups with anionic charge are electrostatically associated with the drug for embolization therapy. The total amount of doxorubicin released is 8% at about 6 hours, the burst release phenomenon is still obvious, and there is a lack of long-term experimental data, and the sustained release effect is not good. CN111773428A discloses a drug sustained-release alginate embolic microsphere, which is prepared by pre-compounding the raw material sodium alginate and the positively charged chemotherapy drug, and then using electrostatic spray technology to prepare the drug-loaded alginate embolic microsphere. The data show that the drug release rate of the microsphere is slow, but the preparation method requires pre-loading of the drug, so the storage conditions of the finished microsphere are relatively harsh to prevent the drug from deteriorating; in addition, the preparation method is relatively complicated and not easy to mass produce. Summary of the invention
[0004] The first aspect of the present invention provides a drug-carrying sodium alginate microsphere, the components of which include: sodium alginate, carboxymethyl chitosan, a pH regulator, an oil-soluble stabilizer, an oily solvent and water.
[0005] The oil-soluble stabilizer includes at least one of cellulose acetate butyrate, cellulose acetate, Span and Tween.
[0006] The molecular weight of the sodium alginate is 1k-1000kDa.
[0007] The carboxymethyl chitosan has a carboxymethyl degree of 50%-99% and a molecular weight of 1k-1000kDa.
[0008] The oily solvent includes at least one of n-butyl acetate, ethyl acetate, methyl acetate and propyl acetate.
[0009] The pH adjuster includes at least one of acetic acid, hydrochloric acid, sulfuric acid, nitric acid, boric acid, aluminic acid, perchloric acid, and hypochlorous acid.
[0010] The mass ratio of the sodium alginate to the carboxymethyl chitosan is 1:(0.5-3).
[0011] Preferably, the mass ratio of sodium alginate to carboxymethyl chitosan is 1:(0.5-1.5).
[0012] The second aspect of the present invention provides a method for preparing drug-loaded sodium alginate microspheres, comprising the following steps:
[0013] Step 1: dissolving sodium alginate in water to obtain a sodium alginate aqueous solution;
[0014] Step 2: dissolving carboxymethyl chitosan in water to obtain a carboxymethyl chitosan aqueous solution;
[0015] Step 3: Mixing an oil-soluble stabilizer with an oily solvent to prepare an oil phase;
[0016] Step 4: Evenly mix the sodium alginate aqueous solution and the carboxymethyl chitosan aqueous solution to obtain an aqueous phase, disperse the aqueous phase in the oil phase, add a pH adjuster, adjust the pH to 3-6, stir the reaction, and then post-treat to obtain microspheres.
[0017] The concentration of sodium alginate in the sodium alginate aqueous solution is 1-10 wt %.
[0018] The concentration of carboxymethyl chitosan in the carboxymethyl chitosan aqueous solution is 1-10 wt %.
[0019] Preferably, the concentration of sodium alginate in the sodium alginate aqueous solution is 5-8wt%, and the concentration of carboxymethyl chitosan in the carboxymethyl chitosan aqueous solution is 5-8wt%.
[0020] The concentration of the oil-soluble stabilizer in the oil phase is 3-10 wt %.
[0021] Preferably, the concentration of the oil-soluble stabilizer in the oil phase is 3-7 wt %.
[0022] Further preferably, the concentration of the oil-soluble stabilizer in the oil phase is 4-7 wt %.
[0023] The volume ratio of the water phase to the oil phase is 1:(5-10).
[0024] Preferably, the volume ratio of the water phase to the oil phase is 1:(7-10).
[0025] The stirring speed in step 4 is 100-300 rpm.
[0026] Preferably, the stirring speed in step 4 is 150-250 rpm.
[0027] The particle size of the microspheres is 40-1000 microns.
[0028] The applicant has found that the concentration of sodium alginate in the sodium alginate aqueous solution is 5-8wt%, the concentration of carboxymethyl chitosan in the carboxymethyl chitosan aqueous solution is 5-8wt%, and the mass ratio of sodium alginate to carboxymethyl chitosan is 1: (0.5-3), which can improve the ball-forming performance, drug-loading performance and compression performance after ball-forming. The existing sodium alginate microsphere products are usually calcium ions coordinated with carboxyl groups, consuming carboxyl groups, resulting in no drug-loading performance or poor drug-loading performance. This patent forms balls through the physical cross-linking of sodium alginate and carboxymethyl chitosan, retaining sufficient active groups, so that it has excellent drug-loading performance. At the same time, in the prior art, chitosan can only be dissolved under acidic conditions, while sodium alginate and acidic chitosan are prone to rapid entanglement of molecular chains in the acidic environment when mixed, and it is not easy to form a homogeneous polyelectrolyte gel, and it is not conducive to dispersion into the oil phase, and it is difficult to form balls. At the same time, carboxymethyl chitosan is soluble in a neutral environment and can be fully mixed with sodium alginate. Then, the oil phase is added and it is easily dispersed into balls to form a homogeneous gel, achieving excellent compression performance.
[0029] Beneficial Effects
[0030] 1. The present application forms spheres through physical cross-linking of sodium alginate and carboxymethyl chitosan without introducing additional chemical cross-linking agents, thus avoiding the subsequent processing costs caused by the problem of cross-linking agent residues.
[0031] 2. The present invention adopts carboxymethyl chitosan to physically cross-link sodium alginate, and the material is degradable in the body, and the patient can receive secondary treatment if necessary.
[0032] 3. The microspheres prepared in this application can be quickly loaded with drugs, and the drug loading rate can reach 70% in 5 minutes.
[0033] 4. The concentration of sodium alginate in the sodium alginate aqueous solution is 5-8wt%, the concentration of carboxymethyl chitosan in the carboxymethyl chitosan aqueous solution is 5-8wt%, and the mass ratio of sodium alginate to carboxymethyl chitosan is 1:
[0034] (0.5-3), which can improve the ball-forming performance, drug loading performance and compression performance after ball-forming.
[0035] 5. The volume ratio of the water phase to the oil phase is 1:(5-10), and the stirring speed is limited to 150-250 rpm, and the particle size is maintained at 100-1000 microns. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a picture of the microsphere microscope at 100 times magnification in Example 1.
[0037] Figure 2 This is the state of the microspheres before compression in Example 1.
[0038] Figure 3 This is the state of the microspheres being compressed in Example 1.
[0039] Figure 4 This is the state of the microspheres after compression in Example 1.
[0040] Figure 5 This is an electronic photograph of the microspheres after drug loading in Example 1.
[0041] Figure 6 The left picture in Example 1 is a picture of the microspheres loaded with DOX for 10 min under an inverted microscope magnified 40 times, and the right picture is a picture of the microspheres loaded with DOX for 10 min under an inverted microscope magnified 100 times.
[0042] Figure 7 This is the drug loading rate curve of the microspheres in Example 1.
[0043] Figure 8 This is a picture of the microsphere microscope in comparative example 1 at 100 times magnification.
[0044] Fig. 9 This is a picture of the microsphere microscope in comparative example 2 at 100 times magnification. DETAILED DESCRIPTION
[0045] Example 1
[0046] The invention discloses a drug-carrying sodium alginate microsphere, which comprises sodium alginate, carboxymethyl chitosan, a pH regulator, an oil-soluble stabilizer, an oily solvent and water.
[0047] The oil-soluble stabilizer is cellulose acetate butyrate; the oily solvent is n-butyl acetate; and the pH adjuster is acetic acid.
[0048] The mass ratio of the sodium alginate to the carboxymethyl chitosan is 1:1.
[0049] A method for preparing drug-carrying sodium alginate microspheres comprises the following steps:
[0050] Step 1: Add 6 g of sodium alginate to 94 g of water to obtain a sodium alginate aqueous solution;
[0051] Step 2: adding 6 g of carboxymethyl chitosan to 94 g of water to obtain a carboxymethyl chitosan aqueous solution;
[0052] Step 3: Mixing an oil-soluble stabilizer with an oily solvent to prepare an oil phase;
[0053] Step 4: Take 10 mL of sodium alginate aqueous solution and 10 mL of carboxymethyl chitosan aqueous solution and mix them evenly to obtain an aqueous phase, disperse it in 200 mL of n-butyl acetate oil phase containing 5.6 wt% cellulose acetate butyrate, add 2 g of acetic acid, stir at 200 rpm for 12 h, let it stand for stratification, pour off the upper layer, collect the product, wash the product with n-butyl acetate, anhydrous ethanol and saline, sieve it, and store the microspheres in a saline solution.
[0054] The particle size of the microspheres is 50-900 microns.
[0055] Comparative Example 1
[0056] A method for preparing drug-carrying sodium alginate microspheres comprises the following steps:
[0057] 1. Prepare a 1% wt sodium alginate aqueous solution: add 1 g of sodium alginate into 99 g of purified water, stir and dissolve evenly to obtain a sodium alginate aqueous solution, recorded as solution A.
[0058] 2. Prepare a 1% carboxymethyl chitosan aqueous solution: add 1 g of carboxymethyl chitosan into 99 g of purified water, stir and dissolve evenly to obtain a carboxymethyl chitosan solution, recorded as solution B.
[0059] 3. Take 10 mL of solution A and 10 mL of solution B, mix and stir evenly, disperse into 180 mL of n-butyl acetate solution containing 5.6% cellulose acetate butyrate, stir for 30 min, add 1 mL of acetic acid and continue the reaction for 3 h.
[0060] 4. Let it stand overnight, pour off the upper liquid, wash the product with n-butyl acetate, anhydrous ethanol and saline, sieve, and store the microspheres in saline solution.
[0061] Comparative Example 2
[0062] A method for preparing drug-carrying sodium alginate microspheres comprises the following steps:
[0063] 1. Step 1: Add 6 g of sodium alginate to 94 g of water to obtain a sodium alginate aqueous solution;
[0064] Step 2: adding 6 g of carboxymethyl chitosan to 94 g of water to obtain a carboxymethyl chitosan aqueous solution;
[0065] Step 3: Mixing an oil-soluble stabilizer with an oily solvent to prepare an oil phase;
[0066] Step 4: Take 10 mL of sodium alginate aqueous solution and 10 mL of carboxymethyl chitosan aqueous solution and mix them evenly to obtain an aqueous phase, disperse it in 200 mL of n-butyl acetate oil phase containing 5.6 wt% cellulose acetate butyrate, add 2 g of acetic acid, stir at 300 rpm for 12 h, let it stand for stratification, pour off the upper layer, collect the product, wash and sieve it to obtain microspheres.
[0067] The particle size of the microspheres is 50-200 microns.
[0068] Performance Testing Methods and Data
[0069] 1. Microsphere morphology. Method: Store the microspheres in physiological saline solution, take 500 μL of microsphere solution and add it to a 24-well plate, and observe the morphology under an inverted microscope. Figure 1 As shown, relatively uniform microspheres were formed. Figure 8 Microspheres are not formed.
[0070] 2. Compressibility: Method: Use the microspheres of the texture analyzer to perform compression test. Take the microspheres out of the storage liquid, gently absorb the liquid on the surface of the microspheres, and perform compression test within 3 minutes. The compression speed is 0.2 mm / s, the microspheres are deformed by 50%, and the pause time is 10 seconds. Observe whether the microspheres are broken. The shape of the microspheres is as follows: Figure 2-4 As shown, the microspheres were not broken.
[0071] 3. Drug loading performance: Method: Take 0.5mL of microspheres and add them into 0.5mL of 25mg / mL doxorubicin solution. Shake gently every 5min. Observe the state of microspheres after 10min. Figure 5 and Figure 6 shown.
[0072] 4. Drug loading rate: Method: Take 0.5mL of microspheres and add them to 0.5mL of 25mg / mL doxorubicin solution. Shake gently every 5min. Test the doxorubicin concentration in the mixed liquid at different time points. Calculate the drug loading rate according to the following formula. The results are as follows: Figure 7 As shown, the drug loading rate reached 70% in 5 min and exceeded 90% in 10 min.
[0073] Drug loading rate = initial doxorubicin concentration (mg / mL) / final doxorubicin concentration (mg / mL) x 100%.
Claims
1. A drug-carrying sodium alginate microsphere, It is characterized in that Components include: Sodium alginate, carboxymethyl chitosan, pH regulator, oil-soluble stabilizer, oily solvent and water.
2. The drug-loaded sodium alginate microspheres according to claim 1, It is characterized in that The oil-soluble stabilizer includes at least one of cellulose acetate butyrate, cellulose acetate, Span and Tween.
3. The drug-loaded sodium alginate microspheres according to claim 2, It is characterized in that The oily solvent includes at least one of n-butyl acetate, ethyl acetate, methyl acetate and propyl acetate.
4. The drug-loaded sodium alginate microspheres according to claim 3, It is characterized in that The pH adjuster includes at least one of acetic acid, hydrochloric acid, sulfuric acid, nitric acid, boric acid, aluminic acid, perchloric acid, and hypochlorous acid.
5. The drug-loaded sodium alginate microspheres according to claim 4, It is characterized in that The mass ratio of the sodium alginate to the carboxymethyl chitosan is 1:(0.5-3).
6. A method for preparing drug-loaded sodium alginate microspheres according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step 1: dissolving sodium alginate in water to obtain a sodium alginate aqueous solution; Step 2: dissolving carboxymethyl chitosan in water to obtain a carboxymethyl chitosan aqueous solution; Step 3: Mixing an oil-soluble stabilizer with an oily solvent to prepare an oil phase; Step 4: Evenly mix the sodium alginate aqueous solution and the carboxymethyl chitosan aqueous solution to obtain an aqueous phase, disperse the aqueous phase in the oil phase, add a pH adjuster, adjust the pH to 3-6, stir the reaction, and then post-treat to obtain microspheres.
7. The method for preparing drug-loaded sodium alginate microspheres according to claim 6, It is characterized in that The concentration of the oil-soluble stabilizer in the oil phase is 3-10 wt %.
8. The method for preparing drug-loaded sodium alginate microspheres according to claim 7, It is characterized in that The volume ratio of the water phase to the oil phase is 1:(5-10).
9. The method for preparing drug-loaded sodium alginate microspheres according to claim 6, It is characterized in that The stirring speed in step 4 is 100-300 rpm.
10. The method for preparing drug-loaded sodium alginate microspheres according to claim 6, It is characterized in that The concentration of sodium alginate in the sodium alginate aqueous solution is 1-10 wt %, and the concentration of carboxymethyl chitosan in the carboxymethyl chitosan aqueous solution is 1-10 wt %.
Citation Information
Cited By
Non-woven material with high water absorbability for facial mask and preparation method of non-woven material
CN119221203A