Preparation device and preparation method of steel slag maintenance material for road
By designing a steel slag curing material preparation device, using electromagnetic heating and crushing technology to determine the optimal particle size and perform alkalization modification, the problem of steel slag expansion and electromagnetic heating in road maintenance is solved, and the material is realized The composition and volume stability and electromagnetic heating effect are improved.
Patent Information
- Application Number
- CN202410900870.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-05
AI Technical Summary
Steel slag expands when encountering water during road maintenance and unstable volume. The traditional treatment methods have problems such as long time, poor quality and poor electromagnetic heating effect, which limits its application in the field of road maintenance.
A preparation device for road steel slag curing materials is designed, including a cracking reactor and an alkalization reactor. Through electromagnetic heating and crushing technology, the optimal electromagnetic response particle size is determined, and alkalizing modification is carried out to generate waterproofing. Silicate ensures stability of material composition and volume.
The dual stability of the composition and volume of steel slag material is achieved, the waterproof performance is enhanced, the electromagnetic heating and maintenance effect of the road surface is improved, the service life of the road is extended, and the shortcomings of the traditional methods are overcome.
Smart Images

Figure CN118892783A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steel slag road maintenance materials, and in particular relates to a preparation device and a preparation method of steel slag road maintenance materials. Background Art
[0002] Steel slag is a major by-product of the steel industry, accounting for about 10% to 15% of steel production. Due to the lack of proper utilization technology for steel slag, the current mainstream method of steel slag disposal is still dumping and abandonment, which not only occupies a large area of land, but also pollutes the soil and water quality. In order to utilize waste steel slag, some scholars have proposed to use the characteristics of steel slag that have a good response effect to microwave and electromagnetic induction heating, and use steel slag to replace mineral aggregates in asphalt mixtures to build roads. This can enhance the electromagnetic heating maintenance performance of the road surface, that is, use microwaves or electromagnetic induction to heat the road surface to achieve road maintenance functions such as ice and snow melting and asphalt self-repair and self-healing.
[0003] However, the free calcium oxide contained in steel slag expands when it comes into contact with water, causing the volume of the steel slag material to be unstable. It will break or even pulverize during long-term use of the road, which will affect the structural stability of the road and cause various road diseases. To solve this problem, the traditional method is to pile up the steel slag in an open-air environment and naturally age it for 2-3 years, and then use it for road construction after its composition stabilizes. However, naturally aging steel slag not only takes a long time, but also has problems such as pulverization and embrittlement after long-term storage, and the quality is poor. In addition, the steel slag under natural aging conditions still contains a small amount of free calcium oxide and other components. No matter how long it is aged, there is still a risk of expansion and pulverization when used to replace road aggregates.
[0004] In addition, due to the porous structure and complex composition of steel slag, the electromagnetic heating response of steel slag of different particle sizes in the same batch is very different. The traditional method of replacing steel slag for road use is blind and random. Most of them are to replace the aggregate in full grade according to the volume fraction replacement method, or simply replace the aggregate in the whole grade according to the particle size with the majority of steel slag in the batch, without considering the use of steel slag particle size with the best electromagnetic response to replace the corresponding several grades of aggregate and avoid the steel slag particle size with poor electromagnetic heating effect. As a result, the prepared road surface has poor electromagnetic heating effect and no significant maintenance effect, which greatly wastes the potential of steel slag as a road maintenance material.
[0005] In addition, existing steel slag crushing devices usually use traditional jaw crushers or roller crushers, which cannot achieve quantitative and standardized crushing after considering the road maintenance effect, and cannot control the crushing position to be exactly where free calcium oxide exists. At the same time, there is also a lack of process for modifying the steel slag to improve its volume and composition stability.
[0006] The above-mentioned problems have greatly limited the application and development of steel slag in the field of road maintenance. Therefore, it is necessary to propose a new preparation device and method for road steel slag maintenance materials. By considering the optimal electromagnetic response particle size of steel slag, quantitative crushing and screening, and then modifying it, it can be prepared into a road maintenance material with stable composition, no fear of water invasion, and excellent maintenance effect. While giving full play to the maintenance function of road steel slag and improving the road maintenance effect, it also reduces the pulverization, fragmentation and other diseases of steel slag itself caused by water in long-term road use, in order to improve the quality of road engineering and extend the service life of roads. Summary of the invention
[0007] In order to overcome the problems in the prior art that steel slag expands when exposed to water, has unstable volume and poor maintenance effect when used as road maintenance material, the present invention provides a preparation device and a preparation method of road steel slag maintenance material.
[0008] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0009] The present invention provides a device for preparing road slag curing material and a method for preparing the road slag curing material. The device for preparing road slag curing material comprises a cracking reactor, a temperature and pressure control device, an alkalization reactor and a base; the cracking reactor comprises a cracking screening bin, the cracking screening bin is provided with pressure and temperature sensors inside, and the top cover is provided with a top cover, a high-pressure gate I is provided at the edge of the top cover to ensure the air tightness of the device, a hollow shaft is provided at the top of the cracking screening bin, a rolling disc is sleeved on the hollow shaft, the rolling disc can be driven by a motor to move vertically and rotate, a multi-stage screening tray is fixedly provided below the rolling disc, and three groups of discharging buffer bins are provided outside the side wall of the cracking screening bin; the temperature and pressure control device comprises a steam inlet valve and an exhaust valve provided at the top of the cracking screening bin, an electromagnetic heating coil I provided on the side wall of the cracking screening bin, and an interlayer I is provided outside the electromagnetic heating coil I; the alkalization reactor comprises a rotating tray, and six groups of alkalization tanks are symmetrically provided on the rotating tray;
[0010] The multi-stage screening tray comprises a first screening tray, a second screening tray, a third screening tray, and an arc-shaped residual material recovery tray arranged from top to bottom, wherein the first screening tray, the second screening tray, and the third screening tray are equipped with a detachable and replaceable arc-shaped metal screen, and the first screening tray, the third screening tray, and the arc-shaped residual material recovery tray are provided with a mass sensor;
[0011] The discharging buffer bin is connected to the cracking screening bin through three groups of discharging ports, the top heights of the discharging ports are aligned with the bottoms of the second screening tray, the third screening tray and the arc-shaped residual material recovery tray, and the discharging ports are provided with high-pressure gates II, and the lower part of the discharging buffer bin is provided with high-pressure gates III;
[0012] A motor bin is also provided at the lower part of the cracking and screening bin, a vibration motor is provided in the middle of the motor bin, and multiple groups of main vibration springs are provided at the edge of the motor bin, and the cracking reactor is connected to the base through the multiple groups of main vibration springs;
[0013] A solution tank is arranged in the middle of the rotating tray, the six groups of alkalization tanks are arranged around the side wall of the solution tank, and a delivery pipe connected with each alkalization tank is arranged in the solution tank, and a bidirectional pressure pump is arranged on the delivery pipe. Electromagnetic heating coil II is also arranged on the side wall and the bottom wall of the alkalization tank, and an interlayer II is arranged outside the electromagnetic heating coil II321.
[0014] As a further improvement of the present invention, conical rolling teeth are provided on the lower side of the rolling disc, which is beneficial for crushing the steel slag at the location where Ca(OH)2 is generated, i.e., where expansion and stress concentration occur, during the rolling and crushing process, thereby improving the crushing efficiency and quality.
[0015] As a further improvement of the present invention, a stirring paddle for accelerating the alkalization reaction rate is also provided at the bottom of the alkalization tank.
[0016] The present invention also provides a preparation method using the above preparation device, comprising the following steps:
[0017] S1. Preliminary selection of steel slag and determination of the optimal electromagnetic response particle size: After dust removal of the steel slag, needle-like particles are removed to obtain coarse steel slag. Road test pieces with different particle sizes are prepared with the coarse steel slag, and electromagnetic response experiments are carried out to confirm the required steel slag particle size range;
[0018] S2. Device preparation: According to the optimal slag particle size range determined in step S1, select an arc-shaped metal screen (122) with a specific mesh size, assemble it on each screening tray, turn on the electromagnetic heating coil I (23) in the cracking screening bin (11), and preheat it at 220° C. for 15 minutes;
[0019] S3, initial screening of steel slag: open the high-pressure gate I (112), lift the top cover (111) together with the hollow shaft (113) and the rolling plate (114), put the coarsely selected steel slag onto the first screening tray inside the cracking reactor (1), open the high-pressure gate II (131) at the discharge port (14) corresponding to the second screening tray and the third screening tray, so that the discharge buffer bin (13) below is connected with the cracking screening bin (11), turn on the vibration motor (151), and make the cracking reactor (1) vibrate as a whole under the support of the main vibration spring (152), and the steel slag aggregate vibrated and screened to the second screening tray and the third screening tray falls into the discharge buffer bin (13) through the discharge port (14). After vibrating and screening for 2 minutes, turn off the vibration motor (151);
[0020] S4, cracking and crushing of steel slag: close the high-pressure gate I (112) and the high-pressure gate II (131), open the steam inlet valve (21), introduce steam, and turn on the motor driving the rolling plate (114), so that under the high temperature and high pressure environment, the rolling plate (114) performs two modes of cracking and crushing of the steel slag to be crushed on the second screening tray, namely vertical crushing and horizontal grinding. After the cracking and crushing time reaches t1, turn off the motor of the rolling plate (114), stop crushing, and open the high-pressure gate II (131) and the vibration motor (151) to perform vibration screening on the steel slag on the multi-stage screening tray. The vibration screening time is t2, so that the crushed steel slag falls into the discharge buffer bin (13). After the discharge is completed, turn off the high-pressure gate II (131) and the vibration motor (151);
[0021] S5, alkalization of steel slag: opening the high pressure gate III (132) to allow the steel slag in the discharge buffer bin (13) to fall into the alkalization tank (32) below, and at the same time recovering the residual material collected on the arc-shaped residual material recovery plate 121. After the steel slag is immersed in the alkaline solution for a period of time t3, the bidirectional pressure pump (313) is turned on to pump the alkaline solution in the alkalization tank (32) into the solution tank (311) through the conveying pipe (312), and the electromagnetic heating coil II (321) is turned on to heat the alkalization tank (32). After the alkalized steel slag inside is dried, the material is discharged. The drying period is t4. At this point, the preparation of the steel slag curing material for this round of road use is completed. The bidirectional pressure pump (313) is turned on again to pump the alkaline solution in the solution tank (311) into the alkalization tank (32);
[0022] S6, multiple rounds of discharging: repeat steps S4 to S5 until all the steel slag on the first screening tray is crushed. During each round of discharging, the rotating tray alkalization tank (32) is rotated 60° clockwise to allow the steel slag from the new round of cracking and crushing to fall into the next alkalization tank (32) for alkalization reaction. During this process, the temperature and pressure in the cracking and screening bin (11) in each round of production are kept stable, and the temperature and pressure in the next round of cracking and screening bin (11) are adjusted according to the crushing results of the current round of production.
[0023] As a further improvement of the present invention, in step S1, the step of confirming the required slag particle size range specifically comprises the following steps:
[0024] S11, determine the total volume fraction v0 of steel slag in asphalt mixture, prepare steel slag samples to be selected, and screen them into n grades according to the specifications of pavement graded crushed stone aggregates according to engineering requirements, where n is the number of grades of aggregates in the pavement design gradation;
[0025] S12, completely replace the corresponding aggregate of each grade with steel slag, prepare n groups of standard Marshall specimens, each group has 4 Marshall specimens, and prepare 1 group of Marshall specimens without using steel slag to replace aggregate as a control group;
[0026] S13. Keeping other experimental conditions the same, place the two Marshall specimens in each group under microwave irradiation and heat for 90 seconds. Use an infrared thermometer to detect and record the microwave response temperature T of each group of specimens. i1 , where T i1 is the arithmetic mean of the top surface temperatures of the two specimens in group i after microwave heating, and the microwave response temperature of the control group is recorded as T 01 ;
[0027] S14. Keeping other experimental conditions the same, place the remaining two Marshall specimens in each group under the electromagnetic induction coil and heat them for 150 seconds. Use an infrared thermometer to detect and record the electromagnetic induction response temperature T of each group of specimens. i2 , where T i2 is the arithmetic mean of the maximum top surface temperatures of the two specimens in group i after electromagnetic induction heating. The electromagnetic induction response temperature of the control group is recorded as T 02 ;
[0028] S15, according to the specific dosage of each group of specimens and T i1 , T i2 , calculate the road electromagnetic response coefficient N of steel slag under microwave heating and electromagnetic induction heating conditions i1 、N i2 , which is calculated by the following formula:
[0029]
[0030] Where k = 1 or 2, V i It is the volume fraction of the mixture occupied by the i-th grade aggregate in the pavement design, i = 1, 2, 3, …, n.
[0031] S16. Arrange steel slag of different particle sizes according to the road electromagnetic response coefficient from large to small. When replacing aggregate for road use, according to the microwave heating or electromagnetic induction heating method required in the pavement maintenance plan, the steel slag particle size with the largest electromagnetic response coefficient is preferentially used to replace the same-grade aggregate. If the volume fraction of the aggregate in this grade is less than v0, the steel slag particle size with the largest electromagnetic response coefficient is selected from the remaining grades to replace the same-grade aggregate, and so on, until the total volume fraction of the steel slag in the asphalt mixture reaches v0.
[0032] As a further improvement of the present invention, in step S2 of the preparation method, the mesh size of the arc-shaped metal screen assembled on the first screening tray is c1, the mesh size of the arc-shaped metal screen assembled on the third screening tray is c2, and the mesh size of the arc-shaped metal screen assembled on the second screening tray is (c1+c2) / 2, wherein c1 and c2 are respectively the upper and lower limits of the required steel slag particle size specifications, and the arc-shaped metal screens are all arc-shaped structures with a convex middle and lower sides.
[0033] As a further improvement of the present invention, the ambient temperature in the cracking and screening bin is between 220° C. and 350° C., and the pressure is between 0.15 MPa and 0.3 MPa.
[0034] As a further improvement of the present invention, in step S5 of the preparation method, the solution used for alkalization modification is one of KOH and NaOH, and the concentration is between 10% and 15%. When the particle size of the steel slag to be alkalized is greater than 9.5 mm, its waterproofing requirement is relatively high, and it is appropriate to use a high concentration solution for alkalization. When the particle size of the steel slag is relatively small, it is appropriate to use a low concentration solution for alkalization.
[0035] As a further improvement of the present invention, in step S6, adjusting the temperature and pressure in the next round of cracking and screening bin according to the production and crushing results of the current round specifically includes the following steps:
[0036] S61: After the discharge is completed, the slag cracking and crushing degree index α in this round of production is calculated, which is specifically calculated by the following formula:
[0037]
[0038] Among them: m1 is the mass of steel slag reduced on the first screening tray screen in this round of production; m2 is the mass of steel slag increased on the third screening tray screen in this round of production; m3 is the mass of steel slag increased on the arc-shaped residual material recovery plate 121 in this round of production;
[0039] S62: If:
[0040] ①: α<0.45, it is judged that the degree of slag crushing is insufficient, and the power of electromagnetic heating coil Ⅰ23 is increased to increase the temperature and pressure in the next round of production cracking screening bin;
[0041] ②: α>0.55, it is judged that the slag has been over-crushed, and the power of electromagnetic heating coil I is reduced, and appropriate exhaust is performed through the exhaust valve to reduce the temperature and pressure in the next round of production cracking screening bin;
[0042] S63: According to the above principles, multiple rounds of adjustments are performed until α reaches 0.5±0.05, and the temperature and pressure of this round are recorded as standard temperature and pressure. In the subsequent production and preparation of steel slag of this particle size specification, the environment in the cracking and screening bin is maintained at the standard temperature and pressure.
[0043] As a further improvement of the present invention, in each round of production, the durations of t1, t2, t3 and t4 are adjusted to ensure that the discharge time of the discharging buffer bin in each round is just matched with the discharge time of the alkalization tank, wherein the cracking and crushing duration t1 is 10min to 20min, the vibration screening duration t2 is 2min to 5min, the soaking reaction duration t3 is 80min to 100min, and the drying duration t4 is 20min to 30min.
[0044] Advantages of the present invention:
[0045] 1. The present invention proposes a preparation device and a preparation method for road steel slag maintenance materials. For the steel slag that has been roughly selected, cracking and screening are used to quantitatively crush it while effectively consuming the free oxide components in the steel slag. Then, the prepared steel slag maintenance material is subjected to alkalization treatment, so that a layer of waterproof silicate is generated on its surface, which greatly enhances the waterproof performance and fundamentally reduces the expansion of the steel slag. In this way, the dual stability of the composition and volume of the steel slag material in the long-term service of road engineering is guaranteed, and the problems of the natural aging of the steel slag material in the traditional processing technology, such as the long process, the complex composition of the steel slag aggregate, the poor quality, and the risk of expansion and pulverization when exposed to water, which makes it impossible to use it as a road maintenance material on a large scale in engineering, are overcome. It has strong economic and engineering benefits.
[0046] 2. The method of the present invention fully considers the different responses of steel slag with different particle sizes. First, the particle size range of this batch of steel slag with the best road maintenance effect is determined by experiment, and combined with the proposed steel slag electromagnetic response coefficient index N ik Under the premise of considering the particle size, a design method for the replacement amount of aggregates by road maintenance materials is proposed, which overcomes the blindness and randomness of the replacement methods in the field of traditional road maintenance materials, greatly improves the electromagnetic heating maintenance effect of the road surface, and prolongs the service life of the road. In addition, this method can not only be used for the relevant design of road steel slag maintenance materials, but also for other external maintenance materials such as ferrite and iron tailings.
[0047] 3. The device in the present invention uses multi-stage screens and dynamic temperature and pressure adjustment control to comprehensively consider the actual crushing of steel slag in each round, the design grading of the pavement and the optimal electromagnetic response particle size of the steel slag material. After each round of production, combined with the degree of crushing of the steel slag in this round, the temperature and pressure in the next round of production device are dynamically adjusted to achieve quantitative and graded preparation of road steel slag maintenance materials, give full play to the maintenance potential of steel slag to replace road aggregates, and overcome the problem that traditional steel slag crushing devices cannot control the size of steel slag crushing particles and lack quantitative consideration, thereby resulting in poor road maintenance effect of the produced steel slag materials.
[0048] 4. The device of the present invention uses a rolling plate with conical teeth to crush the steel slag through two modes: vertical crushing and horizontal rotation grinding. Under high temperature and high pressure, the conical rolling teeth can effectively carry out fixed-point crushing of the steel slag that has undergone expansion reaction and has stress concentration points, thereby increasing the crushing efficiency and ensuring that the position of the steel slag crushing is exactly where the free calcium oxide exists. This overcomes the problem that traditional jaw crushing and roller crushing cannot capture the stress concentration point of the steel slag, and thus cannot control the crushing position, resulting in the steel slag still containing a lot of free calcium oxide after crushing.
[0049] 5. The device of the present invention has high integration and reasonable structural setting. Only coarse steel slag needs to be put into the preparation process. After cracking, crushing, soaking, alkalization, drying and other processes, quantitative, graded, stable and waterproof road steel slag can be produced. It can be directly used as road external admixture maintenance material, realizing integrated production, reducing the time allocation of each process, improving construction efficiency and reducing project cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 is a flow chart of the preparation method described in the present invention;
[0051] Figure 2 It is an overall schematic diagram of the preparation device described in the present invention;
[0052] Figure 3 is a schematic diagram of the rolling disc of the present invention;
[0053] Figure 4 It is a structural schematic diagram of the discharging buffer bin described in the present invention;
[0054] Figure 5 It is a structural schematic diagram of the alkalization reaction kettle described in the present invention;
[0055] Figure 6 It is a cross-sectional view of the alkalization reaction kettle described in the present invention.
[0056] Among them: 1. Cracking reactor; 11. Cracking screening chamber; 111. Top cover; 112. High-pressure gate I; 113. Hollow shaft; 114. Rolling plate;
[0057] 121. Arc-shaped residual material recovery plate; 122. Arc-shaped metal screen;
[0058] 13. Discharge buffer bin; 131. High-pressure gate II; 132. High-pressure gate III;
[0059] 14. Discharge port;
[0060] 15. Motor compartment; 151. Vibration motor; 152. Main vibration spring;
[0061] 21. Steam inlet valve; 22. Exhaust valve; 23. Electromagnetic heating coil I; 231. Interlayer I; 24. Quality sensor;
[0062] 3. Alkalinization reactor; 31. Rotating tray; 311. Solution tank; 312. Delivery pipe; 313. Bidirectional pressure pump;
[0063] 32. Alkalinization tank; 321. Electromagnetic heating coil II; 322. Interlayer II;
[0064] 4. Base. DETAILED DESCRIPTION
[0065] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0066] Embodiment: In this embodiment, the replacement amount of steel slag curing material v0=25%. Microwave heating is subsequently used to perform self-healing and ice-melting curing on the pavement. According to relevant construction specifications and specific working conditions, the design gradation of the AC-16 graded pavement is determined as shown in Table 1:
[0067] Table 1 Pavement design gradation of this embodiment
[0068]
[0069] In this regard, a preparation device and a preparation method of a road slag curing material proposed by the present invention are used, such as Figure 2 As shown, the preparation device includes a cracking reactor 1, a temperature and pressure control device, an alkalization reactor 3, and a base 4;
[0070] The cracking reactor 1 comprises a cracking and screening bin 11, wherein a sensor for detecting environmental pressure and temperature is arranged inside the cracking and screening bin 11, a top cover 111 is arranged at the top end of the cracking and screening bin 11, and a high-pressure gate Ⅰ 112 for ensuring air tightness is arranged at the edge of the top cover 111, and a hollow shaft 113 is arranged at the top end of the cracking and screening bin 11, and a rolling plate 114 is sleeved on the hollow shaft 113, and the rolling plate 114 can be driven by a motor to move vertically and rotate along the hollow shaft 113, such as Figure 3 As shown, a multi-stage screening tray is fixedly arranged below the rolling disc 114, and three groups of discharge buffer bins 13 are arranged outside the side wall of the cracking and screening bin 11; the temperature and pressure control device includes a steam inlet valve 21 and an exhaust valve 22 penetrating the top of the screening bin 11, and an electromagnetic heating coil Ⅰ23 arranged on the side wall of the cracking and screening bin 11, and an interlayer Ⅰ231 is arranged outside the electromagnetic heating coil Ⅰ23; the alkalization reactor 3 includes a rotating tray 31, and six groups of alkalization tanks 32 are symmetrically arranged on the rotating tray 31;
[0071] The multi-stage screening tray comprises a first screening tray, a second screening tray, a third screening tray, and an arc-shaped residual material recovery tray 121 arranged from top to bottom, wherein the first screening tray, the second screening tray, and the third screening tray are equipped with a detachable and replaceable arc-shaped metal screen 122, and the first screening tray, the third screening tray, and the arc-shaped residual material recovery tray 121 are provided with a mass sensor 24;
[0072] The discharge buffer bin 13 is connected to the cracking screening bin 11 through three groups of discharge ports 14. The top heights of the discharge ports 14 are aligned with the bottoms of the second screening tray, the third screening tray, and the arc-shaped residual material recovery tray 121, and the discharge ports 14 are each provided with a high-pressure gate II 131. Figure 4 As shown, a high-pressure gate III 132 is provided at the lower part of the discharge buffer bin 13;
[0073] A motor bin 15 is also provided at the lower part of the cracking and screening bin 11, a vibration motor 151 is provided in the middle of the motor bin 15, and multiple groups of main vibration springs 152 are provided at the edge of the motor bin 15, and the cracking reactor 1 is connected to the base 4 through the multiple groups of main vibration springs 152;
[0074] like Figures 5 to 6 As shown, a solution tank 311 is arranged in the middle of the rotating tray 31, and the six groups of alkalization tanks 32 are arranged around the side wall of the solution tank 311, and a delivery pipe 312 connected to each alkalization tank 32 is arranged in the solution tank 311, and a bidirectional pressure pump 313 is arranged on the delivery pipe 312, and an electromagnetic heating coil II 321 is also arranged on the side wall and the bottom wall of the alkalization tank 32, and an interlayer II 322 is arranged outside the electromagnetic heating coil II 321;
[0075] like Figure 1 As shown, the preparation method comprises the following steps:
[0076] First, after dust removal, the needle-like particles in the steel slag are screened out to obtain coarse steel slag. Road test specimens with different particle sizes are prepared with the coarse steel slag, and electromagnetic response experiments are carried out to determine the required steel slag particle size and dosage. The specific steps are as follows:
[0077] ①: Select appropriate steel slag samples and screen them into 9 grades according to the pavement aggregate specifications in Table 1;
[0078] ②: Each grade of steel slag was used to completely replace the corresponding grade of aggregate. Under laboratory conditions, 9 groups of standard Marshall specimens were prepared, of which 4 Marshall specimens were included in each group. A group of Marshall specimens without steel slag replacing aggregate was prepared as a control group. The amount of steel slag in each group is shown in Table 2.
[0079] Table 2 Slag replacement amount of each group of specimens
[0080] Number of experimental groups Slag content 1 All 0.15mm-0.3mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 7.9% 2 All 0.3mm-0.6mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 6.7% 3 All 0.6mm-1.18mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 5.6% 4 All 1.18mm to 2.36mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 17.6% 5 All the aggregates from 2.36mm to 4.75mm are replaced by steel slag of equal particle size, with a volume fraction of 12.7% 6 All 4.75mm to 9mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 15.6% 7 All 9mm to 13.2mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 12.1% 8 All 13.2mm-16mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 10.6% 9 All 19mm to 26.5mm aggregates are replaced by steel slag of equal particle size, with a volume fraction of 6.3%
[0081] ③: Keeping other experimental conditions the same, place the two Marshall specimens in each group under microwave irradiation and heat for 90 seconds. Use an infrared thermometer to detect and record the microwave response temperature T of each group of specimens. i1 , where T i1is the arithmetic mean of the top surface temperatures of the two specimens in group i after microwave heating, and the microwave response temperature of the control group is recorded as T 01 ;
[0082] ④: Keeping other experimental conditions the same, place the remaining two Marshall specimens in each group under the electromagnetic induction coil and heat them for 150s. Use an infrared thermometer to detect and record the electromagnetic induction response temperature T of each group of specimens. i2 , where T i2 is the arithmetic mean of the maximum top surface temperatures of the two specimens in group i after electromagnetic induction heating. The electromagnetic induction response temperature of the control group is recorded as T 02 ;
[0083] ⑤: According to the specific dosage of each group of specimens and T i1 , T i2 , calculate the road electromagnetic response coefficient N of steel slag under microwave heating and electromagnetic induction heating conditions i1 、N i2 , which is calculated by the following formula:
[0084]
[0085] Where k = 1 or 2, V i It is the volume fraction of the mixture occupied by the i-th grade aggregate in the pavement design, i = 1, 2, 3, …, n.
[0086] The calculation results are shown in Table 3:
[0087] Table 3 Experimental results of electromagnetic response of steel slag
[0088] Number of experimental groups <![CDATA[N i1 ]]> <![CDATA[N i2 ]]> Slag replacement amount 1 2.06 1.76 7.9% 2 4.97 1.48 6.7% 3 4.16 2.13 5.6% 4 5.37 4.88 17.6% 5 3.88 6.29 12.7% 6 5.64 5.19 15.6% 7 4.65 6.44 12.1% 8 5.44 6.31 10.6% 9 3.61 7.92 6.3%
[0089] ⑥: Since microwave heating is planned to be used for subsequent pavement maintenance, N is selected according to the experimental results. i1 As an indicator, N is preferred. i1 The fourth group with the largest value is selected as the replacement scheme, that is, all the aggregates of 4.75mm to 9mm are replaced by steel slag of equal particle size. Since the total replacement amount of steel slag has not reached 25% of the pavement design requirement, N is selected in the remaining groups. i1 The largest group, i.e., Group 8, is used as a subsequent alternative. The steel slag in the aggregates with a size of 3.2 mm to 16 mm accounts for 25%-17.6%=7.4% of the total volume of the mixture.
[0090] Next, the steel slag needs to be quantitatively crushed to 4.75mm-9mm and 13.2mm-16mm. First, 4.75mm-9mm road steel slag maintenance materials are produced and prepared. An arc-shaped metal screen 122 with a specific mesh size is selected and assembled on each screening tray. Among them, the mesh size of the arc-shaped metal screen 122 assembled on the first screening tray is c1=9mm, the mesh size of the arc-shaped metal screen 122 assembled on the third screening tray is c2=4.75mm, and the mesh size of the arc-shaped metal screen 122 assembled on the second screening tray is (c1+c2) / 2=6.9mm. The electromagnetic heating coil Ⅰ23 in the cracking screening bin 11 is turned on and preheated at 220°C for 15 minutes.
[0091] Next, the steel slag is preliminarily screened, the high-pressure gate I112 is opened, the top cover 111 together with the hollow shaft 113 and the rolling plate 114 are lifted, and the coarse steel slag is put into the first screening tray inside the cracking reactor 1. After the steel slag is put into, the top cover 111 is covered again, and the high-pressure gate I112 is closed. The high-pressure gate II131 at the discharge port 14 corresponding to the second and third screening trays is opened to connect the discharge buffer bin 13 below it with the cracking screening bin 11. The vibration motor 151 is turned on to make the cracking reactor 1 vibrate as a whole under the support of the main vibration spring 152. The steel slag aggregates vibrated and screened to the second and third screening trays fall into the discharge buffer bin 13 through the discharge port 14. After vibrating and screening for 2 minutes, the vibration motor 151 is turned off.
[0092] Next, the steel slag is cracked and crushed, the high pressure gate I112 and the high pressure gate II131 are closed, the steam inlet valve 21 is opened, and steam is introduced, so that the free calcium oxide in the steel slag undergoes a hydration reaction under high temperature and high pressure environment, the volume of this position expands, and becomes a stress concentration point that is easy to break and crack. The reaction equation involved is as follows:
[0093] CaO+H2O=Ca(OH)2
[0094] The motor driving the rolling plate 114 is turned on, and the rolling plate 114 performs two modes of cracking and crushing on the steel slag to be crushed on the second screening tray, namely, vertical crushing and horizontal grinding. At this time, the conical teeth on the rolling plate 114 act on the stress concentration point of the steel slag to ensure that the crushing position is the position where the free calcium oxide is located. After the cracking and crushing time reaches t1, the motor of the rolling plate 114 is turned off to stop the crushing, and the high-pressure gate II 131 and the vibration motor 151 are opened to vibrate and screen the steel slag on the multi-stage screening tray. The vibration screening time is t2, so that the crushed steel slag falls into the discharge buffer bin 13. After the discharge is completed, the high-pressure gate II 131 and the vibration motor 151 are closed;
[0095] Next, the steel slag is alkalized and modified, and the high-pressure gate III 132 is opened to allow the steel slag in the discharge buffer bin 13 to fall into the alkalization tank 32 below. At the same time, the residual material collected on the arc-shaped residual material recovery plate 121 is recovered. A large amount of SiO2 in the steel slag reacts with the 15% KOH solution in the alkalization tank 32 to generate silicate with high water resistance on its surface. The reaction equation involved is as follows:
[0096] SiO2+2KOH=K2SiO3+H2O
[0097] After the reaction time reaches t3, the bidirectional pressure pump 313 is turned on to pump the KOH solution in the alkalization tank 32 to the solution tank 311 through the delivery pipe 312, and the electromagnetic heating coil II 321 is turned on to heat the alkalization tank 32 to dry the alkalized steel slag inside. The drying time is t4, and the dried steel slag is discharged and collected. It does not need additional treatment and can be directly used as a road maintenance material with excellent performance. At this point, the preparation of this round of road steel slag maintenance materials is completed, and the bidirectional pressure pump 313 is turned on again to pump the alkaline solution in the solution tank 311 to the alkalization tank 32;
[0098] Repeat the above-mentioned "cracking and crushing-alkalization-drying and discharging" process until all the slag on the first screening tray is crushed. Adjust the durations of t1, t2, t3, and t4 according to the specific situation to ensure that the discharge time of each round of discharging buffer bin 13 matches the discharge time of alkalization tank 32. The alkalization tank 32 is rotated 60° clockwise by rotating the tray so that the slag from the new round of cracking and crushing falls into the next alkalization tank 32 for alkalization reaction. The cracking and crushing duration t1 is 10 min to 20 min, the vibration screening duration t2 is 2 min to 5 min, the soaking reaction duration t3 is 80 min to 100 min, and the drying duration t4 is 20 min to 30 min.
[0099] In addition, in each round of production, the temperature and pressure in the cracking and screening bin 11 are kept stable, and the temperature is between 220°C and 350°C, and the pressure is between 0.15 and 0.3 MPa. After each round of discharging, the slag cracking and crushing degree index α in this round of production is calculated, and the temperature and pressure in the next round of production are adjusted according to the size of α until α is close to 0.5, which is specifically calculated by the following formula:
[0100]
[0101] Among them: m1 is the mass of steel slag reduced on the first screening tray screen in this round of production; m2 is the mass of steel slag increased on the third screening tray screen in this round of production; m3 is the mass of steel slag increased on the arc-shaped residual material recovery plate 121 in this round of production;
[0102] In this embodiment, the calculation of α=0.32 in the first round of production indicates that the degree of slag crushing is insufficient. In the second round of production, the power of the electromagnetic heating coil I23 is increased to increase the temperature and pressure in the cracking and screening bin 11.
[0103] The calculation result of the second round of production is α=0.42, which still indicates that the slag is not broken enough. In the third round of production, the power of the electromagnetic heating coil I23 is further increased.
[0104] When α=0.64 is calculated for the third round of production, it is determined that the slag has been over-crushed. In the fourth round of production, the power of the electromagnetic heating coil I 23 is reduced, and appropriate exhaust is performed through the exhaust valve 22 to reduce the temperature and pressure in the cracking and screening bin 11;
[0105] Calculate the fourth round of production α = 0.54, α has met the condition of 0.5 ± 0.05, then it is judged that the degree of slag crushing meets the production requirements, and the temperature and pressure in the fourth round of production are recorded as the standard temperature and pressure. In the subsequent production of 4.75mm-9mm specification road slag curing materials, the environment in the cracking and screening bin 11 is maintained at the standard temperature and pressure until the production is completed;
[0106] Subsequently, according to the above method flow, the road steel slag maintenance material with a size of 13.2 mm to 16 mm is prepared and produced.
[0107] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0108] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A device for preparing road slag curing material, characterized in that: The invention comprises a cracking reactor (1), a temperature and pressure control device, an alkalization reactor (3), and a base (4); the cracking reactor (1) comprises a cracking screening chamber (11), a pressure and temperature sensor is arranged inside the cracking screening chamber (11), a top cover (111) is arranged at the top end of the cracking screening chamber (11), a high-pressure gate I (112) is arranged at the connection between the top cover (111) and the cracking screening chamber (11), a hollow shaft (113) is arranged at the top end of the cracking screening chamber (11), a rolling plate (114) is sleeved on the hollow shaft (113), and the rolling plate (114) can be driven by a motor to Vertical movement and rotation, a multi-stage screening tray is fixedly arranged below the rolling disc (114), and three groups of discharge buffer bins (13) are arranged outside the side wall of the cracking and screening bin (11); the temperature and pressure control device includes a steam inlet valve (21) and an exhaust valve (22) arranged at the top of the cracking and screening bin (11), and an electromagnetic heating coil I (23) arranged on the side wall of the cracking and screening bin (11), and an interlayer I (231) is arranged outside the electromagnetic heating coil I (23); the alkalization reaction kettle (3) includes a rotating tray (31), and six groups of alkalization tanks (32) are symmetrically arranged on the rotating tray (31); The multi-stage screening tray comprises a first screening tray, a second screening tray, a third screening tray, and an arc-shaped residual material recovery tray (121) arranged from top to bottom, the first screening tray, the second screening tray, and the third screening tray are equipped with a detachable and replaceable arc-shaped metal screen (122), and the first screening tray, the third screening tray, and the arc-shaped residual material recovery tray (121) are provided with a mass sensor (24); The discharge buffer bin (13) is connected to the cracking screening bin (11) through three groups of discharge ports (14), the top heights of the discharge ports (14) are aligned with the bottoms of the second screening tray, the third screening tray and the arc-shaped residual material recovery tray (121), and a high-pressure gate II (131) is provided at the discharge ports (14), and a high-pressure gate III (132) is provided at the lower part of the discharge buffer bin (13); A motor bin (15) is also provided at the lower part of the cracking and screening bin (11), a vibration motor (151) is provided in the middle of the motor bin (15), and a plurality of groups of main vibration springs (152) are provided at the edge of the motor bin (15), and the cracking reactor (1) is connected to the base (4) via the plurality of groups of main vibration springs (152); A solution tank (311) is arranged in the middle of the rotating tray (31), the six groups of alkalization tanks (32) are arranged around the side wall of the solution tank (311), and a delivery pipe (312) connected to each alkalization tank (32) is arranged in the solution tank (311), and a bidirectional pressure pump (313) is arranged on the delivery pipe (312). The side wall and the bottom wall of the alkalization tank (32) are also provided with an electromagnetic heating coil II (321), and an interlayer II (322) is arranged outside the electromagnetic heating coil II (321).
2. The device for preparing road slag curing material according to claim 1, characterized in that: The lower side of the rolling disc (114) is provided with conical rolling teeth.
3. The device for preparing road slag curing material according to claim 1, characterized in that: A stirring paddle (323) is also provided at the bottom of the alkalization tank (32).
4. A preparation method using the preparation device according to claim 1, characterized in that: The steps include: S1. Preliminary selection of steel slag and determination of the optimal electromagnetic response particle size: After dust removal of the steel slag, needle-like particles are removed to obtain coarse steel slag. Road test pieces with different particle sizes are prepared with the coarse steel slag, and electromagnetic response experiments are carried out to confirm the required steel slag particle size range; S2. Device preparation: According to the optimal slag particle size range determined in step S1, select an arc-shaped metal screen (122) with a specific mesh size, assemble it on each screening tray, turn on the electromagnetic heating coil I (23) in the cracking screening bin (11), and preheat it at 220° C. for 15 minutes; S3, initial screening of steel slag: open the high-pressure gate I (112), lift the top cover (111) together with the hollow shaft (113) and the rolling plate (114), put the coarsely selected steel slag onto the first screening tray inside the cracking reactor (1), open the high-pressure gate II (131) at the discharge port (14) corresponding to the second screening tray and the third screening tray, so that the discharge buffer bin (13) below is connected with the cracking screening bin (11), turn on the vibration motor (151), and make the cracking reactor (1) vibrate as a whole under the support of the main vibration spring (152), and the steel slag aggregate vibrated and screened to the second screening tray and the third screening tray falls into the discharge buffer bin (13) through the discharge port (14). After vibrating and screening for 2 minutes, turn off the vibration motor (151); S4, cracking and crushing of steel slag: close the high-pressure gate I (112) and the high-pressure gate II (131), open the steam inlet valve (21), introduce steam, and turn on the motor driving the rolling plate (114), so that under the high temperature and high pressure environment, the rolling plate (114) performs two modes of cracking and crushing of the steel slag to be crushed on the second screening tray, namely vertical crushing and horizontal grinding. After the cracking and crushing time reaches t1, turn off the motor of the rolling plate (114), stop crushing, and open the high-pressure gate II (131) and the vibration motor (151) to perform vibration screening on the steel slag on the multi-stage screening tray. The vibration screening time is t2, so that the crushed steel slag falls into the discharge buffer bin (13). After the discharge is completed, turn off the high-pressure gate II (131) and the vibration motor (151); S5, alkalization of steel slag: opening the high pressure gate III (132) to allow the steel slag in the discharge buffer bin (13) to fall into the alkalization tank (32) below, and at the same time recovering the residual material collected on the arc-shaped residual material recovery plate 121. After the steel slag is immersed in the alkaline solution for a period of time t3, the bidirectional pressure pump (313) is turned on to pump the alkaline solution in the alkalization tank (32) into the solution tank (311) through the conveying pipe (312), and the electromagnetic heating coil II (321) is turned on to heat the alkalization tank (32). After the alkalized steel slag inside is dried, the material is discharged. The drying period is t4. At this point, the preparation of the steel slag curing material for this round of road use is completed. The bidirectional pressure pump (313) is turned on again to pump the alkaline solution in the solution tank (311) into the alkalization tank (32); S6, multiple rounds of discharging: repeat steps S4 to S5 until all the steel slag on the first screening tray is crushed. During each round of discharging, the rotating tray alkalization tank (32) is rotated 60° clockwise to allow the steel slag from the new round of cracking and crushing to fall into the next alkalization tank (32) for alkalization reaction. During this process, the temperature and pressure in the cracking and screening bin (11) in each round of production are kept stable, and the temperature and pressure in the next round of cracking and screening bin (11) are adjusted according to the crushing results of the current round of production.
5. The preparation method according to claim 4, characterized in that: In step S1, the step of determining the required slag particle size range specifically includes the following steps: S11, determine the total volume fraction v0 of steel slag in asphalt mixture, prepare steel slag samples to be selected, and screen them into n grades according to the specifications of pavement graded crushed stone aggregates according to engineering requirements, where n is the number of grades of aggregates in the pavement design gradation; S12, completely replace the corresponding aggregate of each grade with steel slag, prepare n groups of standard Marshall specimens, each group has 4 Marshall specimens, and prepare 1 group of Marshall specimens without using steel slag to replace aggregate as a control group; S13. Keeping other experimental conditions the same, place the two Marshall specimens in each group under microwave irradiation and heat for 90 seconds. Use an infrared thermometer to detect and record the microwave response temperature T of each group of specimens. i1 , where T i1 is the arithmetic mean of the top surface temperatures of the two specimens in group i after microwave heating, and the microwave response temperature of the control group is recorded as T 01 ; S14. Keeping other experimental conditions the same, place the remaining two Marshall specimens in each group under the electromagnetic induction coil and heat them for 150 seconds. Use an infrared thermometer to detect and record the electromagnetic induction response temperature T of each group of specimens. i2 , where T i2 is the arithmetic mean of the maximum top surface temperatures of the two specimens in group i after electromagnetic induction heating. The electromagnetic induction response temperature of the control group is recorded as T 02 ; S15, according to the specific dosage of each group of specimens and T i1 , T i2 , calculate the road electromagnetic response coefficient N of steel slag under microwave heating and electromagnetic induction heating conditions i1 、N i2 , which is calculated by the following formula: Where k = 1 or 2, V i It is the volume fraction of the mixture occupied by the i-th grade aggregate in the pavement design, i = 1, 2, 3, …, n. S16. Arrange steel slag of different particle sizes according to the road electromagnetic response coefficient from large to small. When replacing aggregate for road use, according to the microwave heating or electromagnetic induction heating method required in the pavement maintenance plan, the steel slag particle size with the largest electromagnetic response coefficient is preferentially used to replace the same-grade aggregate. If the volume fraction of the aggregate in this grade is less than v0, the steel slag particle size with the largest electromagnetic response coefficient is selected from the remaining grades to replace the same-grade aggregate, and so on, until the total volume fraction of the steel slag in the asphalt mixture reaches v0.
6. The preparation method according to claim 4, characterized in that: In step S2 of the preparation method, the mesh size of the arc-shaped metal screen (122) assembled on the first screening tray is c1, the mesh size of the arc-shaped metal screen (122) assembled on the third screening tray is c2, and the mesh size of the arc-shaped metal screen (122) assembled on the second screening tray is (c1+c2) / 2, wherein c1 and c2 are respectively the upper and lower limits of the required steel slag particle size specifications.
7. The preparation method according to claim 4, characterized in that: The ambient temperature in the cracking and screening bin (11) is between 220°C and 350°C, and the pressure is between 0.15MPa and 0.3MPa.
8. The preparation method according to claim 4, characterized in that: In step S5 of the preparation method, the solution used for alkalization modification is any one of KOH and NaOH, and the concentration is between 10% and 15%.
9. The preparation method according to claim 4, characterized in that: In step S6, the temperature and pressure in the next round of cracking and screening bin (11) are adjusted according to the production and crushing results of the current round, which specifically includes the following steps: S61: After the discharge is completed, the slag cracking and crushing degree index α in this round of production is calculated, which is specifically calculated by the following formula: Wherein: m1 is the mass of steel slag reduced on the first screening tray screen in this round of production; m2 is the mass of steel slag increased on the third screening tray screen in this round of production; m3 is the mass of steel slag increased on the arc-shaped residual material recovery plate (121) in this round of production; S62: If: ①: α<0.45, it is judged that the degree of slag crushing is insufficient, and the power of electromagnetic heating coil I (23) is increased to increase the temperature and pressure in the next round production cracking screening bin (11); ②: α>0.55, it is judged that the steel slag has been over-crushed, the power of the electromagnetic heating coil I (23) is reduced, and appropriate exhaust is performed through the exhaust valve (22) to reduce the temperature and pressure in the next round of production cracking screening bin (11); S63: According to the above principle, multiple rounds of adjustment are performed until α reaches 0.5±0.05, and the temperature and pressure of this round are recorded as standard temperature and pressure. In the subsequent production and preparation of steel slag of this particle size specification, the environment in the cracking and screening bin (11) is maintained at the standard temperature and pressure.
10. The preparation method according to claim 4, characterized in that: In each round of production, the durations of t1, t2, t3 and t4 are adjusted to ensure that the discharge time of the discharging buffer bin (13) and the discharging time of the alkalization tank (32) in each round can be matched, wherein the cracking and crushing duration t1 is 10 minutes to 20 minutes, the vibration screening duration t2 is 2 minutes to 5 minutes, the soaking reaction duration t3 is 80 minutes to 100 minutes, and the drying duration t4 is 20 minutes to 30 minutes.