Phosphorus-aluminum co-doped nickel oxide material as well as preparation method and application thereof

Through the simplified preparation method of phosphorus-aluminum co-doped nickel oxide material, the problem of limited photocatalytic degradation of antibiotics in existing doped nickel oxide materials is solved, and the efficient photocatalytic degradation effect is achieved, which is suitable for industrial production.

CN118892853AActive Publication Date: 2024-11-05SINOMACH (DEYANG) INSPECTION TECH CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410941695.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing doped nickel oxide materials have limited effects in photocatalytic degradation of antibiotics, and the production method is complex and unfavorable to industrial production.

Method used

Using the preparation method of phosphorus-aluminum co-doped nickel oxide material, the NaH2PO4·H2O and NiAl-LDH powder are heated in a tube furnace to obtain phosphorus-aluminum co-doped nickel oxide material with good photocatalytic properties.

Benefits of technology

This method simplifies the process flow and reduces the cost. The degradation rate of phosphorus aluminum co-doped nickel oxide material reaches 89.9% when photocatalyzed the tetracycline, which is significantly higher than the self-degradation rate of the precursor and the degradation rate of NiAl-LDH. Better photocatalytic degradation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892853A_ABST
    Figure CN118892853A_ABST
Patent Text Reader

Abstract

The invention relates to a phosphorus-aluminum co-doped nickel oxide material as well as a preparation method and application thereof, and belongs to the technical field of photocatalytic degradation of pollutants such as antibiotics. The technical problem to be solved by the invention is to provide the preparation method of the phosphorus-aluminum co-doped nickel oxide material, which is simple in process flow and easy to control. The method comprises the following steps: uniformly spreading NaH2PO4.H2O and NiAl-LDH powder in porcelain boats respectively, placing the porcelain boat filled with NaH2PO4.H2O in a tubular furnace for upward flow, placing the porcelain boat filled with NiAl-LDH powder in the tubular furnace for downward flow, heating the tubular furnace to 250-350 DEG C, keeping for 1-3 hours in a protective atmosphere, and cooling to obtain the NiAl-LDH / NaH2PO4.H2O composite material. The method is simple in process, low in energy consumption, low in cost and beneficial to industrial production, the synthetic material has good photocatalytic performance, the degradation rate of 10 mg / L tetracycline is 89.9% and is 12.5 times that of self-degradation of tetracycline, and the degradation rate of tetracycline is 1.82 times that of a precursor NiAl-LDH, it is indicated that the catalyst has better photocatalytic degradation performance, and the application prospect is wide. The problem of environmental pollution can be better solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phosphorus-aluminum co-doped nickel oxide material and a preparation method and application thereof, and belongs to the technical field of photocatalytic degradation of pollutants such as antibiotics. Background Art

[0002] Antibiotics remaining in the environment will not only destroy the water ecological balance, but will also induce the production of resistance genes in microorganisms, thereby generating more drug-resistant super pathogens.

[0003] In recent years, people have used hydrolysis, electrochemical oxidation, microbial degradation and other methods to remove antibiotics. Among them, hydrolysis is generally used in industry, but it is sensitive to pH and temperature, and its degradation time is long and its efficiency is low; electrochemical oxidation can change the chemical properties of organic matter and improve the degradability of antibiotics, but the cost of electrochemical oxidation is high, and the byproducts produced by its reaction may cause secondary pollution; microbial degradation is the main method for degrading antibiotics in the environment, which can convert organic pollutants into H2O, CO2 and other environmentally friendly substances, but it often produces odors during the reaction. Photocatalysis is a green and safe technology that converts solar energy into chemical energy, which can help degrade organic matter, and the process is efficient, fast, green and safe. The catalyst plays an important role in the photocatalytic reaction, and a single catalyst often has the problem of rapid recombination of photogenerated electrons and holes, which is not conducive to the photocatalytic reaction. In addition, some popular catalysts such as TiO2, Fe2O3 and ZnO2 only absorb ultraviolet light. Ultraviolet light accounts for about 1% to 2% of sunlight, and visible light accounts for about 50%. Therefore, developing catalysts that respond to visible light can make more efficient use of solar energy.

[0004] Nickel oxide is a highly active catalyst with abundant surface active sites. It can effectively promote photocatalytic reactions and has good stability. However, it also faces the problem of rapid recombination of photogenerated carriers. There are many ways to modify nickel oxide, such as precious metal deposition, deposition or doping of nickel oxide with precious metals such as gold, silver, and platinum, but the cost is high; selecting semiconductor materials that match the energy level of nickel oxide for compounding may not necessarily achieve better photocatalytic effects. Doping the catalyst is also a modification method.

[0005] The Chinese invention patent with application number 201210143328.X discloses a method for preparing a Ru-Li co-doped nickel oxide thin film, which first prepares a Ru-Li co-doped nickel sol, then coats the film and performs heat treatment for 1-2 hours to obtain a Ru-Li co-doped nickel oxide thin film. When preparing the Ru-Li co-doped nickel sol, first stir it for 30 to 40 minutes under water bath heating conditions, add the doping element and continue stirring for 90 to 100 minutes, then let it stand in the air for 24 to 48 hours, and finally ultrasonically clean it for 10 to 15 minutes and dry it to obtain the Ru-Li co-doped nickel sol. This method has a long reaction time for preparing Ru-Li co-doped nickel and the work is cumbersome and complicated.

[0006] The Chinese invention patent with application number 202311374555.8 discloses a method for preparing a zinc-cobalt co-doped NiO-X film for an inverse perovskite battery, comprising the following steps: S1. Select a substrate, first use detergent and deionized water for ultrasonic cleaning, then put it into acetone and anhydrous ethanol for ultrasonic cleaning respectively, and dry the substrate with a nitrogen gun; S2. Use radio frequency plasma superimposed pulse negative bias to clean the substrate; S3. Use a DC / RF coupled reactive sputtering process to deposit a NiOX film on the ITO surface of the cleaned substrate, and use a DC sputtering process to co-deposit metal zinc and metal cobalt on the ITO surface; S4. After sputtering, wait for the substrate to cool to room temperature, heat the substrate to a constant temperature, cool it to room temperature again to take out the sample, and obtain a zinc-cobalt co-doped NiOX film. The preparation process of this patent is complicated and not conducive to the industrial production of the product.

[0007] The Chinese invention patent with application number 201811227041.9 discloses a lithium-silver co-doped nickel oxide film and its application in perovskite solar cells. A certain amount of Ni(NO3)2·6H2O, LiNO3 and AgNO3 are weighed and added to deionized water for stirring and dissolution. The molar ratio range is 0.989-0.98:0.001-0.005:0.01-0.015, and then NaOH solution is added dropwise until the pH reaches 9.8-10. After washing and drying, the nanoparticles of lithium-silver co-doped nickel oxide are obtained by calcining at 270°C. It is applied to the hole transport layer of the inverted planar perovskite solar cell to improve its photoelectric conversion efficiency.

[0008] In summary, the existing doping is used for perovskite batteries or resistive memory devices, and its photocatalytic degradation effect of antibiotics is limited. In addition, its preparation method is complicated and cumbersome, which is not conducive to the industrial production of the product. Summary of the invention

[0009] In view of the above defects, the first technical problem solved by the present invention is to provide a method for preparing phosphorus-aluminum co-doped nickel oxide material with a simple and easy-to-control process flow.

[0010] The method for preparing the phosphorus-aluminum co-doped nickel oxide material of the present invention comprises the following steps:

[0011] NaH2PO4·H2O and NiAl-LDH powders are evenly spread in porcelain boats respectively. The porcelain boat containing NaH2PO4·H2O is placed upstream of the air flow of the tubular furnace, and the porcelain boat containing NiAl-LDH powder is placed downstream of the air flow of the tubular furnace. The tubular furnace is heated to 250-350°C and maintained in a protective atmosphere for 1-3 hours, and then cooled to obtain phosphorus-aluminum co-doped nickel oxide material.

[0012] In one embodiment of the present invention, the mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 8 to 12:1; in a specific embodiment, the mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 10:1.

[0013] In one embodiment of the present invention, the heating rate is 2-5°C / min. In a specific embodiment, the heating rate is 2°C / min.

[0014] In one embodiment of the present invention, the temperature of the tube furnace is raised to 300° C. and maintained for 2 hours.

[0015] In one embodiment of the present invention, NiAl-LDH powder is prepared by a hydrothermal method.

[0016] In one embodiment of the present invention, NiAl-LDH powder is synthesized by the following method: Ni(NO3)2·6H2O, Al(NO3)3·9H2O, urea, NH4F and water are mixed, heated at 100-140°C for 10-14 hours, a precipitate is taken, washed and dried to obtain NiAl-LDH powder; wherein the molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O and urea is 2.5-3.5:1:18-22.

[0017] In one embodiment of the present invention, the molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O and urea is 3:1:20; heating is performed at 120°C for 12 hours.

[0018] The second technical problem solved by the present invention is to provide a phosphorus-aluminum co-doped nickel oxide material.

[0019] The phosphorus-aluminum co-doped nickel oxide material of the present invention is prepared by adopting the above-mentioned method for preparing the phosphorus-aluminum co-doped nickel oxide material. The material has low cost and good photocatalytic performance.

[0020] The present invention also provides the use of the phosphorus-aluminum co-doped nickel oxide material of the present invention in photocatalytic degradation of antibiotics.

[0021] The phosphorus-aluminum co-doped nickel oxide material of the present invention can be applied to photocatalytic degradation of antibiotics.

[0022] In one embodiment of the present invention, the antibiotic is tetracycline.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The method of the invention has a simple process, and the target product can be obtained by phosphating the precursor, thereby saving steps, reducing energy consumption, and having a low cost, which is conducive to industrial production. The synthetic material has good photocatalytic performance, and the degradation rate of 10 mg / L tetracycline reaches 89.9%, which is 12.5 times that of the self-degradation thereof and 1.82 times that of the precursor NiAl-LDH, indicating that the catalyst has better photocatalytic degradation performance and can be used to better solve environmental pollution problems. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 1 is the XRD diagram of NiAl-LDH powder and P-Al-NiO in Example 1 of the present invention.

[0026] Figure 2 The SEM images of NiAl-LDH powder and P-Al-NiO in Example 1 of the present invention and the EDS element mapping image of P-Al-NiO are shown.

[0027] Figure 3 This is a diagram of the photocatalytic degradation performance of P-Al-NiO in Example 1. DETAILED DESCRIPTION

[0028] The method for preparing the phosphorus-aluminum co-doped nickel oxide material of the present invention comprises the following steps:

[0029] NaH2PO4·H2O and NiAl-LDH powders are evenly spread in porcelain boats respectively. The porcelain boat containing NaH2PO4·H2O is placed upstream of the air flow of the tubular furnace, and the porcelain boat containing NiAl-LDH powder is placed downstream of the air flow of the tubular furnace. The tubular furnace is heated to 250-350°C and maintained in a protective atmosphere for 1-3 hours, and then cooled to obtain phosphorus-aluminum co-doped nickel oxide material.

[0030] The protective atmosphere described in the present invention is an atmosphere that does not participate in the reaction, including but not limited to an inert atmosphere such as helium, argon, or a nitrogen atmosphere.

[0031] In one embodiment of the present invention, the mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 8 to 12:1; in a specific embodiment, the mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 10:1.

[0032] In one embodiment of the present invention, the heating rate is 2-5°C / min. In a specific embodiment, the heating rate is 2°C / min.

[0033] In one embodiment of the present invention, the temperature of the tube furnace is raised to 300° C. and maintained for 2 hours.

[0034] In one embodiment of the present invention, NiAl-LDH powder is prepared by a hydrothermal method.

[0035] In one embodiment of the present invention, NiAl-LDH powder is synthesized by the following method: Ni(NO3)2·6H2O, Al(NO3)3·9H2O, urea, NH4F and water are mixed, heated at 100-140°C for 10-14 hours, a precipitate is taken, washed and dried to obtain NiAl-LDH powder; wherein the molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O and urea is 2.5-3.5:1:18-22.

[0036] In one embodiment of the present invention, the molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O and urea is 3:1:20; heating is performed at 120°C for 12 hours.

[0037] In a specific embodiment of the present invention, the preparation method of NiAl-LDH powder is as follows: Ni(NO3)2·6H2O, Al(NO3)3·9H2O, urea (0.48mmol Ni(NO3)2·6H2O, 0.16mmolAl(NO3)3·9H2O, 3.2mmol urea) with a molar ratio of 3:1:20, and a certain amount of NH4F (1.28mmolNH4F) are added to 60mL deionized water, and then ultrasonicated for half an hour to obtain a uniform solution. The above solution is transferred to a 100mL polytetrafluoroethylene-lined autoclave and heated at 120°C for 12 hours. Wash with distilled water and ethanol several times, and vacuum dry overnight at 60°C to obtain NiAl-LDH powder.

[0038] The phosphorus-aluminum co-doped nickel oxide material of the present invention is prepared by adopting the above-mentioned method for preparing the phosphorus-aluminum co-doped nickel oxide material. The material has low cost and good photocatalytic performance.

[0039] The phosphorus-aluminum co-doped nickel oxide material of the present invention can be applied to photocatalytic degradation of antibiotics.

[0040] In one embodiment of the present invention, the antibiotic is tetracycline.

[0041] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0042] Example 1

[0043] The phosphorus-aluminum co-doped nickel oxide material is prepared by the following method:

[0044] Step 1: Preparation of NiAl-LDH powder

[0045] First, NiAl-LDH was synthesized by a hydrothermal method: Ni(NO3)2·6H2O, Al(NO3)3·9H2O, urea (0.48mmol Ni(NO3)2·6H2O, 0.16mmol Al(NO3)3·9H2O, 3.2mmol urea) with a molar ratio of 3:1:20, and a certain amount of NH4F (1.28mmol NH4F) were added to 60mL deionized water, and then ultrasonicated for half an hour to obtain a uniform solution. The above solution was transferred to a 100mL polytetrafluoroethylene-lined autoclave and heated at 120°C for 12 hours. It was washed with distilled water and ethanol several times and vacuum dried at 60°C overnight to obtain NiAl-LDH powder.

[0046] Step 2: Preparation of phosphorus-aluminum co-doped nickel oxide material

[0047] NaH2PO4·H2O and precursor NiAl-LDH powder were weighed at a mass ratio of 10:1 and evenly spread in a porcelain boat. The porcelain boat containing NaH2PO4·H2O was placed upstream of the tube furnace, and the porcelain boat containing NiAl-LDH powder was placed downstream of the tube furnace. The temperature of the tube furnace was raised to 300°C at a heating rate of 2°C per minute and maintained in a N2 atmosphere for 2 hours (i.e., the reaction temperature was 300°C and the reaction time was 2 hours), and then cooled naturally to room temperature. The dark green powder obtained was P and Al co-doped nickel oxide, named P-Al-NiO.

[0048] The X-ray diffraction patterns of the above materials are shown in Figure 1. The results show that the main diffraction peaks of the obtained product are in good agreement with the NiAl-LDH standard card (PDF#15-0087), and the peaks are sharp, indicating that NiAl-LDH has high crystallinity. The three characteristic diffraction peaks of P-Al-NiO are respectively attributed to the three crystal planes (111), (200) and (220), belonging to the NiO phase (PDF#47-1049), which indicates that the precursor NiAl-LDH undergoes material changes during the high-temperature phosphating treatment. In addition, it can be observed that the diffraction peaks of P-Al-NiO are broadened, and the intensity of the diffraction peaks is much lower than that of standard nickel monoxide (PDF#47-1049). It can be inferred that the doping of P and Al leads to low crystallinity of NiO and disordered lattice.

[0049] Figure 2 (a) SEM image of NiAl-LDH; (b) SEM image of P-Al-NiO; (cg) EDS element mapping of P-Al-NiO, where d is Ni element; e is O element; f is P element; g is Al element. It can be seen that the morphology of P-Al-NiO (Figure b) obtained after high-temperature phosphating of the precursor NiAl-LDH has not changed significantly, and still maintains the nanoflower shape. This unique nanoflower structure can provide a larger specific surface area. From Figures cd, it can be seen that Al, P, Ni and O elements are evenly distributed on the surface of the material, proving that P and Al are successfully doped in NiO.

[0050] The photocatalytic performance of the material was determined. Tetracycline (TC) was used as the target pollutant and a xenon lamp was used to simulate the visible light source. The specific steps were as follows: 10 mg of the sample was dispersed in a TC (100 mL, 10 mg / L) aqueous solution. The suspension was stirred in the dark for 1 hour to achieve adsorption equilibrium between the photocatalyst and the tetracycline solution. Then, the solution was placed under a light source for illumination. The visible light was generated by a 300W xenon lamp through an ultraviolet cutoff filter (λ>420nm). 3 mL of the sample solution was centrifuged within a fixed time and the sample was measured by a UV-visible spectrophotometer.

[0051] Figure 3 This is a photocatalytic degradation performance diagram. Under visible light irradiation for 2 hours, the self-degradation rate of TC is only about 7.2%, which belongs to the type of unsatisfactory self-degradation performance. The degradation rate of the precursor NiAl-LDH is about 49.3%, and the degradation rate of P-Al-NiO is 89.9%, which is 12.5 times that of the self-degradation and 1.82 times that of the precursor NiAl-LDH.

[0052] Example 2

[0053] Referring to the method of Example 1, some parameters were changed to obtain P and Al co-doped nickel oxide, and the changed parameters are shown in Table 1. The degradation rate under visible light irradiation for 2 hours is shown in Table 1.

[0054] Table 1

[0055]

[0056] It can be seen that the phosphorus-aluminum co-doped nickel oxide material can be successfully prepared by the method of the present invention. The material can be used for visible light photocatalytic degradation of tetracycline with a high degradation rate.

Claims

1. A method for preparing a phosphorus-aluminum co-doped nickel oxide material, characterized in that: The following steps are involved: NaH2PO4·H2O and NiAl-LDH powders are evenly spread in porcelain boats respectively. The porcelain boat containing NaH2PO4·H2O is placed upstream of the air flow of the tubular furnace, and the porcelain boat containing NiAl-LDH powder is placed downstream of the air flow of the tubular furnace. The tubular furnace is heated to 250-350°C and maintained in a protective atmosphere for 1-3 hours, and then cooled to obtain phosphorus-aluminum co-doped nickel oxide material.

2. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 1, characterized in that: The mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 8 to 12:1; preferably, the mass ratio of NaH2PO4·H2O to NiAl-LDH powder is 10:

1.

3. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 1, characterized in that: The heating rate is 2-5°C / min; preferably, the heating rate is 2°C / min.

4. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 1, characterized in that: The temperature of the tube furnace was raised to 300°C and maintained for 2 hours.

5. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 1, characterized in that: NiAl-LDH powder was prepared by hydrothermal method.

6. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 1, characterized in that: The NiAl-LDH powder is synthesized by a hydrothermal method; preferably, the NiAl-LDH powder is synthesized by the following method: Ni(NO3)2·6H2O, Al(NO3)3·9H2O, urea, NH4F and water are mixed, heated at 100-140°C for 10-14 hours, a precipitate is taken, washed and dried to obtain NiAl-LDH powder; wherein the molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O and urea is 2.5-3.5:1:18-22.

7. The method for preparing the phosphorus-aluminum co-doped nickel oxide material according to claim 6, characterized in that: The molar ratio of Ni(NO3)2·6H2O, Al(NO3)3·9H2O, and urea is 3:1:20; heating at 120°C for 12 hours.

8. The phosphorus-aluminum co-doped nickel oxide material prepared by the method for preparing the phosphorus-aluminum co-doped nickel oxide material according to any one of claims 1 to 7.

9. Use of the phosphorus-aluminum co-doped nickel oxide material according to claim 8 in photocatalytic degradation of antibiotics.

10. The use of the phosphorus-aluminum co-doped nickel oxide material in photocatalytic degradation of antibiotics according to claim 9, characterized in that: The antibiotic is tetracycline.

Citation Information

Patent Citations

  • Preparation method of Ru-Li codoped nickel oxide film

    CN102653863A

  • Lithium and silver co-doped nickel oxide film and application thereof in perovskite solar cell

    CN109545969A

  • Preparation method of zinc and cobalt co-doped NiOX thin film for trans-perovskite battery

    CN117488254A

  • Molybdenum-based catalyst for preparing low-carbon alcohol from synthesis gas by taking alkaline carrier material mesoporous NiO-Al2O3 as carrier and preparation method of molybdenum-based catalyst

    CN112844418A

  • Phosphorus-doped modified carbon quantum dot and preparation method of composite photocatalyst thereof

    CN115418225A