Forming method of multipurpose gamma 'reinforced high-temperature alloy powder
Through the method of screening and process matching, the component matching problem of high-temperature alloy powder in different forming processes is solved, and the uniform forming and optimized mechanical properties of alloy materials are achieved. It is suitable for thermal isostatic pressure and laser additive manufacturing, reducing the R&D costs.
Patent Information
- Application Number
- CN202411151487.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-05
AI Technical Summary
The existing high-temperature alloy powder is difficult to be used in both thermal isostatic consolidation and laser additive manufacturing processes, which leads to the inability to match the alloy components, and is prone to problems such as stress concentration, cracking and original particle boundary defects, which limits its multi-purpose application.
By determining the composition and tissue characteristics of γ′ enhanced high-temperature alloy powder, screening different particle size segments, vacuum induction smelting and aerosolization are used to prepare powders, combining thermal isostatic pressure and laser additive manufacturing processes, the matching forming temperature range and Process parameters to achieve uniform forming of alloy materials and optimize mechanical properties.
The dendrites and grains of alloy materials are uniform and fine, without original particle boundary defects, and no thermal crack defects, which improves the mechanical properties and forming process performance, making high-temperature alloy powders suitable for multiple process routes at the same time, reducing R&D costs.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-temperature alloy preparation, and in particular to a forming method of multi-purpose γ′-strengthened high-temperature alloy powder. Background Art
[0002] High-temperature alloys are called the heart of turbines and have always attracted the attention of metallurgical workers. At present, the core hot-end components of advanced gas turbines, such as high-temperature alloy turbine blades and turbine disks, are all made of high-γ′ content high-temperature alloys. High γ′ content usually refers to high-temperature alloys with a γ′ content of 50 vol% or more, which is used to distinguish solid solution strengthened alloys with a lower degree of alloying. Such components are usually formed by precision casting, powder metallurgy and isothermal forging respectively. There are also integral turbine blades prepared by diffusion bonding of cast blades and powder turbine disks. Although the above traditional process routes are irreplaceable in the short term, the cost and cycle from part design, mold manufacturing to part forming are relatively high, and sometimes it is difficult to fully meet the progress requirements of the rapid development of new aircraft engines in my country. In addition, as the service time of existing engine parts gradually increases, the number of damaged parts in service that need to be repaired is also increasing. Additive manufacturing is a powerful supplement to the traditional process route: it is suitable for the development of engine parts that require rapid launch and small batches during the development period, the manufacture of high-cost value-added parts such as gas turbine engines, and the on-site rapid repair and replacement of key engine parts.
[0003] However, current alloys are often designed for a single purpose, resulting in a large number of alloy grades, but limited actual applications, resulting in huge waste. Therefore, realizing the application of an alloy in multiple fields and multiple uses has become a focus, and the synchronous matching of alloy composition and preparation process for different uses is the key.
[0004] High-temperature alloy powder is the preferred material for high-performance aircraft engine turbine disks. Powder turbine disks are mainly formed by hot isostatic pressing. High-temperature alloy powder is now also used in additive manufacturing of complex components, such as high-temperature alloy integral turbine blades. Due to the huge differences in the process characteristics of hot isostatic pressing and additive manufacturing, the alloy composition cannot be matched at the same time. For example, additive manufacturing is prone to stress concentration and cracking due to rapid heating and cooling, so the alloy is required to have a low tendency to thermal cracking; for hot isostatic pressing components, since the powder is solid-state sintering, it is easy to produce original particle boundaries, and due to the huge specific surface area of the powder material, the oxygen content is also easy to increase by orders of magnitude. These forming characteristics are all issues that need to be considered for multi-purpose powder materials, and increase the difficulty of determining the forming parameters of the same high-temperature alloy powder using two processes at the same time. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a forming method for a multi-purpose γ′ strengthened high-temperature alloy powder. The forming method provided by the present application can be simultaneously applicable to hot isostatic pressing consolidation forming process and laser additive manufacturing process. The alloy material prepared by the forming method has uniform and fine dendrites and grains, no original particle boundary defects, no thermal cracking defects, and has excellent mechanical properties and good forming process performance.
[0006] In view of this, the present application provides a method for forming a multi-purpose γ′ strengthened high temperature alloy powder, comprising the following steps: According to the composition characteristics of γ′ strengthened high temperature alloy powder and the organizational characteristics of bulk materials prepared for different purposes, the temperature range of organizational transformation for different purposes is determined; According to different uses of the γ′ strengthened high temperature alloy powder, the high temperature alloy powder is screened into particle size segments of different ranges, and then formed according to the temperature range; In terms of mass percentage, the composition of the γ′ strengthened high temperature alloy powder is (19-21) Co-(12-14) Cr-(1-3) W-(3-5) Mo-(0.5-1.5) Nb-(2-3) Ta-(0.7~1.5) Hf-(3-4) Al-(1-2) Ti-(0.02-0.03) B-(0.04-0.06) Zr-(0.001-0.01) C-remaining Ni; The different uses include use in a hot isostatic pressing consolidation forming process or a laser additive manufacturing process.
[0007] Preferably, the method for preparing the high temperature alloy powder comprises the following steps: Step 1: Prepare raw materials for preparing master alloy ingots according to the element ratio of γ′ strengthened high temperature alloy powder; Step 2: preparing a master alloy ingot by vacuum induction melting, wherein the vacuum pressure of the vacuum induction melting is less than 1 Pa; Step 3: remelt the master alloy ingot at a temperature of 1500-1600°C, use nickel foil to cover the Hf block, the thickness of the nickel foil is 0.1-1.5 mm, add the Hf block after the master alloy ingot is completely melted, and then refine and pour to avoid Hf oxidation. The refining temperature is 1550-1600°C, the refining time is >30min, and electromagnetic stirring is performed. The pouring temperature is 1450-1550°C, and then the high-temperature alloy powder is prepared by gas atomization powder making, and the atomization pressure is 2.5-5.5MPa. Step 4: Sieve the prepared alloy powder to a particle size of <200 μm.
[0008] Preferably, the γ′-strengthened high-temperature alloy powder is used in a hot isostatic pressing consolidation forming process, and the screened particle size is 0-63 μm; the γ′-strengthened high-temperature alloy powder is used in a laser additive manufacturing process, and the screened particle size is 53-150 μm.
[0009] Preferably, the high temperature alloy powder is used in a hot isostatic pressing consolidation forming process, specifically: The γ′ strengthened high temperature alloy powder was screened into a particle size range of 0~63μm, and then vibrated, degassed, and sealed in a stainless steel sleeve. The vibration time was >20s, the frequency was 50~70Hz, and the vacuum pressure was less than 10 -3 Pa, high temperature vacuum degassing is carried out, and the stainless steel sheath is placed in a hot isostatic press for hot isostatic pressing and consolidation forming. The preheating temperature of the hot isostatic pressing is 1000~1200℃, the temperature of the hot isostatic pressing is 1100~1200℃, the pressure is 150~200MPa, and the time is >3h.
[0010] Preferably, the degassing temperature is determined based on the different gas release sensitive temperatures of the γ′ strengthened high temperature alloy powder, specifically 25°C / 1h+120~180°C / 1~3h+300~350°C / 1~3h+550~600°C / 1~3h, and the total degassing time is >5h.
[0011] Preferably, the high temperature alloy powder is used in a laser additive manufacturing process, specifically: The γ′ strengthened high-temperature alloy powder is sieved to a particle size range of 53~150μm, and then the high-temperature alloy powder is placed in a laser additive manufacturing device for forming. The laser power is 600~900w and the scanning speed is 800~1000mm / s.
[0012] Preferably, heat treatment is also included after the forming, and the heat treatment system includes: 900~1100℃ / 1~3h air cooling + 1100~1150℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling, or 900~1100℃ / 1~3h air cooling + 1155~1200℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling.
[0013] Preferably, the heat treatment system includes: 1000℃ / 2h air cooling + 1115~1135℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling, or 1000℃ / 2h air cooling + 1155~1195℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling.
[0014] Preferably, the forming method further comprises characterizing the γ′ strengthened high temperature alloy powder and the alloy material after forming, specifically: Scanning electron microscopy and electron probe were used to characterize the microstructure morphology and composition of different regions of γ′ strengthened high temperature alloy powder and formed alloy material. Synchrotron radiation X-rays were used to characterize the precipitation phases of γ′-strengthened high-temperature alloy powders and the alloy materials after forming, and the hardness, tensile properties, creep properties, high-temperature durability, impact toughness and fatigue properties of the alloys were tested.
[0015] Preferably, the precipitated phases of the γ′ strengthened high temperature alloy powder and the alloy material after forming are characterized and analyzed and compared by synchrotron radiation X-ray, specifically: Synchrotron X-ray diffraction was used to quickly characterize the trace precipitates of γ′ strengthened superalloy powder, including γ′ strengthened phase and carbide phase. The energy of synchrotron X-ray was 70-80 KeV, the wavelength λ was 0.163137 Å, the X-ray spot was 100-200 μm, and the exposure time was 1-2 s to obtain the powder diffraction ring pattern. The formed alloy materials are characterized by XRD in the same manner as above, including the alloy materials formed by hot isostatic pressing consolidation forming process and the alloy materials formed by laser additive manufacturing; By comparing the XRD curves of γ′ strengthened high temperature alloy powder and the alloy material after forming, the precipitation law and organizational inheritance characteristics of the precipitated phase from the high temperature alloy powder to the alloy material after forming were obtained.
[0016] The present application provides a forming method for a multi-process common γ′ strengthened high-temperature alloy powder. The method first determines the temperature range of organizational transformation under different uses according to the inherent composition characteristics of the high-temperature alloy powder (19-21) Co-(12-14) Cr-(1-3) W-(3-5) Mo-(0.5-1.5) Nb-(2-3) Ta-(0.7~1.5) Hf-(3-4) Al-(1-2) Ti-(0.02-0.03) B-(0.04-0.06) Zr-(0.001-0.01) C- remaining Ni and the organizational characteristics of the bulk material prepared for different uses. Then, according to the different uses of the high-temperature alloy powder, the high-temperature alloy powder is screened into particle size segments with different ranges. Finally, the high-temperature alloy powder is formed according to the above-mentioned temperature range. The forming method provided in the present application balances the alloy elements and the forming process, formulates a matching temperature range for different purposes according to the characteristics of different process organization transformation, and realizes accurate customization of the forming process. The alloy powder provided in the present application can be applied to both hot isostatic pressing consolidation forming and laser additive manufacturing processes, ultimately making the alloy material have uniform and fine dendrites and grains, free of original particle boundary defects and thermal cracking defects, and having excellent mechanical properties and good forming process performance. Furthermore, the present application can be characterized by combining a variety of test characterization methods, thereby improving the detection sensitivity of trace phases and the comparability of alloys in different states (powder, block). DETAILED DESCRIPTION
[0017] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0018] In view of the problem that γ'-strengthened high-temperature alloy powder materials in the prior art cannot be simultaneously applied to different purposes, the present application provides a forming method for a multi-purpose γ'-strengthened high-temperature alloy powder, which enables the material to meet multi-purpose applications at the same time through component design and process customization matching, so that the γ'-strengthened high-temperature alloy powder has a higher Mo and Ta content, appropriately reduces the Ti content, and reduces the carbon content by more than 70% compared with similar traditional alloys. At the same time, on the basis of adding 0.7~1.5wt% Hf elements, the original particle boundary defects are reduced through a specific forming process, and the MC and γ' phases are further strengthened, the crack tendency is reduced, and the fatigue resistance is improved; and the forming process parameters are finely matched in combination with the balance of other alloy elements, so that the same alloy powder material is simultaneously suitable for hot isostatic pressing consolidation forming to prepare aircraft engine turbine disks or laser additive manufacturing to prepare gas turbine integral turbine impellers. Specifically, an embodiment of the present invention discloses a forming method for a multi-purpose γ'-strengthened high-temperature alloy powder, comprising the following steps: According to the composition characteristics of γ′ strengthened high temperature alloy powder and the organizational characteristics of bulk materials prepared for different purposes, the temperature range of organizational transformation for different purposes is determined; According to different uses of the γ′ strengthened high temperature alloy powder, the high temperature alloy powder is screened into particle size segments of different ranges, and then formed according to the temperature range; In terms of mass percentage, the composition of the γ′ strengthened high temperature alloy powder is (19-21) Co-(12-14) Cr-(1-3) W-(3-5) Mo-(0.5-1.5) Nb-(2-3) Ta-(0.7~1.5) Hf-(3-4) Al-(1-2) Ti-(0.02-0.03) B-(0.04-0.06) Zr-(0.001-0.01) C-remaining Ni; The different uses include use in a hot isostatic pressing consolidation forming process or a laser additive manufacturing process.
[0019] The use in the present application specifically refers to the use of γ′ strengthened high temperature alloy powder in a hot isostatic pressing consolidation molding process or in a laser additive manufacturing process.
[0020] The present invention reduces the carbon content by more than 70% compared with similar traditional alloys through careful balance optimization of alloy components and parameter matching combined with the characteristics of the forming process. At the same time, Hf elements are added to reduce the defects of the original grain boundaries (PPBs), further strengthening MC and γ′, reducing the crack tendency and improving fatigue resistance. The same alloy powder material is suitable for hot isostatic pressing consolidation forming to prepare aircraft engine turbine disks or laser additive manufacturing instruments to prepare gas turbine integral turbine impellers and prepare alloy block materials in corresponding states.
[0021] In the forming method provided in the present application, a high temperature alloy powder is first prepared by a vacuum induction melting process, which specifically includes the following steps: Step 1: Prepare raw materials for preparing master alloy ingots according to the element ratio of γ′ strengthened high temperature alloy powder; Step 2: preparing a master alloy ingot by vacuum induction melting, wherein the vacuum pressure of the vacuum induction melting is less than 1 Pa; Step 3, remelting the master alloy ingot, the remelting temperature is 1500~1600℃, using nickel foil to cover the Hf block, the nickel foil thickness is 0.1~1.5mm, adding the Hf block after the master alloy ingot is completely melted, the refining temperature is 1550~1600℃m, the refining time is>30min, and electromagnetic stirring is performed, the pouring temperature is 1450~1550℃, and the high-temperature alloy powder is prepared by a gas atomization powder making furnace with a capacity of 50~300kg, and the atomization pressure is 2.5~5.5MPa; Step 4: Sieve the prepared alloy powder to a particle size of <200 μm.
[0022] In the above process, the prepared raw materials are prepared according to the raw materials familiar to those skilled in the art, and this application does not impose any special restrictions on this. The technical means of vacuum induction melting are well known to those skilled in the art, and this application does not impose any special restrictions on this. The Hf block is coated with a nickel foil with high density and thickness, which can make Hf fully contact with the melt without being oxidized by the atmosphere compared to traditional aluminum foil. The remelting temperature is preferably 1550~1580℃, the refining temperature is preferably 1550~1580℃, and the pouring temperature is preferably 1480~1520℃. The powder making method is prepared by gas atomization, and the atomization pressure is preferably 4~5.0MPa. After finally screening through a mechanical vibrating screen, a high-temperature alloy powder with a particle size of <200μm is obtained. In the present application, the composition of the γ′ strengthened high temperature alloy powder is (19-21) Co-(12-14) Cr-(1-3) W-(3-5) Mo-(0.8-1.2) Nb-(2.2-2.8) Ta-(0.8~1.2) Hf-(3-4) Al-(1-2) Ti-(0.02-0.03) B-(0.05-0.06) Zr-(0.003-0.007) C-residue Ni; specifically (19.3-20.7) Co-(12.2-13.9) Cr-(1.4-2.7) W-(3. 3-4.8)Mo-(0.9-1.1)Nb-(2.3-2.6)Ta-(0.9~1.1)Hf-(3.3-3.8)Al-(1.2-1.8)Ti-(0.02-0.03)B-(0.05-0.06)Zr-(0.004-0.006)C-remaining Ni; For example, the composition of the high-temperature alloy powder described in the present application is 20Co-13Cr-3W-4Mo-1Nb-2.5Ta-1Hf-3.5Al-1.5Ti-0.02B-0.04Zr-0.005C-remaining Ni.
[0023] The above-mentioned γ′ strengthened high temperature alloy powder of the present application can be simultaneously applied to the following processes, specifically: The γ′-strengthened high-temperature alloy powder is consolidated and formed by hot isostatic pressing; Alternatively, a laser additive manufacturing process is used to rapidly melt and solidify γ′ strengthened high temperature alloy powder into a knot.
[0024] For high temperature alloy powder used in hot isostatic pressing consolidation forming process, specifically: The γ′ strengthened high temperature alloy powder was screened into a particle size range of 0~63μm, and then vibrated, degassed, and sealed in a stainless steel sleeve. The vibration time was >20s, the frequency was 50~70Hz, and the vacuum pressure was less than 10 -3Pa, high temperature vacuum degassing is carried out, and the stainless steel sheath is placed in a hot isostatic press for hot isostatic pressing and consolidation forming. The preheating temperature of the hot isostatic pressing is 1000~1200℃, the temperature of the hot isostatic pressing is 1100~1200℃, the pressure is 150~200Mpa, and the time is >3h.
[0025] In the above hot isostatic pressing consolidation forming process, the determination of the degassing temperature depends on the different gas escape sensitive temperatures of the γ′ strengthened high temperature alloy powder, and the specific parameters are 25℃ / 1h+120~180℃ / 1~3h+300~350℃ / 1~3h+550~600℃ / 1~3h, and the total degassing time is >5h. The preheating temperature of the hot isostatic pressing is 1100~1150℃, and the heat preservation and pressure holding parameters and time are 1165~1185℃ / 160~180Mpa / 4~5h.
[0026] Alternatively, the γ′-strengthened high-temperature alloy powder is used in a laser additive manufacturing process, that is, the γ′-strengthened high-temperature alloy powder is rapidly melted and solidified into a shape, specifically: The γ′ strengthened high-temperature alloy powder is sieved to a particle size range of 53~150μm, and then the high-temperature alloy powder is placed in a laser additive manufacturing device for forming. The laser power is 600~900w and the scanning speed is 800~1000mm / s.
[0027] In the above-mentioned laser additive manufacturing process, the laser power is 700~800w, and the scanning speed is 900~1000mm / s.
[0028] The present application then heat treats the formed alloy, and the heat treatment system includes: 900~1100℃ / 1~3h air cooling + 1100~1150℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling, or 900~1100℃ / 1~3h air cooling + 1155~1195℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling; specifically: 920~1080℃ / 2h air cooling + 1115 ~1135℃ / 1~4h oil cooling +800~850℃ / 16~20h air cooling or oil cooling, or 920~1080℃ / 2h air cooling +1155~1195℃ / 1~4h oil cooling +800~850℃ / 16~20h air cooling or oil cooling; more specifically: 1000℃ / 2h air cooling +1165℃ / 4h oil cooling +850℃ / 16h air cooling, or 1000℃ / 2h air cooling +1115℃ / 4h oil cooling +850℃ / 16h air cooling or oil cooling.
[0029] Furthermore, the forming method of the present application also includes characterizing the high-temperature alloy powder and the formed alloy material separately, using a scanning electron microscope and an electron probe to characterize the microstructure morphology of the powder and the alloy and the composition of different regions, using synchrotron radiation X-rays to characterize the precipitation phase of the alloy and the powder, and testing the mechanical properties of the alloy such as hardness, tensile properties, creep properties, high temperature durability, impact toughness and fatigue properties, more specifically: Synchrotron radiation X-ray diffraction was used to quickly characterize the trace precipitated phases of γ′ strengthened superalloy powder, including γ′ strengthened phase and carbide phase. The synchrotron radiation X-ray energy was 70-80 KeV, the wavelength λ was 0.163137 Å, the X-ray spot was 100-200 μm, and the exposure time was 1-2 s to obtain the powder diffraction ring pattern. The same method as above was used to perform XRD characterization on the alloy materials after forming, including the alloy materials after hot isostatic pressing consolidation forming process and the alloy materials after laser additive manufacturing forming.
[0030] The microstructure and defect characteristics of alloy materials prepared by powder to hot isostatic pressing and additive manufacturing forming processes are compared, where the defects include but are not limited to micropore defects after hot isostatic pressing consolidation forming or thermal crack defects after additive manufacturing forming.
[0031] Furthermore, the same parameters were used to conduct nanohardness tests on powder particles and bulk alloys prepared by hot isostatic pressing and additive manufacturing. Depth control was adopted, and the indentation depth was in the range of 50nm~300nm, ensuring that the detection range requirements of fine original powders and bulk materials could be met and the results were comparable.
[0032] The forming method provided in the present application is designed by matching the composition and process, so that the high-temperature alloy powder is suitable for multiple process routes at the same time, including hot isostatic pressing consolidation and laser additive manufacturing, realizing the "one material for multiple uses" of the high-temperature alloy powder material, and reducing the comprehensive research and development cost of the material by 50%; the carbon content of the high-temperature alloy powder of the present application is further reduced, and the hard and brittle carbides are less. Through the control of the forming process, the precipitated carbides are made small in size and are not easy to cause stress cracking; the addition of Hf element improves the shrinkage compensation ability of the alloy melt and reduces the tendency of crack formation during solidification; the addition of Hf element while balancing other elements (Mo, Ta) plays a purifying role and seizes the solidification The impurity elements in the residual liquid phase of the process, while reducing the original particle boundary tendency; further, Hf is an extremely easy to oxidize metal, and Hf needs to be quickly sunk into the metal melt. A packaging method different from the traditional aluminum foil is adopted. The Hf block is coated with a high-density nickel foil and the Hf element package is added after melting, so that Hf can fully contact the melt without being oxidized by the atmosphere; in the forming process, a lower temperature pretreatment is used before hot isostatic pressing and heat treatment to reduce the initial melting of low-melting point phases; a more sophisticated degassing process reduces the hydrogen and oxygen content of the alloy powder, reduces the original particle boundary defects (PPB), and thus improves the mechanical properties of the bulk alloy and even the components. Furthermore, the combination of synchrotron radiation X-ray diffraction, focused ion beam scanning electron microscopy, transmission electron microscopy and nanohardness is used to characterize the organization and properties of powders and alloys, improve the detection sensitivity of trace phases and the comparability of alloys in different states (powder, bulk).
[0033] In order to further understand the present invention, the forming method of multi-process common γ'-strengthening high-temperature alloy powder provided by the present invention is described in detail below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments. Example 1
[0034] A) A multi-purpose γ'-strengthened high-temperature alloy powder and a method for preparing the alloy thereof, wherein the alloy composition is 20Co-13Cr-2W-4Mo-1Nb-2.5Ta-1.0Hf-3.5Al-1.5Ti-0.02B-0.04Zr-0.005C-residual Ni (wt%), a high-temperature alloy master alloy of the above composition is prepared by vacuum induction melting, and the alloy powder is prepared by vacuum induction remelting and gas atomization, specifically comprising the following steps: Step 1: Prepare the raw materials for preparing the master alloy ingot, clean the surface with ultrasonic wave and wipe it with alcohol; Step 2: preparing a master alloy ingot by vacuum induction melting, wherein the vacuum pressure during the melting process is less than 1 Pa, and the capacity of the crucible used to prepare the alloy ingot is capable of accommodating a master alloy weighing 50-4000 kg; Step 3: remelt the master alloy ingot in step 2 in an atomizing powder making furnace, the remelting temperature is 1500~1600℃, during the remelting process of the master alloy, high-density nickel foil is used to replace aluminum foil to cover the Hf block, the thickness of the nickel foil is 0.1~1.5mm, and after the master alloy is completely melted, the nickel foil Hf element package is added to make Hf fully contact with the melt without being oxidized by the atmosphere; the refining temperature is 1550~1600℃m, the refining time is>30min, and electromagnetic stirring is performed, the pouring temperature is 1450~1550℃, and the high-temperature alloy powder is prepared by gas atomization powder making, the atomization pressure is 4MPa, and the weight of the powder prepared in a single furnace is 300kg; Step 4: The prepared alloy powder is screened through a mechanical vibrating screen, and the particle size is less than 200 μm, and the super coarse powder and flaky and shaped powder are removed. The powder after screening is set aside; B) The γ'-strengthened high-temperature alloy prepared above can be prepared and formed by the following process methods: (1) Using hot isostatic pressing to consolidate γ′-strengthened high-temperature alloy powder; (2) Using laser additive manufacturing to rapidly melt and solidify γ′-strengthened high-temperature alloy powder; C) The hot isostatic pressing consolidation forming process is specifically as follows: the γ′ strengthened high temperature alloy powder is screened into a particle size range of 0-63 μm, the alloy powder is vibrated, degassed, and sealed in a stainless steel sheath, the vibrating time is greater than 20 s, the frequency is 60 Hz, and the vacuum pressure is less than 10 -3 Pa, use TPD or TPS to measure the characteristic temperature of multiple gases in the alloy powder, determine the combined temperature degassing parameters, the temperature is 25℃ / 1h+130℃ / 1h+310℃ / 1h+550℃ / 3h, the total degassing time is>5h, use argon arc welding to seal the package, put the high-temperature alloy powder package into a hot isostatic press for hot isostatic pressing and consolidation forming, the forming parameters are 1100℃ / 4h preheating treatment, and then 1165℃ / 150MPa / 4h hot isostatic pressing; The laser additive manufacturing process is specifically as follows: sieving the γ′-strengthened high-temperature alloy powder into a particle size range of 53-150 μm, and placing the high-temperature alloy powder in the sieved particle size range into a laser additive manufacturing device for forming, with a laser power of 700 w and a scanning speed of 1000 mm / s; D) heat treating the high temperature alloys obtained after the above forming respectively, and the heat treatment parameters are 1000℃ / 2h air cooling + 1165℃ / 4h oil cooling + 850℃ / 16h air cooling; E) Characterization of the alloy before and after forming includes: using scanning electron microscopy and electron probe to characterize the microstructure of the powder and alloy and the composition of different regions, using synchrotron radiation X-ray to characterize the precipitation phase of the powder and alloy, and testing the mechanical properties of the alloy; The above-mentioned synchrotron radiation X-ray characterization of the precipitation phase of the alloy and powder is as follows: Synchrotron X-ray diffraction (XRD) was used to quickly characterize the trace precipitated phases of γ' strengthened high temperature alloy powder, including γ' and carbide phases. The synchrotron X-ray energy was 76KeV, the wavelength λ was 0.163137 Å, the X-ray spot was 100μm, and the exposure time was 2s to obtain the powder diffraction ring pattern. The results showed that the powder in the particle size segment <32μm had trace phases, including γ' and MC carbides, and the powder in the particle size segment of 75~100μm and the powder in the particle size segment of 100~150μm had trace phases, including γ' and MC carbides. The γ' peak heights of the three particle size segments were not much different. The powder and the additively manufactured alloy showed a fine dendritic structure. The interdendritic region was mainly enriched with Hf, Ti, Nb, and Ta, which further strengthened the interdendritic region. The same method as above is used to perform XRD characterization on bulk materials after powder forming, including hot isostatic pressing consolidation forming alloys and additive manufacturing forming high-temperature alloys; Compare the XRD curves of powder and bulk alloys to understand the precipitation law and organizational inheritance characteristics of the precipitation phase from high-temperature alloy powder to bulk alloy; the powder and additive manufacturing alloys have fine dendritic structures, and the interdendritic regions are mainly enriched with Hf, Ti, Nb, and Ta. The interdendritic regions are further strengthened, and the hot isostatic pressing and additive manufacturing high-temperature alloys obtained have fine, uniform structures without holes, original grain boundary defects, and thermal cracks; F) The same parameters were used to perform nanohardness tests on powder particles and bulk alloys prepared by hot isostatic pressing and additive manufacturing. Depth control was adopted, and the indentation depth was 50nm and 200nm to ensure that the detection range requirements of fine original powder and bulk material and the results were comparable. Under the indentation depth of 200nm, the hardness of additive manufacturing and hot isostatic pressing alloys were 8.7 and 9.3GPa, respectively. Under the indentation depth of 50nm, the hardness of additive manufacturing and hot isostatic pressing alloys were 14.9 and 14.6GPa, respectively, which were comparable to the performance of rapidly solidified original coarse powder (100~150μm). The nanohardness of the powder at indentation depths of 200nm and 50nm was 8.8GPa and 15.3GPa, respectively. Therefore, this embodiment can make the nanohardness of the bulk material comparable to the performance of the original powder prepared by rapid solidification by reasonably matching process control. Example 2
[0035] The method is basically the same as that of Example 1, except that the heat treatment parameters after the hot isostatic pressing process are 1000°C / 2h air cooling + 1115°C / 4h oil cooling + 850°C / 16h air cooling; The hardness test results show that the nanohardness of the alloy is 7.9 GPa at an indentation depth of 200 nm, and the nanohardness of the alloy is 13.7 GPa at an indentation depth of 50 nm.
[0036] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0037] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for forming a multi-purpose γ′-strengthened high-temperature alloy powder, comprising the following steps: According to the composition characteristics of γ′ strengthened high temperature alloy powder and the organizational characteristics of bulk materials prepared for different purposes, the temperature range of organizational transformation for different purposes is determined; According to different uses of the γ′ strengthened high temperature alloy powder, the high temperature alloy powder is screened into particle size segments of different ranges, and then formed according to the temperature range; In terms of mass percentage, the composition of the γ′ strengthened high temperature alloy powder is (19-21) Co-(12-14) Cr-(1-3) W-(3-5) Mo-(0.5-1.5) Nb-(2-3) Ta-(0.7~1.5) Hf-(3-4) Al-(1-2) Ti-(0.02-0.03) B-(0.04-0.06) Zr-(0.001-0.01) C-remaining Ni; The different uses include use in a hot isostatic pressing consolidation forming process or a laser additive manufacturing process.
2. The forming method according to claim 1, characterized in that: The method for preparing the high temperature alloy powder comprises the following steps: Step 1: Prepare raw materials for preparing master alloy ingots according to the element ratio of γ′ strengthened high temperature alloy powder; Step 2: preparing a master alloy ingot by vacuum induction melting, wherein the vacuum pressure of the vacuum induction melting is less than 1 Pa; Step 3: remelt the master alloy ingot at a temperature of 1500-1600°C, use nickel foil to cover the Hf block, the thickness of the nickel foil is 0.1-1.5 mm, add the Hf block after the master alloy ingot is completely melted, and then refine and pour to avoid Hf oxidation. The refining temperature is 1550-1600°C, the refining time is >30min, and electromagnetic stirring is performed. The pouring temperature is 1450-1550°C, and then the high-temperature alloy powder is prepared by gas atomization powder making, and the atomization pressure is 2.5-5.5MPa. Step 4: Sieve the prepared alloy powder to a particle size of <200 μm.
3. The forming method according to claim 1, characterized in that: The γ′ strengthened high temperature alloy powder is used for hot isostatic pressing consolidation forming process, and the screened particle size is 0-63 μm; the γ′ strengthened high temperature alloy powder is used for laser additive manufacturing process, and the screened particle size is 53-150 μm.
4. The forming method according to claim 1, characterized in that: The high temperature alloy powder is used in a hot isostatic pressing consolidation forming process, specifically: The γ′ strengthened high temperature alloy powder was screened into a particle size range of 0~63μm, and then vibrated, degassed, and sealed in a stainless steel sleeve. The vibration time was >20s, the frequency was 50~70Hz, and the vacuum pressure was less than 10 -3 Pa, high temperature vacuum degassing is carried out, and the stainless steel sheath is placed in a hot isostatic press for hot isostatic pressing and consolidation forming. The preheating temperature of the hot isostatic pressing is 1000~1200℃, the temperature of the hot isostatic pressing is 1100~1200℃, the pressure is 150~200MPa, and the time is >3h.
5. The forming method according to claim 4, characterized in that: The degassing temperature is determined based on the different gas release sensitive temperatures of the γ′ strengthened high temperature alloy powder, specifically 25°C / 1h+120~180°C / 1~3h+300~350°C / 1~3h+550~600°C / 1~3h, and the total degassing time is >5h.
6. The forming method according to claim 1, characterized in that: The high temperature alloy powder is used in a laser additive manufacturing process, specifically: The γ′ strengthened high-temperature alloy powder is sieved to a particle size range of 53~150μm, and then the high-temperature alloy powder is placed in a laser additive manufacturing device for forming. The laser power is 600~900w and the scanning speed is 800~1000mm / s.
7. The forming method according to any one of claims 1 to 6, characterized in that: The forming process further includes heat treatment, and the heat treatment system includes: 900~1100℃ / 1~3h air cooling + 1100~1150℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling, or 900~1100℃ / 1~3h air cooling + 1155~1200℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling.
8. The forming method according to claim 7, characterized in that: The heat treatment system includes: 1000℃ / 2h air cooling + 1115~1135℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling, or 1000℃ / 2h air cooling + 1155~1195℃ / 1~4h oil cooling + 800~850℃ / 16~20h air cooling or oil cooling.
9. The forming method according to any one of claims 1 to 7, characterized in that: The forming method further includes characterizing the γ′ strengthened high temperature alloy powder and the alloy material after forming, specifically: Scanning electron microscopy and electron probe were used to characterize the microstructure morphology and composition of different regions of γ′ strengthened high temperature alloy powder and formed alloy material. Synchrotron radiation X-rays were used to characterize the precipitation phases of γ′-strengthened high-temperature alloy powders and the alloy materials after forming, and the hardness, tensile properties, creep properties, high-temperature durability, impact toughness and fatigue properties of the alloys were tested.
10. The forming method according to claim 9, characterized in that: The synchrotron radiation X-ray is used to characterize the precipitation phases of the γ′ strengthened high temperature alloy powder and the alloy material after forming, and analyze and compare them, specifically: Synchrotron X-ray diffraction was used to quickly characterize the trace precipitates of γ′ strengthened superalloy powder, including γ′ strengthened phase and carbide phase. The energy of synchrotron X-ray was 70-80 KeV, the wavelength λ was 0.163137 Å, the X-ray spot was 100-200 μm, and the exposure time was 1-2 s to obtain the powder diffraction ring pattern. The formed alloy materials are characterized by XRD in the same manner as above, including the alloy materials formed by hot isostatic pressing consolidation forming process and the alloy materials formed by laser additive manufacturing; By comparing the XRD curves of γ′ strengthened high temperature alloy powder and the alloy material after forming, the precipitation law and organizational inheritance characteristics of the precipitated phase from the high temperature alloy powder to the alloy material after forming were obtained.