Method for improving wear resistance of 3D printing 2205 duplex stainless steel
By adding TiB2 particles to 3D printed 2205 duplex stainless steel and adopting ball milling treatment and specific process parameters, the problem of insufficient wear resistance is solved, the wear resistance of the parts is improved, the friction coefficient is reduced, and the overall and Local reinforcement strategies improve the performance of the parts.
Patent Information
- Application Number
- CN202411065433.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The wear resistance of 3D printed 2205 duplex stainless steel parts is poor, making it difficult to perform real-time regulation during SLM forming, affecting its application effect.
Integral strengthening and local strengthening, TiB2 particles are added and ball milled to adhere to the surface of 2205 duplex stainless steel powder, combining specific 3D printing process parameters and scanning strategies, including argon protection, ball milling process and nerves The powder ratio calculated by the network algorithm achieves the improvement of wear resistance of the parts.
The average friction coefficient is significantly reduced from 0.7142 to 0.4305, which improves the wear resistance of the parts, and prevents particles from peeling during wear through uniform dispersion and firm interface combination, thereby improving the surface and internal properties of the parts.
Smart Images

Figure CN118893220A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials and relates to a method for improving the wear resistance of 3D printed 2205 duplex stainless steel. Background Art
[0002] Compared with austenitic stainless steel, 2205 duplex stainless steel is composed of ferrite (δ) and austenite (γ), and has the characteristics of high strength, good toughness and corrosion resistance. It is widely used in medical devices, automotive parts, ship fasteners and other fields. With the new round of scientific and technological revolution and industrial revolution sweeping in, complexity, miniaturization and precision have become a significant development trend. As one of the most promising additive manufacturing technologies, metal 3D technology is based on the forming principle of layered manufacturing, using laser beam to melt the selected area layer by layer to achieve part forming. It can be used to manufacture metal parts with complex shapes, good mechanical properties, high precision and relative density close to 100%. However, due to the properties of 2205 duplex stainless steel and the limitations of metal 3D technology, the wear resistance of 3D printed 2205 duplex stainless steel parts is often poor. Therefore, how to control the wear resistance in real time during the SLM forming process and avoid or reduce the post-processing of parts has become a major challenge in the field of metal additive manufacturing. Summary of the invention
[0003] The purpose of the present invention is to improve the wear resistance of 3D printed 2205 duplex stainless steel to meet the requirements of 2205 duplex stainless steel in actual use.
[0004] The present invention proposes a method for improving the wear resistance of 3D printed 2205 duplex stainless steel, which adopts two methods: overall strengthening and local strengthening. The 3D printing method adopts a scraper powder feeding method to print. Before printing, an appropriate amount of TiB2 particles are added to the 2205 duplex stainless steel powder, and the particles are attached to the surface of the 2205 duplex stainless steel powder by ball milling, and then the printing preparation is performed; before mixing the powder, the powder needs to be vacuum dried in a vacuum box, and the temperature is controlled at 90-120℃ for 2-4 hours and dried for 6-8 hours. The amount of TiB2 added is controlled within the range of 1% to 15% of the total mass, the particle size of TiB2 is controlled at 1-5 microns, and the particle size of the 2205 duplex stainless steel powder is controlled at 12-53 microns. The ball-to-material mass ratio is 2:1, the total weight of the two is 6kg, the speed of the ball mill is 150-250 rpm, argon is used for protection during ball milling to prevent powder oxidation, the ball milling time is 400-500 minutes, and the ball milling mixing powder is changed after every half an hour and stopped for 5 minutes.
[0005] For the overall strengthening printing method, that is, all the printed parts are prepared by mixed powder with TiB2 strengthening particles, the printing particle size is controlled below 53 microns, the atmosphere is argon atmosphere, and the process parameters are as follows: the laser power is controlled within the range of 210-290W, the scanning speed is 600-1000mm / s, the scanning overlap rate is 33%, and the internal and external contour scanning strategy adopts multi-contour scanning, and the number of scans is 2. The internal scanning line scanning strategy adopts zigzag scanning, and the scanning angle is rotated 30° on the basis of the previous layer, that is, the scanning direction of the adjacent two layers is 30°, alternating, and the layer thickness is controlled at 0.03 microns. During printing, the concentration of the high-precision oxygen sensor is controlled to be maintained below 800ppm, and the air pressure in the cavity is maintained at 2.0-2.5kPa.
[0006] For the internal and external contour scanning strategy, multi-contour scanning is adopted, and the number of scans is 2, that is, the internal and external contour scanning is based on the original one, and the number of scans is added to the inner circle to change the distribution of the melt channel at the boundary and improve the surface boundary performance of the part. The internal scanning line scanning strategy adopts zigzag scanning to make the adjacent melt channels in opposite directions to improve the internal surface performance of the part. The scanning angle is rotated 30° based on the previous layer, that is, the scanning directions of the adjacent two layers are 30°, and they are performed alternately to reduce the accumulation of thermal stress.
[0007] For the local strengthening printing method, heterogeneous powder printing can be used to achieve the effect of gradient strengthening, that is, the main body of the printed part is printed with 2205 duplex stainless steel powder, and the surface of the printed part is printed with mixed powder with TiB2 strengthening particles. The printing process parameters are the same as those for overall strengthening. The local strengthening printing method can not only achieve uniform distribution, but also locally strengthen the surface wear resistance, while reducing the amount of mixed powder to improve economic benefits.
[0008] For the local enhanced printing method, a neural network algorithm is used to calculate the amount of 2205 powder required for the printing main body and the amount of 2205-TiB2 mixed powder required for surface enhancement, and the calculated 2205-TiB2 mixed powder is evenly loaded into the bottom of the powder cylinder, and then the 2205 powder is spread on the top of the mixed powder. As the printing progresses, when the 2205 powder used for the printing main body is exhausted, it is automatically converted to printing with 2205-TiB2 mixed powder, thereby achieving local surface enhancement of the printed part.
[0009] Using argon atmosphere for protection, part of TiB2 reacts with laser and melts and decomposes into TiB during the printing process. The generated TiB and the original TiB2 can act as nucleating agents to refine the grains on the one hand, and can act as hard points on the other hand. The uniformly dispersed TiB2 reinforcement shows high adhesion and low fragmentation / fracture during sliding. At the same time, the strong interface between the TiB2 phase and the 2205 matrix prevents the peeling of particles during wear. The wear resistance of 3D printed 2205 duplex stainless steel under the combined action of the two factors. The wear resistance of 3D printed 2205 duplex stainless steel is improved under the combined action of the two factors, and the average friction coefficient is finally reduced from 0.7142 to 0.4305.
[0010] On the basis of the above technical scheme, compared with the prior art, the advantages of the present invention are: (1) ball milling process is adopted and the ball milling process parameters are controlled so that TiB2 particles can be attached to the surface of 2205 duplex stainless steel powder without affecting the sphericity of the powder, so that the two are not easy to separate during the powder spreading process and the phenomenon of uneven powder mixing resulting from uneven spreading distribution is not easy to occur; (2) TiB2 particles are adopted and protected by argon atmosphere. TiB2 can act as a nucleating agent to refine the grains on the one hand and as a hard point on the other hand. The uniformly dispersed TiB2 reinforcement shows high adhesion and low degree of fragmentation / fracture during sliding. At the same time, the strong interface between the TiB2 phase and the 2205 matrix is bonded, thereby preventing the particles from peeling off during wear. The wear resistance of 3D printed 2205 duplex stainless steel under the combined action of the two factors; (3) the internal and external contour scanning strategy adopts multi-contour scanning with a scanning number of 2, that is, the internal and external contour scanning adds one scanning number in the inner circle on the original basis to change the distribution of the melt channel at the boundary and improve the surface boundary performance of the workpiece. The internal scanning line scanning strategy adopts zigzag scanning to make the adjacent melt paths in opposite directions to improve the internal surface performance of the part. The scanning angle is rotated 30° based on the previous layer, that is, the scanning directions of the two adjacent layers are 30°, and they are performed alternately to reduce the accumulation of thermal stress; (4) Both overall strengthening and local strengthening are adopted. When the overall wear resistance of the printed part is required to be high, the overall strengthening method is adopted, and when the wear resistance of the printed part is only required to be high on the surface, the local strengthening method is adopted. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0012] Figure 1is a process flow chart of the present invention; Figure 2 SEM images of metal powder particle size distribution, (A) TiB2 metal powder SEM; (B) 2205 duplex stainless steel powder SEM; (C) ball milled mixed powder SEM; Figure 3 It is a schematic diagram of the internal contour scanning strategy; Figure 4 It is a schematic diagram of the internal scanning line scanning strategy; Figure 5 This is the SEM image of the 2205-TiB2 sample; Figure 6 The wear resistance of 2205 sample and 2205-TiB2 sample is compared; Figure 7 Comparison of wear resistance between 2205 specimen and locally strengthened specimen. DETAILED DESCRIPTION
[0013] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0014] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0015] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0016] In some embodiments, a method of improving the wear resistance of 3D printed 2205 duplex stainless steel of the present invention comprises the following steps: Embodiment 1 Step (1), the dried pure 2205 duplex stainless steel powder and titanium diboride powder (TiB2) are mixed in a mass ratio of 95:5 to obtain a mixed powder 2205-TiB2. TiB2, as a ceramic phase, can significantly improve the wear resistance. Drying removes moisture to avoid oxidation. Preferably, 2205 duplex stainless steel with a powder particle size distribution of 15-53 μm is used to prepare the powder by gas atomization (such as Figure 2 Powder shown in B), titanium diboride powder with a particle size distribution of 1-5 µm (such as Figure 2The ball-to-material mass ratio is 2:1, the total weight of the two is 6 kg, the ball milling speed is 150 rpm, argon is used to protect the powder from oxidation, the ball milling time is 400 minutes, and the ball milling direction is changed every half an hour and stopped for 5 minutes. The ball milling process parameters are controlled so that the TiB2 particles can adhere to the surface of the 2205 duplex stainless steel powder (such as Figure 2 The powder is shown in C in the figure), and the sphericity of the powder is not affected at the same time. In this way, the two are not easy to separate during the powder spreading process, and the uneven distribution caused by uneven mixing of powders is not easy to occur.
[0017] Step (2), for the overall strengthening printing method, the mixed powder is used to prepare the friction and wear specimens using 3D printing technology to achieve overall strengthening of the 2205 specimens. The printing size is 20mm (length) × 10mm (width) × 10mm (height). 3D printing uses selective laser melting (SLM) technology, the laser power is controlled within the range of 210W, the scanning speed is 600 mm / s, the scanning overlap rate is 33%, and the internal and external contour scanning strategy uses multi-contour scanning (such as Figure 3 As shown in the figure, the number of scans is 2, the internal scan line scanning strategy adopts zigzag scanning, and the scanning angle is rotated 30° based on the previous layer, that is, the scanning directions of the two adjacent layers are 30° (as shown in the figure). Figure 4 As shown), the layers are alternately controlled at 0.03 microns. During printing, the concentration of the high-precision oxygen sensor is controlled to be maintained below 800ppm, and the pressure in the cavity is maintained at 2.0-2.5kPa. After printing, samples are taken for friction and wear performance testing. By comparing the friction coefficient curves of the 2205-TiB2 sample with the 2205 sample, the friction coefficient of the 2205-TiB2 sample is significantly reduced, and the wear resistance is significantly improved (as shown in Figure 2). Figure 6 as shown).
[0018] Embodiment 2 Step (1), mixing the dried pure 2205 duplex stainless steel powder and titanium diboride powder (TiB2) at a mass ratio of 95:5 to obtain a mixed powder 2205-TiB2. TiB2, as a ceramic phase, can significantly improve the wear resistance. Drying removes moisture to avoid oxidation. Preferably, 2205 duplex stainless steel with a powder particle size distribution of 15-53 µm is used to prepare the powder by gas atomization, and titanium diboride powder with a particle size distribution of 1-5 µm is used. The ball-to-material mass ratio is 2:1, the total weight of the two is 2 kg, the ball milling speed is 150 rpm, argon is used for protection during ball milling to prevent powder oxidation, the ball milling time is 400 minutes, and the ball milling mixing is changed after every half an hour and stopped for 5 minutes. The ball milling process parameters are controlled so that the TiB2 particles can adhere to the surface of the 2205 duplex stainless steel powder without affecting the sphericity of the powder, so that the two are not easy to separate during the powder spreading process, and the phenomenon of uneven spreading caused by uneven powder mixing is not easy to occur.
[0019] Step (2), for the local strengthening printing method, the neural network algorithm is used to calculate the amount of 2205 powder required for the printing body as 2.3kg and the amount of 2205-TiB2 mixed powder required for surface strengthening as 0.2kg, and the calculated 2205-TiB2 mixed powder is evenly loaded into the bottom of the powder cylinder, and then the 2205 powder is spread on the top of the mixed powder, so that as the printing progresses, when the 2205 powder used for the printing body is exhausted, it is automatically converted to using 2205-TiB2 mixed powder for printing, so as to achieve local strengthening of the surface wear resistance, while reducing the amount of mixed powder to improve economic benefits. The powder is used to prepare friction and wear samples using 3D printing technology to achieve local strengthening of the 2205 sample, and the printing size is 20mm (length) × 10mm (width) × 10mm (height). 3D printing uses selective laser melting (SLM) technology, with laser power controlled within 210W, scanning speed 600 mm / s, scanning overlap rate 33%, multi-contour scanning strategy for internal and external contours, scanning times 2, zigzag scanning strategy for internal scanning lines, and scanning angle rotated 30° on the basis of the previous layer, that is, the scanning directions of two adjacent layers are 30°, alternating, and the layer thickness is controlled at 0.03 microns. During printing, the concentration of the high-precision oxygen sensor is controlled to be maintained below 800ppm, and the air pressure in the cavity is maintained at 2.0-2.5kPa. After printing, samples are taken for friction and wear performance testing. By comparing the friction coefficient curves of the local reinforced sample with those of the 2205 sample, the friction coefficient of the local reinforced sample is significantly reduced, and the wear resistance is significantly improved (such as Figure 7 as shown).
[0020] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel, characterized in that: Two methods of overall strengthening and local strengthening are adopted; the 3D printing method adopts the method of scraper powder feeding. Before printing, an appropriate amount of TiB2 particles are added to the 2205 duplex stainless steel powder, and the particles are attached to the surface of the 2205 duplex stainless steel powder through ball milling, and then the printing preparation is carried out; before mixing the powder, it is necessary to vacuum dry it in a vacuum box, and the temperature is controlled at 90-120℃ for 2-4 hours and dried for 6-8 hours; the amount of TiB2 added is controlled in the range of 1% to 15% of the total mass, the particle size of TiB2 is controlled at 1-5 microns, and the particle size of 2205 duplex stainless steel powder is controlled at 12-53 microns; the ball-to-material mass ratio is 2:1, the ball milling speed is 150-250 rpm, argon is used for protection during ball milling to prevent powder oxidation, the ball milling time is 400-500 minutes, and the ball milling mixing is changed after every half an hour and stopped for 5 minutes.
2. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel as claimed in claim 1, characterized in that: For the overall enhanced printing method, that is, all printed parts are prepared from mixed powders with added TiB2 reinforcing particles, the printing particle size is controlled below 53 microns, the atmosphere uses argon atmosphere, and the process parameters are as follows: the laser power is controlled within the range of 210-290W, the scanning speed is 600-1000mm / s, the scanning overlap rate is 33%, the internal and external contour scanning strategy adopts multi-contour scanning, and the number of scans is 2; the internal scanning line scanning strategy adopts zigzag scanning, and the scanning angle is rotated 30° on the basis of the previous layer, that is, the scanning directions of the two adjacent layers are 30°, alternating, and the layer thickness is controlled at 0.03 microns; during printing, the concentration of the high-precision oxygen sensor is controlled to be maintained below 800ppm, and the air pressure in the cavity is maintained at 2.0-2.5kPa.
3. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel as claimed in claim 2, characterized in that: The inner and outer contour scanning strategy adopts multi-contour scanning with 2 scan times, that is, the inner and outer contour scanning adds one scan time in the inner circle on the original basis to change the distribution of the melt channel at the boundary and improve the surface boundary performance of the part; the internal scanning line scanning strategy adopts zigzag scanning to make the adjacent melt channels in opposite directions to improve the internal surface performance of the part; the scanning angle is rotated 30° on the basis of the previous layer, that is, the scanning directions of the two adjacent layers are 30°, alternating to reduce thermal stress accumulation.
4. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel as claimed in claim 1, characterized in that: For the local strengthening printing method, heterogeneous powder printing is used to achieve the effect of gradient strengthening, that is, the main body of the print is printed with 2205 duplex stainless steel powder, and the surface of the print is printed with mixed powder with TiB2 strengthening particles added. The printing process parameters are the same as those for overall strengthening.
5. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel as claimed in claim 4, characterized in that: For the local enhanced printing method, a neural network algorithm is used to calculate the amount of 2205 powder required for the printing body and the amount of 2205-TiB2 mixed powder required for surface enhancement, and the calculated 2205-TiB2 mixed powder is evenly loaded into the bottom of the powder cylinder, and then the 2205 powder is spread on top of the mixed powder. As the printing progresses, when the 2205 powder used for the printing body is exhausted, it is automatically converted to printing with 2205-TiB2 mixed powder, thereby achieving local surface enhancement of the printed part.
6. A method for improving the wear resistance of 3D printed 2205 duplex stainless steel as claimed in claim 1, characterized in that: Using argon atmosphere for protection, during the printing process, part of the TiB2 reacts with the laser and melts and decomposes into TiB. The generated TiB and the original TiB2 act as nucleating agents to refine the grains on the one hand, and as hard points on the other hand. The uniformly dispersed TiB2 reinforcement shows high adhesion and low degree of fragmentation / fracture during sliding. At the same time, the strong interface between the TiB2 phase and the 2205 matrix prevents the peeling of particles during wear, and finally reduces the average friction coefficient from 0.7142 to 0.4305.
Citation Information
Patent Citations
Method for improving 3D printing 17-4PH stainless steel yield strength
CN107012381A
Method for preparing titanium-based nano composite material based on selective laser melting 3D printing
CN109943786A
Two-phase particle reinforced additive aluminum alloy and preparation method thereof
CN115430843A
Wear-resistant and corrosion-resistant titanium-based composite material centrifuge scraper and preparation method thereof
CN117926145A
Materials, methods and techniques for surface alloying sand casted articles
US20220126357A1