Ultra-high-strength steel hot stamping die and use method thereof

Through the design and optimization of cooling and lubrication system combined with induction heating and thermal expansion layer, the forming accuracy and mold life problems in hot stamping of high-strength materials are solved, efficient cooling and precise lubrication are achieved, and finished product quality and mold durability are significantly improved.

CN118893138BActive Publication Date: 2024-12-03SOUTHWEST PETROLEUM UNIV
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411382116.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

When handling hot stamping of high-strength materials, the forming accuracy is insufficient, the material rebound is difficult to control, the mold life is short, and the formation accuracy of complex geometric shapes is difficult to guarantee.

Method used

The design of induction heating combined with thermal expansion layer is optimized to optimize the cooling system and lubrication system, and the cooling efficiency is improved through the cooling chamber, cooling pipeline and partition structure, and secondary stamping and gas film lubrication technology is used to reduce friction and eliminate material stress.

Benefits of technology

Effectively control material rebound, improve finished product dimensional accuracy and mold durability, extend mold life, and is suitable for precision forming of complex shapes and high-strength materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893138B_ABST
    Figure CN118893138B_ABST
Patent Text Reader

Abstract

The present invention relates to an ultra-high strength steel hot stamping die and a method for using the same applied to the technical field of hot stamping dies. The die has an efficient cooling system. The design of a cooling cavity, a cooling pipe and a partition plate enables rapid cooling of the die during operation, thereby ensuring operational stability. The precise lubrication system forms a uniform lubrication layer through the application of a lubrication tube and graphite powder, thereby effectively reducing material surface friction and protecting the surface quality of the finished product. During the stamping process, the die eliminates material stress and reduces springback through the combination of an induction heating tube and a thermal expansion layer, thereby ensuring dimensional accuracy and structural strength of the finished product. The secondary stamping design of the die improves the molding accuracy of the material, has strong adaptability, can meet the needs of different operating environments, and enhances the durability of the die. The die is particularly suitable for processing highly difficult materials such as ultra-high strength steel, thereby improving production efficiency and product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hot stamping dies, and in particular to an ultra-high strength steel hot stamping die and a use method thereof. Background Art

[0002] In the existing technology, the hot stamping forming process of ultra-high-strength steel is widely used in the fields of automobile manufacturing, aerospace, etc. to manufacture structural parts with high strength and high toughness. However, with the increasing requirements for material performance, traditional hot stamping die technology still has some problems when processing ultra-high-strength steel, such as insufficient forming accuracy, difficult to control material springback, and short die life.

[0003] Chinese invention patent CN109762965B discloses a method for continuous online preparation of ultra-high strength and toughness Mn-B steel structural parts. Through continuous transmission of electrode rollers and self-resistance heating, cyclic heating and quenching of Mn-B steel are achieved. This technology can effectively reduce oxidation and promote the application of low-cost non-coated plates. Through repeated heating and quenching, the elements can be uniformly diffused, thereby improving the performance uniformity of the components. However, this technology mainly focuses on the microstructure control and performance optimization of the material, and fails to solve practical problems such as rebound control and die wear of hot stamping dies in high-strength forming.

[0004] Chinese invention patent CN107008809B discloses a hot stamping and drawing die for ultra-high-strength steel box-shaped parts. The drawing performance of ultra-high-strength boron-manganese steel under different forming process parameters is studied, and a block structure is adopted to evenly arrange cooling water channels inside the die, combined with an external cooling water flow rate control system to control the quenching process. However, although this design improves the cooling efficiency of the die and the performance of the box-shaped parts, in actual applications, the complexity of the die structure increases the cost of manufacturing and maintenance, and when dealing with more complex geometries and high-strength materials, there are still challenges in forming accuracy and die life.

[0005] The above-mentioned existing technologies have made certain progress in improving material properties and mold cooling efficiency, but they still have the following limitations. When processing high-strength materials, the existing technologies are difficult to effectively control material rebound, which affects the dimensional accuracy of the finished product. Under high temperature and high pressure environments, the mold is prone to wear or deformation, resulting in a short life, frequent maintenance, and increased use costs. The forming accuracy of complex geometric shapes is difficult to guarantee, especially in the hot stamping forming of high-strength materials, the mold accuracy requirements are more stringent. Summary of the invention

[0006] In view of the above-mentioned prior art, the technical problem to be solved by the present invention is how to effectively control the springback of the material, improve the durability of the mold and enhance the forming accuracy.

[0007] To solve the above problems, the present invention provides an ultra-high-strength steel hot stamping mold, including a cavity, a core is provided at the top of the cavity, a material to be stamped is provided between the cavity and the core, a core cooling block is slidably connected to the top of the core, a plurality of cooling tubes are fixedly connected in the cavity, and the plurality of cooling tubes are arranged in the cavity along with the mold, a groove is provided at the top of the core, a plurality of micropores are provided on the core, the plurality of micropores all penetrate the core and are connected with the groove, an induction heating tube is provided at the corner of the outer end of the core, a thermal expansion layer is fixedly connected to the end of the thermal expansion layer away from the core, a micro-motion core is fixedly connected to the end of the thermal expansion layer away from the core, the thermal expansion layer and the micro-motion core are both slidably connected to the core, through holes connected to the micropores are provided at positions corresponding to the micropores on the induction heating tube, the thermal expansion layer and the micro-motion core, a cooling channel is provided in the induction heating tube, and a cooling cavity is provided in the core cooling block.

[0008] In the above-mentioned ultra-high-strength steel hot stamping die, by adopting a design combining induction heating with a thermal expansion layer, it is possible to effectively eliminate material stress and reduce springback during the hot stamping process, thereby ensuring the dimensional accuracy of the finished product. By optimizing the design of the cooling system and adopting a structure of a cooling cavity, cooling pipe and partition, the cooling efficiency of the die is improved, excessive wear of the die during high-temperature operation is avoided, and the service life of the die is extended. The die adopts a secondary stamping and air film lubrication design, which can reduce friction during the stamping process, improve the surface finish and geometric accuracy of the finished product, and is suitable for the precision forming of complex shapes and high-strength materials.

[0009] As a further improvement of the present application, a partition is fixedly connected to the center of the cooling chamber, and the bottom end of the partition is three to five centimeters away from the inner wall of the cooling chamber. Cooling pipes are fixedly connected to both ends of the core cooling block, and the cooling pipes are connected to the external cooling system. Multiple cooling pipes are also connected to the external cooling system.

[0010] As a further improvement of the present application, a lubrication tube is fixedly connected to the center of the core cooling block in the vertical direction. The lubrication tube runs through the core cooling block. The bottom end of the lubrication tube is flush with the bottom end of the core cooling block. The top end of the lubrication tube is connected to an external feeding system, and the external feeding system is used to provide graphite powder.

[0011] As a further improvement of the present application, the outer end of the core is fixedly connected to a limit block, the induction heating tube passes through the limit block and the passing part is connected to an external cooling system.

[0012] As another improvement of the present application, a cooling block baffle is provided at the top contacting the core cooling block, the top of the cooling block baffle is fixedly connected to the power part of the press, the bottom of the cooling block baffle is fixedly connected to a cooling block fixing plate, the cooling block fixing plate is used to fix the core cooling block, and a plurality of guide pillars are fixedly connected between the cooling block baffle and the cooling block fixing plate.

[0013] As another improved supplement of the present application, a core baffle is fixedly connected to the top end of the core, a core fixing plate is fixedly connected to the bottom end of the core baffle, a through groove matching the outer end of the core cooling block is provided at corresponding positions of the core baffle and the core cooling block, and the core baffle and the core fixing plate are both slidably connected to a plurality of guide columns.

[0014] As another improvement supplement of the present application, a cavity baffle is clamped on the outer end of the cavity, and a cavity pressure plate is fixedly connected to the bottom end of the cavity baffle, the cavity baffle and the cavity pressure plate are slidably connected to a plurality of guide pillars, a cavity fixing plate is fixedly connected to the bottom end of the cavity, the bottom end of the cavity fixing plate is fixedly connected to the fixed part of the press, and the cavity fixing plate is slidably connected to the plurality of guide pillars.

[0015] As another improvement of the present application, the induction heating tube is made of pure copper, and the thermal expansion layer is made of thermostrictive material for expanding its volume when heated. A one-way valve is fixedly connected to the top of the lubrication tube, and the conduction direction of the one-way valve is from the top of the lubrication tube to the bottom of the lubrication tube.

[0016] A method for using an ultra-high strength steel hot stamping die, the method comprising the following steps:

[0017] S1: Place the material to be stamped in the cavity, and use the power part of the press to push the cooling block baffle and the core cooling block downward until the core cooling block abuts against the inner wall of the core. Then the core cooling block pushes the core downward through tight cooperation. At this time, the cooling block baffle, the core cooling block and the core move downward together to gradually press the material to be stamped into the cavity. When the material to be stamped abuts against the core, the core cooling block continues to move downward, squeezing the gas between the core and the core cooling block, and ejecting the gas through the micropores to form an air film between the outer end of the core and the material to be stamped.

[0018] S2: After completing the first step of stamping, the core is lifted by one to two centimeters, and the core cooling block is lifted to the top of the core at the same time. Graphite powder is sprayed between the core and the core cooling block through the lubrication pipe using high-pressure gas. The cooling block baffle, the core cooling block and the core are pushed downward by the power part of the press again to perform the second stamping. The graphite powder plays a lubricating role in this process.

[0019] S3: The core cooling block continues to move downward, squeezing the gas between the core and the core cooling block, squeezing the graphite powder between the outer end of the core and the material to be punched, ensuring the lubrication effect of the material.

[0020] S4: Start the induction heating tube to heat the material to be stamped. The heat is transferred to the thermal expansion layer through the micro-motion core. The thermal expansion layer expands due to the heat and pushes the micro-motion core to squeeze the corner area of ​​the material to be stamped, eliminate the stress in this area, and reduce the rebound of the material to be stamped.

[0021] S5: Then, coolant is introduced into the cooling tube 1, the induction heating tube and the cooling cavity to cool the mold and the material to be stamped, thereby completing the forming process of the stamping material.

[0022] In summary, this application has the following beneficial effects:

[0023] 1. Efficient cooling and operational stability. The cooling system of the mold achieves efficient cooling through the design of the cooling cavity, cooling pipes and partitions. The coolant is evenly distributed in the cooling cavity to ensure that the core cooling block is quickly cooled during operation to prevent mold deformation. The connection between the cooling pipe and the external cooling system further improves the cooling efficiency and extends the service life of the mold. The reasonable design of the cooling block baffle, cooling block fixing plate, core baffle and cavity fixing plate ensures the structural strength and operational stability of the mold under high temperature and high pressure environment and avoids operational errors.

[0024] 2. Precise lubrication and surface protection. The lubrication system of the mold is connected to the external feeding system through a lubrication pipe. Graphite powder is sprayed in with high-pressure gas to form a uniform lubrication layer between the core and the material to be stamped. Graphite powder reduces the friction between the core and the material during the stamping process, protects the surface quality of the material, and improves the smoothness and forming accuracy of the stamping. The air film formed by the gas spraying through the micropores further reduces the friction on the material surface and prevents surface damage caused by direct contact.

[0025] 3. Material stress elimination and springback control. During the stamping process, the induction heating tube heats the material, and the heat is transferred to the thermal expansion layer through the micro-motion core. The thermal expansion layer expands in volume after being heated, pushing the micro-motion core to squeeze the corner area of ​​the material to be stamped, effectively eliminating the stress at the corner of the material. This design greatly reduces the springback phenomenon of the material after stamping, ensuring the dimensional accuracy and structural strength of the finished product, and is particularly suitable for stamping high-strength materials.

[0026] 4. Secondary stamping improves forming accuracy. The mold is designed with a secondary stamping step. After the initial stamping, the core and core cooling block move upward and spray graphite powder, and then move downward again for secondary stamping. The secondary stamping and lubrication of graphite powder further improve the forming accuracy of the material, so that the material is fully lubricated and protected during the stamping process, and the accuracy and surface quality of the final product are significantly improved.

[0027] 5. Strong adaptability and enhanced durability. Through the material selection and structural optimization of the induction heating tube, thermal expansion layer, lubrication tube and cooling chamber, this mold not only adapts to operating environments of different temperatures and pressures, but also significantly enhances its durability. The induction heating tube made of pure copper and the thermal expansion layer made of thermostrictive material ensure that the mold maintains excellent operating performance when processing high-difficulty materials such as ultra-high-strength steel, extends the service life of the mold, and reduces maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the overall structure diagram of this application;

[0029] Figure 2 This is an overall exploded view of this application;

[0030] Figure 3 Partial explosion for this application Figure 1 ;

[0031] Figure 4 Partial explosion for this application Figure 2 ;

[0032] Figure 5 Partial explosion for this application Figure 3 ;

[0033] Figure 6 Partial explosion for this application Figure 4 ;

[0034] Figure 7 This is the front view of the application;

[0035] Figure 8 For this application Figure 7 Middle AA section view;

[0036] Fig. 9 For this application Figure 8 Middle BB section view;

[0037] Fig.10 For this application Figure 8 Enlarged view of point C in the middle;

[0038] Fig.11 This is the appearance structure diagram of this application.

[0039] Description of the numbers in the figure:

[0040] 1. Cavity; 2. Core; 3. Core cooling block; 4. Cooling tube 1; 5. Groove; 6. Micropore; 7. Induction heating tube; 8. Thermal expansion layer; 9. Micro-motion core; 10. Cooling cavity; 11. Partition; 12. Lubrication tube; 13. Limit block; 14. Cooling block baffle; 15. Cooling block fixing plate; 16. Guide column; 17. Core baffle; 18. Core fixing plate; 19. Cavity fixing plate; 20. Cavity baffle; 21. Cavity pressure plate. DETAILED DESCRIPTION

[0041] Three embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0042] Example 1

[0043] like Figures 1 to 11As shown, this embodiment provides an ultra-high strength steel hot stamping die, which includes the following main components:

[0044] The cavity 1 is the main molding space of the mold, which is used to place the material to be stamped. The outer end of the cavity 1 is clamped with a cavity baffle 20, and the bottom end of the cavity baffle 20 is fixedly connected with a cavity pressure plate 21. The cavity baffle 20 and the cavity pressure plate 21 are both slidably connected to a plurality of guide pillars 16, so that the cavity 1 has good positioning and stability during the molding process.

[0045] The core 2 is a sliding component arranged at the top of the cavity 1 and is responsible for punching the material to be punched. A groove 5 is arranged at the top of the core 2 and the groove 5 is connected to the outside of the core 2 through a plurality of micropores 6. These micropores 6 are used for exhausting air during the punching process.

[0046] The core cooling block 3 is slidably connected to the top of the core 2 and moves in coordination with the core 2 during the stamping process to cool the core 2. A cooling cavity 10 is provided in the core cooling block 3, and the cooling cavity 10 can be connected to an external cooling system to achieve efficient cooling.

[0047] A plurality of cooling tubes 4 are arranged in the mold cavity 1 and arranged along the mold to ensure that the temperature of the mold cavity 1 can be effectively controlled.

[0048] The induction heating tube 7 is located at the corner of the outer end of the core 2, and heats the stamping material by induction heating. The far end of the induction heating tube 7 is fixedly connected to a thermal expansion layer 8, and the thermal expansion layer 8 is further connected to the micro-motion core 9. A cooling channel is provided in the induction heating tube 7, and is cooled by an external cooling system.

[0049] The outer end of the core 2 is fixedly connected with a limit block 13, and the induction heating tube 7 passes through the limit block 13 and is connected to the external cooling system through the passing part, so as to ensure the stability of the position and function of the induction heating tube 7 during the stamping process.

[0050] The top end of the core 2 is fixedly connected to a core baffle 17, the bottom end of the core baffle 17 is fixedly connected to a core fixing plate 18, a through groove matching the outer end of the core cooling block 3 is provided at the position corresponding to the core baffle 17 and the core cooling block 3, the core baffle 17 and the core fixing plate 18 are both slidably connected to a plurality of guide columns 16 to ensure that the core 2 remains stable during the stamping process and can accurately adjust its position.

[0051] Working process

[0052] Material positioning and preliminary stamping: the material to be stamped is placed in the cavity 1, and the core 2 starts to move downward to stamp the material for the first time. During this process, the core cooling block 3 moves with the core 2, and the cooling cavity 10 in the core cooling block 3 effectively cools the core 2 to prevent the mold from being damaged due to high temperature.

[0053] Air film formation and lubrication: During the stamping process, the core cooling block 3 continues to move downward, squeezing the gas between the core 2 and the core cooling block 3, so that the gas is ejected from the groove 5 through the micropores 6 to form an air film, thereby reducing the friction between the core 2 and the material and ensuring the surface quality of the material.

[0054] Secondary stamping and stress elimination: after the stamping is completed, the core 2 moves upward by 1 to 2 cm, and the core cooling block 3 also moves upward to the top of the core 2. Then, graphite powder is sprayed in using the lubrication system, and the core 2 is started to move downward again for the second stamping. At this time, the induction heating tube 7 starts to work, heating the material to a predetermined temperature, and the heat is transferred to the thermal expansion layer 8 through the micro-motion core 9. The thermal expansion layer 8 expands after being heated, pushing the micro-motion core 9 to extrude the corner position of the material, eliminating stress and reducing the rebound of the material.

[0055] After the final cooling, heating and secondary stamping are completed, coolant is introduced into the mold through the cooling tube 1 4, the induction heating tube 7 and the cooling cavity 10 to perform the final cooling step to ensure that the material is set and the hot stamping process is completed.

[0056] Precise control and stability. Through the design of the core baffle 17, the core fixing plate 18 and the limit block 13, the stability of the mold during the stamping process is greatly enhanced. The sliding connection of the guide column 16 ensures the positioning accuracy of the core 2 and the cavity 1 under high temperature and high pressure environment.

[0057] Efficient cooling and stress elimination, the combined design of the induction heating tube 7, the thermal expansion layer 8 and the micro-motion core 9 can effectively heat the material while eliminating the material stress through the thermal expansion effect, reduce rebound and improve the molding quality. The design of the cooling cavity 10 and the cooling tube 4 ensures that the mold can be cooled quickly after high-temperature operation, thereby extending the service life of the mold.

[0058] Air film lubrication and material protection: gas is ejected through the micropores 6 to form an air film, which effectively reduces the direct contact between the core 2 and the material during the stamping process, reduces friction, and protects the surface quality of the material. At the same time, the molding accuracy of the material is improved through secondary lubrication stamping.

[0059] To sum up, the ultra-high strength steel hot stamping die of this embodiment can complete the stamping operation efficiently and stably under high temperature and high pressure environment through carefully designed structure and work flow, and shows significant advantages in material stress elimination, springback control and surface quality protection.

[0060] Example 2

[0061] like Figures 1 to 11As shown, based on Example 1, Example 2 further optimizes the cooling system, lubrication system and structural stability of the mold, and the embodiment includes the following key components:

[0062] A partition 11 is fixedly connected to the center of the cooling cavity 10 in the core cooling block 3. The bottom end of the partition 11 is three to five centimeters away from the inner wall of the cooling cavity 10. This design divides the internal flow path of the cooling cavity 10 by the partition 11, so that the coolant can flow more evenly in the cooling cavity 10, thereby improving the cooling efficiency. Cooling pipes are fixedly connected to both ends of the cooling cavity 10. These cooling pipes are connected to the external cooling system to maintain the low temperature state of the core cooling block 3 and avoid deformation of the mold due to high-temperature stamping.

[0063] A lubrication pipe 12 is fixedly connected to the center of the core cooling block 3 in the vertical direction. The lubrication pipe 12 passes through the core cooling block 3, and the bottom end is flush with the bottom end of the core cooling block 3. The top end of the lubrication pipe 12 is connected to an external feeding system, and the external feeding system is used to provide graphite powder. A one-way valve is also fixedly connected to the top end of the lubrication pipe 12. The conduction direction of the one-way valve is from the top end of the lubrication pipe 12 to the bottom end, ensuring that the graphite powder can flow smoothly from the top end of the lubrication pipe 12 to the bottom end during the lubrication process and enter the working area of ​​the mold.

[0064] The top of the cooling block baffle 14 is fixedly connected to the power part of the press, the top of the core cooling block 3 is contacted with the cooling block baffle 14, and the bottom of the cooling block baffle 14 is fixedly connected to a cooling block fixing plate 15 for fixing the relative position of the core cooling block 3 to ensure the stability of the core cooling block 3 during the stamping process. A plurality of guide columns 16 are fixedly connected between the cooling block baffle 14 and the cooling block fixing plate 15, and these guide columns 16 ensure the stability of the core cooling block 3 while allowing necessary sliding between the core cooling block 3 and the core 2.

[0065] The induction heating tube 7 is made of pure copper and has good thermal conductivity, which makes the heating efficiency high and stable. The thermal expansion layer 8 is made of thermostrictive material, which expands in volume when heated, and effectively transfers pressure to the micro-motion core 9, which is used to accurately control the stress elimination at the corners of the material to be stamped and reduce springback. The bottom end of the cavity 1 is fixedly connected with a cavity fixing plate 19, which is used to further enhance the overall structural strength and stability of the cavity 1. The bottom end of the cavity fixing plate 19 is connected to the fixed part of the press, and the cavity fixing plate 19 is slidably connected to multiple guide pillars 16.

[0066] Working process

[0067] Optimized application of the cooling system. During the stamping process, the core cooling block 3 is connected to the external cooling system through a cooling pipe. The coolant flows in the cooling cavity 10 and is separated by the partition 11 to ensure that the coolant is evenly distributed in different areas of the cooling cavity 10, thereby improving the cooling efficiency of the core cooling block 3 and avoiding mold failure due to local overheating.

[0068] Operation of the lubrication system: After the initial stamping is completed, the core cooling block 3 moves upward together with the core 2, and graphite powder is sprayed into the gap between the core 2 and the core cooling block 3 through the lubrication pipe 12. The graphite powder enters the lubrication pipe 12 smoothly through the one-way valve from the external feeding system, and is sprayed into the stamping area under the push of high-pressure gas. This process greatly reduces the friction between the core 2 and the material to be stamped, and improves the surface quality of the material.

[0069] Stability of the cooling block and the guide column. During the stamping process, the guide column 16 is fixedly connected between the cooling block baffle 14 and the cooling block fixing plate 15, ensuring the relative stability of the core cooling block 3 under high temperature and high pressure environment. The guide column 16 allows necessary sliding adjustments during the cooling process, but at the same time maintains the structural strength and stability of the entire mold.

[0070] Efficient heating and precise control. The induction heating tube 7 is made of pure copper and can heat the material to be stamped efficiently and evenly. After the thermal expansion layer 8 is heated, the micro-motion core 9 applies pressure to the corners of the material to eliminate stress and avoid unnecessary rebound of the material during the cooling process, thereby ensuring the accuracy and strength after forming.

[0071] The cooling efficiency is significantly improved. By arranging the partition 11 in the cooling cavity 10, the flow path of the coolant is made more reasonable, which effectively improves the efficiency of the cooling system and ensures the long-term and stable operation of the mold under high temperature conditions.

[0072] The precise control of the lubrication system, the combination of the lubrication pipe 12 and the external feeding system, and the control of the flow direction of the graphite powder by the one-way valve ensure the lubrication effect, reduce the wear of the mold and the material, extend the mold life and improve the product quality.

[0073] The structural strength and stability are enhanced, and the combined design of the cooling block baffle 14, the cooling block fixing plate 15 and the guide column 16 greatly improves the stability of the core cooling block 3, avoiding structural loosening or deformation caused by high temperature or high pressure during the stamping process.

[0074] The optimization of material selection and operation accuracy, the use of the induction heating tube 7 of pure copper material and the thermal expansion layer 8 of thermostrictive material improve the heating efficiency and control accuracy, so that the mold can maintain excellent operating performance when processing ultra-high-strength steel materials, ensuring the dimensional accuracy and mechanical properties of the finished product.

[0075] In summary, Example 2 further optimizes the cooling and lubrication system of the mold on the basis of Example 1, and achieves a more efficient and precise stamping process through improvements in material selection and structural design, providing more reliable technical support for the forming of ultra-high-strength steel materials.

[0076] Example 3

[0077] like Figures 1 to 11 As shown, based on Example 1 and Example 2, Example 3 further describes in detail the specific use method and operation steps of the mold, especially the operations at various stages of the stamping process.

[0078] S1: Material placement and initial punching

[0079] The material to be punched is placed at the top of the cavity 1. At this time, the cooling block baffle 14 and the core cooling block 3 are pushed downward by the power part of the press until the core cooling block 3 is against the inner wall of the core 2. Then the core cooling block 3 pushes the core 2 downward through a tight fit. At this time, the cooling block baffle 14, the core cooling block 3 and the core 2 move downward together to gradually press the material to be punched into the cavity 1. When the material to be punched is against the core 2, the core cooling block 3 continues to move downward to squeeze the gas between the core 2 and the core cooling block 3. The gas is ejected through the micropores 6 on the core 2 to form a layer of air film between the outer end of the core 2 and the material to be punched. This layer of air film reduces friction and protects the surface quality of the material.

[0080] S2: Lifting and lubrication preparation

[0081] After completing the first stamping, the core 2 moves upward by 1 to 2 centimeters, and the core cooling block 3 also moves upward to the top position of the core 2. At this time, graphite powder is sprayed between the core 2 and the core cooling block 3 through the lubrication tube 12. The lubrication tube 12 provides graphite powder through an external feeding system and uses high-pressure gas to spray the graphite powder evenly. This step prepares lubrication for the secondary stamping and effectively reduces the friction between the core 2 and the material to be stamped.

[0082] S3: Secondary stamping and lubrication

[0083] The cooling block baffle 14, the core cooling block 3 and the core 2 are pushed downward together by the power part of the press again for the second stamping. At this time, the graphite powder acts as a lubricant to further reduce the friction during the stamping process, improve the smoothness of the stamping and the forming accuracy of the material. The core cooling block 3 continues to move downward and squeezes the gas between the core 2 and the core cooling block 3 again, squeezing the graphite powder between the outer end of the core 2 and the material to be stamped, ensuring that the material is fully lubricated during the stamping process.

[0084] S4: Induction Heating and Stress Relief

[0085] After the secondary stamping is completed, the induction heating tube 7 is started to heat the material to be stamped. The induction heating tube 7 is made of pure copper and has efficient thermal conductivity. It can quickly and evenly heat the material to be stamped. As the material is heated, the heat is transferred to the thermal expansion layer 8 through the micro-motion core 9. The thermal expansion layer 8 is made of thermostrictive material. After being heated, its volume expands, pushing the micro-motion core 9 to squeeze the corner area of ​​the material to be stamped. This process effectively eliminates the stress at the corner of the material, reduces the material rebound, and ensures the accuracy and strength after forming.

[0086] S5: Final Cooldown

[0087] After heating is completed, coolant is introduced into the cooling tube 4, the induction heating tube 7 and the cooling cavity 10 to cool the mold and the material to be stamped. This step quickly reduces the temperature of the mold and the material, completes the shaping process of the material, and ensures the high-quality output of the finished product.

[0088] When in use, the material to be punched is placed at the top of the cavity 1, and then the cooling block baffle 14, the core cooling block 3 and the core 2 are pushed downward by the power part of the press, and the core 2 punches the material to be punched during the movement. During this process, the core cooling block 3 continues to move downward, squeezing the gas between the core 2 and the core cooling block 3, so that the gas is ejected from the micropores 6, and the gas forms an air film between the outer end of the core 2 and the material to be punched;

[0089] After the core 2 is stamped, the core 2 is moved upward by one to two centimeters, and the core cooling block 3 is moved upward to the top of the core 2. Graphite powder is sprayed between the core 2 and the core cooling block 3 by high-pressure gas through the lubrication pipe 12, and the cooling block baffle 14, the core cooling block 3 and the core 2 are pushed downward by the power part of the press again to perform secondary stamping on the stamped material, and the graphite powder plays a lubricating role;

[0090] During the continuous downward movement of the core cooling block 3, the gas between the core 2 and the core cooling block 3 is squeezed, and the graphite powder is squeezed into between the outer end of the core 2 and the material to be stamped;

[0091] Then, the material to be stamped is inductively heated by the induction heating tube 7. When the material to be stamped is heated, the heat is transferred to the thermal expansion layer 8 through the micro-motion core 9. The thermal expansion layer 8 expands in volume after being heated, and pushes the micro-motion core 9 to squeeze the corner position of the material to be stamped, thereby eliminating the corner stress of the material to be stamped and reducing the springback of the material to be stamped.

[0092] After the stress of the material to be stamped is eliminated, coolant is introduced into the cooling tube 1 4, the induction heating tube 7 and the cooling cavity 10 to cool the mold and the material to be stamped.

[0093] Air film formation and surface protection: During the initial stamping process, the gas ejected from the micropores 6 forms an air film between the outer end of the core 2 and the material to be stamped, which reduces the friction on the material surface during the stamping process, protects the surface quality of the material, and reduces the damage of the mold to the material.

[0094] Graphite powder lubrication and stamping accuracy. The graphite powder sprayed through the lubrication tube 12 effectively reduces the friction between the core 2 and the material to be stamped. Especially in the secondary stamping process, the lubrication effect of the graphite powder significantly improves the molding accuracy of the material and reduces the friction resistance during the stamping process.

[0095] Stress elimination and rebound control: the thermal expansion layer 8 expands due to heat under the action of the induction heating tube 7, and the corners of the material are squeezed by the micro-motion core 9, which effectively eliminates the stress inside the material, significantly reduces the rebound phenomenon of the material, and ensures the dimensional accuracy and structural strength of the stamped product.

[0096] Efficient cooling and material protection. After stamping is completed, coolant is injected in time for cooling. The cooling pipe 4 and the induction heating pipe 7 work together to quickly reduce the temperature of the mold and the material, ensuring that the material will not undergo secondary deformation in the state, while extending the service life of the mold.

[0097] Example 3 provides an efficient, precise and controllable hot stamping method through optimized operating steps. This method not only improves the working efficiency of the mold, but also significantly improves the quality and precision of the finished product. It is particularly suitable for stamping and forming highly difficult materials such as ultra-high strength steel.

[0098] In view of current practical needs, the above-mentioned implementation mode adopted in this application is not limited to the scope of protection. Various changes made within the knowledge scope of technical personnel in this field without departing from the concept of this application still fall within the scope of protection of the present invention.

Claims

1. An ultra-high strength steel hot stamping die, characterized in that: The mold cavity (1) comprises a mold core (2) at the top of the mold cavity (1), a material to be punched is arranged between the mold cavity (1) and the core (2), a core cooling block (3) is slidably connected to the top of the core (2), a plurality of cooling tubes (4) are fixedly connected in the mold cavity (1), and the plurality of cooling tubes (4) are arranged in the mold cavity (1), a groove (5) is provided at the top of the core (2), a plurality of micropores (6) are provided on the core (2), and the plurality of micropores (6) all penetrate the core (2) and are connected to the groove (5), an induction heating tube (7) is provided at the corner of the outer end of the core (2), a heat expansion layer (8) is fixedly connected to the end of the heat expansion layer (8) away from the core (2), and a micro-movement core (9) is fixedly connected to the end of the heat expansion layer (8) away from the core (2). The thermal expansion layer (8) and the micro-motion core (9) are both slidably connected to the core (2); through holes connected to the micro-holes (6) are provided at positions corresponding to the micro-holes (6) on the induction heating tube (7), the thermal expansion layer (8) and the micro-motion core (9); a cooling channel is provided in the induction heating tube (7); a cooling cavity (10) is provided in the core cooling block (3); a cooling block baffle (14) is provided at the top end of the core cooling block (3); the top end of the cooling block baffle (14) is fixedly connected to the power part of the press; the bottom end of the cooling block baffle (14) is fixedly connected to a cooling block fixing plate (15); the cooling block fixing plate (15) is used to fix the core cooling block (3); a plurality of guide pillars (16) are fixedly connected between the cooling block baffle (14) and the cooling block fixing plate (15).

2. The ultra-high strength steel hot stamping die according to claim 1, characterized in that: A partition (11) is fixedly connected to the center of the cooling chamber (10), and the bottom end of the partition (11) is three to five centimeters away from the inner wall of the cooling chamber (10). Cooling pipes are fixedly connected to both ends of the core cooling block (3), and the cooling pipes are connected to an external cooling system. The plurality of cooling pipes (4) are also connected to the external cooling system.

3. The ultra-high strength steel hot stamping die according to claim 1, characterized in that: A lubrication pipe (12) is fixedly connected to the center of the core cooling block (3) in a vertical direction, the lubrication pipe (12) passes through the core cooling block (3), the bottom end of the lubrication pipe (12) is flush with the bottom end of the core cooling block (3), and the top end of the lubrication pipe (12) is connected to an external feeding system, and the external feeding system is used to provide graphite powder.

4. The ultra-high strength steel hot stamping die according to claim 1, characterized in that: The outer end of the core (2) is fixedly connected to a limiting block (13), the induction heating tube (7) passes through the limiting block (13), and the passing portion is connected to an external cooling system.

5. The ultra-high strength steel hot stamping die according to claim 1, characterized in that: The top end of the core (2) is fixedly connected to a core baffle (17), the bottom end of the core baffle (17) is fixedly connected to a core fixing plate (18), a through groove matching the outer end of the core cooling block (3) is provided at corresponding positions of the core baffle (17) and the core cooling block (3), and the core baffle (17) and the core fixing plate (18) are both slidably connected to a plurality of guide pillars (16).

6. The ultra-high strength steel hot stamping die according to claim 1, characterized in that: The outer end of the cavity (1) is clamped with a cavity baffle (20), and the bottom end of the cavity baffle (20) is fixedly connected to a cavity pressure plate (21), the cavity baffle (20) and the cavity pressure plate (21) are slidably connected to a plurality of guide pillars (16), the bottom end of the cavity (1) is fixedly connected to a cavity fixing plate (19), the bottom end of the cavity fixing plate (19) is fixedly connected to a fixed part of a press, and the cavity fixing plate (19) is slidably connected to a plurality of guide pillars (16).

7. The ultra-high strength steel hot stamping die according to claim 3, characterized in that: The induction heating tube (7) is made of pure copper, the thermal expansion layer (8) is made of a thermostrictive material and is used to expand in volume when heated, and a one-way valve is fixedly connected to the top end of the lubrication tube (12), and the conduction direction of the one-way valve is from the top end of the lubrication tube (12) to the bottom end of the lubrication tube (12).

8. The method for using an ultra-high strength steel hot stamping die according to any one of claims 1 to 7, characterized in that: How to use it The steps include: S1: placing the material to be stamped in the mold cavity (1), and pushing the cooling block baffle (14) and the core cooling block (3) downwards through the power part of the press until the core cooling block (3) abuts against the inner wall of the core (2), and then the core cooling block (3) pushes the core (2) downwards through a tight fit, and at this time, the cooling block baffle (14), the core cooling block (3) and the core (2) move downwards together to gradually press the material to be stamped into the mold cavity (1), and when the material to be stamped abuts against the core (2), the core cooling block (3) continues to move downwards, squeezing the gas between the core (2) and the core cooling block (3), and ejecting the gas through the micropores (6), forming an air film between the outer end of the core (2) and the material to be stamped; S2: After the first step of stamping is completed, the core (2) is lifted by one to two centimeters, and the core cooling block (3) is lifted to the top of the core (2). Graphite powder is sprayed between the core (2) and the core cooling block (3) through the lubrication pipe (12) using high-pressure gas. The cooling block baffle (14), the core cooling block (3) and the core (2) are pushed downward by the power part of the press again to perform a second stamping. The graphite powder plays a lubricating role in this process. S3: the core cooling block (3) continues to move downward, squeezing the gas between the core (2) and the core cooling block (3), squeezing the graphite powder between the outer end of the core (2) and the material to be punched, and ensuring the lubrication effect of the material; S4: starting the induction heating tube (7) to heat the material to be stamped, and transferring the heat to the thermal expansion layer (8) through the micro-motion core (9). The thermal expansion layer (8) expands due to the heat and pushes the micro-motion core (9), thereby squeezing the corner area of ​​the material to be stamped, eliminating the stress in the area, and reducing the springback of the material to be stamped; S5: Cooling liquid is then introduced into the cooling tube 1 (4), the induction heating tube (7) and the cooling cavity (10) to cool the mold and the material to be stamped, thereby completing the forming process of the stamping material.

Citation Information

Patent Citations

  • A hot stamping and deep drawing die for ultra-high strength steel box-shaped parts

    CN107008809B

  • A method for continuous online preparation of ultra-high strength and toughness Mn-B steel structural parts

    CN109762965B

  • Molding mold for V-shaped rib of stator frame of electric generator

    CN101716630A

  • Die water circulation system and machining system for hot punching forming special-shaped plate

    CN108176766A

  • Needling machine damping device, and machining equipment of device assembly

    CN111636153A